Metallic bond grinding wheel for slotting of ceramic material and preparation method of metallic bond grinding wheel

By designing L-shaped steps and laser laser pretreatment in the ceramic core workpiece groove grinding wheel, the bonding strength between the steel matrix and the abrasive layer is improved, and the problem of the grinding wheel eclipse and low bonding strength is solved, and the workpiece groove edge collapse is achieved. The 40μm and grinding wheel have good wear resistance, which meets the needs of domestic substitution.

CN119017279AActive Publication Date: 2024-11-26ZHENGZHOU SHINE MORE SUPERABRASIVES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411480874.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-26
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

During the processing process, the existing ceramic core workpiece groove grinding wheel has problems such as the grinding wheel slanting, flange glue and abrasive layer and the steel substrate, which leads to the workpiece groove collapse not small enough, and the domestic grinding wheel is less developed, making it difficult to Meets the requirements of high shape retention, high wear resistance and high sharpness.

Method used

A metal bonding agent grinding wheel for grooved ceramic material is designed. By designing L-shaped steps and laser laser pretreatment on the steel substrate, the contact area and bonding strength between the steel substrate and the abrasive layer are increased, and a specific metal bonding agent is used to form a specific metal bonding agent. and the sintering process ensures the parallelism and coaxiality of the grinding wheel and avoids the abrasive layer de-ring.

Benefits of technology

The workpiece notch edge collapse is less than 40μm, the grinding wheel is sharp and wear-resistant, meets customer quality requirements, improves the bond strength and batch stability of the grinding wheel, and can replace imported grinding wheels and realize domestic production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017279A_ABST
    Figure CN119017279A_ABST
Patent Text Reader

Abstract

The invention discloses a metallic bond grinding wheel for slotting a ceramic material and a preparation method of the metallic bond grinding wheel, and belongs to the technical field of preparation of superhard materials. In the preparation process of the grinding wheel, the contact part of the steel substrate and the grinding material layer is pretreated, the process can promote the formation of a plurality of hemispherical pits in the surface of the steel substrate, the contact area of the steel substrate and the grinding material layer is increased, the pits are filled with the grinding material layer, the holding force of the steel substrate to the grinding material layer is improved, and the grinding effect is improved. Therefore, the bonding strength between the steel substrate and the abrasive layer is improved, and the phenomenon of ring separation of the abrasive layer in the machining process is avoided. The feeding area of the steel base body is designed to be in an L-shaped step shape, and the contact area of the grinding material layer and the steel base body is increased. The grinding material layer shrinks, the steel base body can be firmly hooped, the coaxiality of the grinding wheel, the grinding material layer and the steel base body is smaller than or equal to 0.008 mm, and the parallelism of the end face of the grinding wheel is smaller than or equal to 0.015 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superhard material preparation, and in particular relates to a metal bond grinding wheel for grooving ceramic materials and a preparation method thereof. Background Art

[0002] Fiber optic ceramic ferrule, also known as ceramic ferrule body, is a precisely centered cylinder in the fiber optic connector plug. It is a high-precision special ceramic component made of nano zirconium oxide (ZrO2) material through a series of formulations and processing. The precision slotting processing of this type of high-precision special ceramic component puts forward comprehensive performance requirements for the grinding wheel, such as high shape retention, high wear resistance, high sharpness, and high material removal rate. The workpiece slot edge collapse is required to be less than 40μm. The processing equipment can automatically detect the size of the slot edge collapse. If it exceeds 40μm, the equipment will alarm and stop working. At present, imported metal bond slotting grinding wheels are used for processing.

[0003] This type of grinding wheel has a large diameter and thickness (diameter over 200mm, thickness over 20mm), and has a reinforced flange on one side of the grinding wheel. It is made by bonding the reinforced flange with the conventional 1A1 type grinding wheel. During use, it is easy to have serious grinding wheel deflection and flange debonding problems. Compared with the outer diameter of the grinding wheel, the abrasive working layer is narrower (≤10mm). If the bonding strength between the working layer and the steel substrate is low, the abrasive layer of the grinding wheel is easy to be debonded as a whole during the grooving process. At present, this type of grinding wheel mainly relies on foreign imports. There are few reports of this type of grinding wheel in China, and further research is needed. Summary of the invention

[0004] In order to overcome the problems in the prior art, the present invention provides a metal bond grinding wheel for grooving ceramic materials (grinding wheel drawing as shown in FIG. Figure 1 and Figure 2 As shown in the figure, the steel substrate and the reinforced flange are designed as a whole to ensure that the parallelism of the two end surfaces of the grinding wheel is ≤0.015mm and the working layer runout is ≤0.015mm. During the manufacturing process of the grinding wheel, the contact surface between the steel substrate and the abrasive working layer is specially treated, and the grinding wheel is manufactured on this basis; the grinding wheel can be used for grooving of ceramic insert workpieces, which can meet the workpiece notch edge collapse of <40μm, and the grinding wheel groove is sharp and wear-resistant, meeting the customer's quality requirements.

[0005] A metal bond grinding wheel for grooving ceramic materials, the grinding wheel comprising a substrate and an abrasive layer arranged on the surface of the substrate; the abrasive layer is made of a main abrasive and a metal bond, the main abrasive is diamond, the metal bond is composed of the following components in percentage by mass: copper powder, tin powder, nickel powder, silver powder and graphite, the weight parts of each raw material are as follows: 20-40 parts of diamond, 60-70 parts of copper powder, 10-20 parts of tin powder, 5-15 parts of nickel powder, 5-15 parts of silver powder, 2-8 parts of graphite, the particle size of diamond is 35-91 μm, and each component of the metal bond is in powder form, and the particle size is greater than or equal to 170 meshes.

[0006] Furthermore, the substrate is a toothless structure, and an L-shaped step is circumferentially provided on the outer edge of the upper end surface of the substrate. The L-shaped step has a width of 5 to 10 mm and a depth of 1.0 to 2.0 mm, and the L-shaped step is used to accommodate the abrasive layer.

[0007] Furthermore, the total width of the abrasive layer is 5-10 mm, the thickness of the effective grinding area is 0.5 mm-1.5 mm, and the width of the effective grinding area is 2-4 mm.

[0008] The preparation method of the metal bond grinding wheel for grooving the ceramic material is as follows: (1) Matrix processing: rough turning of the matrix, flat grinding of the matrix, and fine turning of the matrix to produce an L-shaped step; (2) Mixing: Mix the components of the metal binder, the main abrasive and the wetting agent for 2 to 5 hours to obtain a mixture; (3) Substrate pretreatment: After cleaning the substrate, perform laser treatment, and then perform sandblasting after cleaning and drying; (4) Molding and sintering: the substrate of step (3) and the mixed material of step (2) are put into a mold, spread and flattened, and then placed in an atmosphere sintering furnace for sintering and molding. The specific sintering process is: in a hydrogen atmosphere, at a sintering temperature of 800-950° C. and a sintering pressure of 10-15 MPa, heat preservation treatment for 1-2 h, after the heat preservation is completed, the temperature is lowered to room temperature, and demolding is performed to obtain a grinding wheel blank; (5) Mechanical processing: machining the outer cylindrical end surface and inner hole of the grinding wheel blank in step (4), making a positioning hole on the steel substrate on one side of the abrasive layer based on the positioning of the inner hole, and finally obtaining a semi-finished grinding wheel; (6) Processing of effective grinding area of ​​abrasive layer: Use resin super-hard grinding wheel to grind the abrasive layer of the semi-finished grinding wheel in step (5) so that the effective grinding area is finely processed to 0.5mm~1.5mm thick × 2mm~4mm wide. Before processing, the end face runout of the substrate is ≤0.01mm before processing. After processing, the end face runout of the abrasive layer is ≤0.015mm to be qualified; (7) Dynamic balancing correction: On a high-precision dynamic balancing machine, the weight is removed by punching holes. The dynamic imbalance is ≤0.2g. The qualified one is considered a finished product.

[0009] Furthermore, the specific process of step (3) is as follows: S1. The substrate is acid-washed in 90-95wt% nitric acid for 5-10 min, then cleaned with distilled water, then alkaline-washed in 40-50wt% NaOH aqueous solution for 5-10 min to remove impurities and oil stains, then cleaned with distilled water, and dried; S2, placing the substrate dried in step S1 into a laser machine, and lasering a uniform hemispherical pit on the bottom surface of the L-shaped step, wherein the radius of the hemispherical pit is 0.1-0.3 mm; S3, washing the substrate obtained in step S2 with pure water and drying; S4. In order to increase the surface roughness of the steel substrate and treat the oxide layer after laser blasting, the substrate treated with S3 was placed in a sandblasting machine and the surface of the substrate was treated with 80-150 mesh corundum sand.

[0010] Preferably, the bottom surface of the L-shaped step has 5 to 10 hemispherical pits radially distributed. Sandblasting pressure 100 to 200 kg / cm 2 , sandblasting time is 10~30 s. The power of the laser machine is 50~100W.

[0011] Furthermore, in step (2), the wetting agent is liquid paraffin, and 10-20 mL of liquid paraffin is added for every 1 kg of the total weight of the main abrasive and the metal binder; the wetting agent evaporates during the sintering molding preparation process.

[0012] Furthermore, in step (5), the positioning holes are countersunk holes with a diameter of 6 to 7 mm, and 4 to 6 positioning holes are evenly distributed along the circumference of the inner hole of the working surface of the substrate abrasive layer.

[0013] Furthermore, in step (5), after the grinding wheel is processed, the coaxiality between the abrasive layer and the substrate is ≤0.008 mm; the upper end surface of the working layer of the abrasive layer is at the same height as the substrate, and the parallelism with the bottom surface of the substrate is ≤0.015 mm.

[0014] The innovation of the present invention is: 1) Pretreatment of the contact area between the steel substrate and the abrasive layer during the preparation of the grinding wheel. This process can form many hemispherical pits on the surface of the steel substrate, increase the contact area between the steel substrate and the abrasive layer, and fill the abrasive layer into the pits, which improves the holding force of the steel substrate on the abrasive layer, thereby improving the bonding strength between the steel substrate and the abrasive layer and avoiding the abrasive layer debonding phenomenon during the processing process.

[0015] 2) The feeding area of ​​the steel substrate is designed as an L-shaped step, which increases the contact area between the abrasive layer and the steel substrate. The shrinkage of the abrasive layer can also firmly clamp the steel substrate.

[0016] 3) The coaxiality of the abrasive layer and the steel substrate of the metal bonded grinding wheel produced in this way is ≤0.008mm, and the parallelism of the end face of the grinding wheel is ≤0.015mm; Compared with the prior art, the present invention has the following beneficial effects: 1) The grinding wheel blank produced by the present invention has a simple processing technology and is easy to operate; 2) By pre-treating the steel substrate with laser, the bonding strength between the steel substrate and the abrasive layer is improved, thus avoiding the abrasive layer from falling off during use; 3) The grinding wheel of the present invention can be used for slotting of optical fiber ceramic core materials. Compared with imported grinding wheels, it meets the requirement of workpiece notch edge collapse less than 40 μm, has good wear resistance, high batch stability, and can achieve domestic substitution. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of a metal bond grinding wheel; Figure 2 This is a partial enlarged view of the working part of the metal bond abrasive layer; Figure 3 Schematic diagram of the surface state of the steel substrate after laser irradiation. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is further described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the following examples, the particle sizes of the raw materials copper powder, tin powder, nickel powder, silver powder and graphite used are all ≤50 μm, and they can be directly purchased from ordinary commercial products. The abrasive diamond is an ordinary commercial product.

[0020] Example 1 A metal bond grinding wheel for grooving ceramic materials, such as Figure 1 As shown, it includes a steel substrate and an abrasive layer, wherein the abrasive layer includes abrasive and a metal binder, and is specifically composed of the following raw materials in parts by weight: 65 parts of copper powder, 15 parts of tin powder, 10 parts of nickel powder, 10 parts of silver powder, 5 parts of graphite, and 30 parts of diamond (mesh size is 400 mesh).

[0021] One side of the steel substrate is a trapezoidal structure, which is a substrate reinforcement flange part. In the present invention, the grinding wheel model used is 3A1 D200×T20.2×H24×E0.5×X7, where: D represents the diameter of the grinding wheel, T represents the total thickness of the grinding wheel, H represents the diameter of the inner hole of the grinding wheel, E represents the thickness of the effective grinding area of ​​the abrasive layer, and X represents the total width of the abrasive layer, and the units are all: mm.

[0022] The preparation method of the metal bond grinding wheel specifically comprises the following steps: (1) Matrix processing: The matrix is ​​rough turned, flat ground, and fine turned. The outer edge of the upper end surface of the matrix is ​​fine turned to form an L-shaped step with a width of 7 mm and a depth of 1.5 mm for placing an abrasive layer during molding. Compared with the conventional grinding wheel matrix, the steel matrix has a toothless structure. The matrix structure is as follows: Figure 2 shown.

[0023] (2) Take 65 parts of copper powder, 15 parts of tin powder, 10 parts of nickel powder, 10 parts of silver powder, 5 parts of graphite, and 30 parts of diamond (mesh size is 400 mesh), and add 20 mL of liquid paraffin for every 1 kg of raw materials based on the total weight of the above raw materials. Add the raw materials and liquid paraffin into a mixing tank and seal it. Put the sealed mixing tank into a three-dimensional mixer and mix for 3 hours to obtain a mixture; (3) Pretreatment of steel substrate S1. Pretreatment cleaning: The steel substrate was pickled in a 90% nitric acid solution for 10 minutes, cleaned with distilled water, then alkaline washed in a 50% NaOH aqueous solution for 10 minutes to remove impurities and oil stains, then cleaned with distilled water and dried; S2, Laser The steel substrate dried in step S1 is placed in a laser machine (power 50w), and the bottom surface of the L-shaped step is lasered to form uniform hemispherical pits with a radius of 0.1mm. There are 5 to 10 hemispherical pits distributed radially on the bottom surface of the L-shaped step. The effect after laser lasering is as follows Figure 3 shown.

[0024] S3, cleaning and drying The steel substrate obtained in step S2 is washed three times with pure water, and then dried in a vacuum drying oven at 50° C. for 10 minutes.

[0025] S4, Steel substrate sandblasting Put the S3 treated steel substrate into the sandblasting machine (sandblasting pressure 150kg / cm 2 , sandblasting time 20s), 100-mesh corundum sand was used to treat the substrate surface, mainly to increase the surface roughness of the steel substrate and treat the oxide layer after laser blasting.

[0026] (4) Molding and sintering: the steel substrate of step (3) and the mixed material of step (2) are placed in a mold, spread and flattened, and then placed in an atmosphere sintering furnace for sintering and molding. The specific sintering process is: in a hydrogen atmosphere, at a sintering temperature of 800° C. and a sintering pressure of 10 MPa, heat preservation treatment for 4 hours, after the heat preservation is completed, the temperature is lowered to room temperature, and demolding is performed to obtain a grinding wheel blank; (5) Mechanical processing: The outer cylindrical end surface and inner hole of the grinding wheel blank of step 4) are processed. Based on the positioning of the inner hole, positioning holes (4 to 6 through holes with a diameter of 6.6 mm) are made on the steel substrate on one side of the abrasive layer working layer. After the grinding wheel is processed, the coaxiality of the abrasive layer and the substrate is ≤0.008 mm, the upper end surface of the abrasive layer working layer is at the same height as the substrate, and the parallelism with the bottom surface of the substrate is ≤0.015 mm, thereby obtaining a semi-finished grinding wheel; (6) Processing of effective grinding area of ​​abrasive layer: The abrasive layer is ground with resin super-hard grinding wheel and finished to 0.5mm thick × 4mm wide. Before processing, the end face runout of the substrate is ≤0.01mm. After processing, the end face runout of the abrasive layer is ≤0.015mm to be qualified.

[0027] (7) Dynamic balancing correction: On a high-precision dynamic balancing machine, the weight is removed by punching holes. The dynamic imbalance is ≤0.2g. The qualified one is the finished product.

[0028] The groove size of the processed ceramic workpiece is 0.5mm wide × 0.8mm deep. At a grinding wheel speed of 30m / s, 100 pieces can be processed continuously, and there is no edge collapse or cracks > 40μm on the workpiece groove. Each grinding wheel can process more than 1,000 pieces without trimming, and the groove shape is well maintained, meeting the customer's batch processing needs.

[0029] Example 2 The metal bond grinding wheel provided in this embodiment is adjusted in thickness of abrasive layer and ring width as compared with that in embodiment 1 as follows: The grinding wheel model used is 3A1 D200×T20.2×H24×E1.5×X10, where D represents the diameter of the grinding wheel, T represents the total thickness of the grinding wheel, H represents the diameter of the inner hole of the grinding wheel, E represents the thickness of the effective grinding area of ​​the abrasive layer, and X represents the total width of the abrasive layer, all in units of mm.

[0030] Compared with the preparation method of the metal bond grinding wheel in Example 1, some preparation parameters are adjusted as follows: In step (1), the L-shaped step of the steel substrate has a width of 10 mm and a depth of 2.5 mm; Step (4) forming and sintering: in a hydrogen atmosphere, at a sintering temperature of 850° C. and a sintering pressure of 15 MPa, heat preservation treatment is performed for 4 hours. After the heat preservation is completed, the temperature is lowered to room temperature and demolding is performed to obtain a grinding wheel blank; Step (6) Processing of effective grinding area of ​​abrasive layer: Grind the abrasive layer with a resin super-hard grinding wheel and finish it to 1.5 mm thick × 4 mm wide. Before processing, the end face runout of the substrate must be ≤0.01 mm. After processing, the abrasive layer runout must be ≤0.015 mm to be qualified.

[0031] The groove size of the processed ceramic workpiece is 1.5mm wide × 1.0mm deep. At a grinding wheel speed of 30m / s, 100 pieces can be processed continuously, and there is no edge collapse or cracks > 40μm on the workpiece groove. Each grinding wheel can process more than 1,000 pieces without trimming, and the groove shape is well maintained, meeting the customer's batch processing needs.

[0032] Example 3 The metal bond grinding wheel provided in this embodiment is adjusted in the following manner compared with that in Embodiment 1: The grinding wheel model used is 3A1 D250×T20.2×H24×E1.5×X10, where D represents the diameter of the grinding wheel, T represents the total thickness of the grinding wheel, H represents the diameter of the inner hole of the grinding wheel, E represents the thickness of the effective grinding area of ​​the abrasive layer, and X represents the total width of the abrasive layer, all in units of mm.

[0033] Compared with the preparation method of the metal bond grinding wheel in Example 1, some preparation parameters are adjusted as follows: In step (1), the L-shaped step of the steel substrate has a width of 10 mm and a depth of 2.5 mm; Step (4) forming and sintering: in a hydrogen atmosphere, at a sintering temperature of 950° C. and a sintering pressure of 25 MPa, heat preservation treatment is performed for 4 hours. After the heat preservation is completed, the temperature is lowered to room temperature and demolding is performed to obtain a grinding wheel blank; Step (6) Processing of effective grinding area of ​​abrasive layer: Grind the abrasive layer with a resin super-hard grinding wheel and finish it to 1.5 mm thick × 8 mm wide. Before processing, the end face runout of the substrate must be ≤0.01 mm. After processing, the abrasive layer runout must be ≤0.015 mm to be qualified.

[0034] The groove size of the processed ceramic workpiece is 1.5mm wide × 1.5mm deep. At a grinding wheel speed of 30m / s, 100 pieces can be processed continuously, and there is no edge collapse or cracks > 40μm on the workpiece groove. Each grinding wheel can process more than 1,000 pieces without trimming, and the groove shape is well maintained, meeting the customer's batch processing needs.

[0035] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the invention claimed for protection. The scope of protection claimed for the present invention is defined by the attached claims and their equivalents.

[0036] In the description of the present invention, it is necessary to understand that the terms "front", "rear", "left", "right", "center", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the protection content of the present invention.

Claims

1. A metal bond grinding wheel for grooving ceramic materials, characterized in that: The grinding wheel includes a substrate and an abrasive layer arranged on the surface of the substrate; the abrasive layer is made of a main abrasive and a metal binder, the main abrasive is diamond, and the metal binder is composed of the following components in percentage by mass: copper powder, tin powder, nickel powder, silver powder and graphite, and the weight parts of each raw material are as follows: 20-40 parts of diamond, 60-70 parts of copper powder, 10-20 parts of tin powder, 5-15 parts of nickel powder, 5-15 parts of silver powder, and 2-8 parts of graphite. The particle size of diamond is 35-91 μm, and each component of the metal binder is powdered, and the particle size is greater than or equal to 170 meshes.

2. The metal bond grinding wheel for grooving ceramic materials according to claim 1, characterized in that: The substrate is a toothless structure, and an L-shaped step is provided in the circumferential direction on the outer edge of the upper end surface of the substrate, with a step width of 5-10 mm and a depth of 1.0-2.0 mm. The L-shaped step is used to accommodate the abrasive layer.

3. The metal bond grinding wheel for grooving ceramic materials according to claim 1, characterized in that: The total width of the abrasive layer is 5~10mm, the thickness of the effective grinding area is 0.5mm~1.5mm, and the width of the effective grinding area is 2~4mm.

4. The method for preparing a metal bond grinding wheel for grooving ceramic materials according to any one of claims 1 to 3, characterized in that: The process is as follows: (1) Matrix processing: rough turning of the matrix, flat grinding of the matrix, and fine turning of the matrix to produce an L-shaped step; (2) Mixing: Mix the components of the metal binder, the main abrasive and the wetting agent for 2 to 5 hours to obtain a mixture; (3) Substrate pretreatment: After cleaning the substrate, perform laser treatment, and then perform sandblasting after cleaning and drying; (4) Molding and sintering: the substrate of step (3) and the mixed material of step (2) are put into a mold, spread and flattened, and then placed in an atmosphere sintering furnace for sintering and molding. The specific sintering process is: in a hydrogen atmosphere, at a sintering temperature of 800-950° C. and a sintering pressure of 10-15 MPa, heat preservation treatment for 1-2 h, after the heat preservation is completed, the temperature is lowered to room temperature, and demolding is performed to obtain a grinding wheel blank; (5) Mechanical processing: machining the outer cylindrical end surface and inner hole of the grinding wheel blank in step (4), making a positioning hole on the steel substrate on one side of the abrasive layer based on the positioning of the inner hole, and finally obtaining a semi-finished grinding wheel; (6) Processing of effective grinding area of ​​abrasive layer: Use resin super-hard grinding wheel to grind the abrasive layer of the semi-finished grinding wheel in step (5) so that the effective grinding area is finely processed to 0.5mm~1.5mm thick × 2mm~4mm wide. Before processing, the end face runout of the substrate is ≤0.01mm before processing. After processing, the end face runout of the abrasive layer is ≤0.015mm to be qualified; (7) Dynamic balancing correction: On a high-precision dynamic balancing machine, the weight is removed by punching holes. The dynamic imbalance is ≤0.2g. The qualified one is considered a finished product.

5. The preparation method according to claim 4, characterized in that: The specific process of step (3) is as follows: S1. The substrate is acid-washed in 90-95wt% nitric acid for 5-10 min, then cleaned with distilled water, then alkaline-washed in 40-50wt% NaOH aqueous solution for 5-10 min, then cleaned with distilled water, and dried; S2, placing the substrate dried in step S1 into a laser machine, and lasering a uniform hemispherical pit on the bottom surface of the L-shaped step, wherein the radius of the hemispherical pit is 0.1-0.3 mm; S3, washing the substrate obtained in step S2 with pure water and drying; S4. Place the substrate treated in S3 into a sandblasting machine and use 80-150 mesh corundum sand to treat the surface of the substrate.

6. The preparation method according to claim 5, characterized in that: There are 5 to 10 hemispherical pits radially distributed on the bottom of the L-shaped step, and the sandblasting pressure is 100 to 200 kg / cm 2 , sandblasting time 10~30 s.

7. The preparation method according to claim 4, characterized in that: In step (2), the wetting agent is liquid paraffin. Based on the total weight of the main abrasive and the metal binder, 10 to 20 mL of liquid paraffin needs to be added for every 1 kg.

8. The preparation method according to claim 4, characterized in that: In step (5), the positioning holes are countersunk holes with a diameter of 6 to 7 mm, and 4 to 6 positioning holes are evenly distributed along the circumference of the inner hole of the working surface of the substrate abrasive layer.

9. The preparation method according to claim 4, characterized in that: In step (5), after the grinding wheel is processed, the coaxiality between the abrasive layer and the substrate is ≤0.008 mm, the upper end surface of the working layer of the abrasive layer is at the same height as the substrate, and the parallelism with the bottom surface of the substrate is ≤0.015 mm.

Citation Information

Patent Citations

  • Diamond-coated tool

    CN102257176A

  • Diamond grinding wheel and manufacturing method thereof

    CN107598787A

  • Butterfly wing-desert beetle bionic grinding head preparation process and grinding head

    CN118181170A

  • Flat grinding wheel and flat grinding wheel base body

    CN203156584U

  • Super-abrasive grinding wheel and manufacture thereof

    JP1998109270A