Wafer processing method
By fixing the wafer with the annular frame without using a sheet of paste layer, and dividing and removing the annular convex parts on the retaining table, the problem of fragmentation and scattering during the removal of the annular convex parts during wafer processing is solved, and the problem of fragmentation and scattering is achieved. High-quality and efficient wafer processing.
Patent Information
- Application Number
- CN202410614165.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-26
AI Technical Summary
During the wafer processing process, fragmentation and processing chips are easily generated during the removal of the annular convex parts, resulting in reduced quality and low productivity. The existing methods require the reduction of the device formation area to reduce the adhesive force of the adhesive tape, which affects the influence of the Split quality.
The wafer is fixed with the annular frame by using a sheet without a paste layer, and the wafer unit is formed by hot pressing, and the annular convex parts are divided and removed on the retaining table to avoid adhesion and debris adhesion, and to improve the removal of annular convex parts. convenience and quality of the device chip.
High-quality and high-productivity wafer processing is achieved, preventing paste and debris problems, improving the stability and production efficiency of device chips, and reducing the need for narrowing the device formation area.
Smart Images

Figure CN119017569A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for processing a wafer having a back surface having an annular convex portion on the outer periphery and a circular concave portion formed in a region surrounded by the annular convex portion. Background Art
[0002] Device chips are mounted in electronic devices such as mobile phones and personal computers. Device chips are generally manufactured by grinding a wafer having a plurality of devices such as ICs (Integrated Circuits) formed on the front side from the back side to thin it, and dividing the wafer into individual devices.
[0003] The wafer thinned by grinding has a reduced rigidity and is easily broken. Therefore, a region corresponding to a device forming region where a plurality of devices are formed on the back side of the wafer is ground to form a circular concave portion, and the periphery of the circular concave portion is left as an annular convex portion. The annular convex portion serves to reinforce the thinned circular concave portion during wafer transport, etc. (for example, refer to Patent Document 1).
[0004] On the other hand, when the wafer is divided into individual chips, the annular convex portion hinders the division, so it is necessary to remove the annular convex portion from the wafer in advance. When removing the annular convex portion, an adhesive tape is pasted on the entire area of the back side of the wafer including the circular concave portion and the annular convex portion, and the wafer is held on the holding table through the adhesive tape. The holding table has a convex shape corresponding to the circular concave portion of the wafer, and the circular concave portion is consistent with the convex shape. Then, an annular breaking groove is formed on the wafer held by the holding table, and the annular convex portion is removed (for example, refer to patent document 2).
[0005] In addition, as another method for removing the annular protrusion from the chip, the following method is known: sticking adhesive tape on the front side of the chip, using a flat holding workbench to suck and hold the chip through the adhesive tape, and forming a disconnection groove on the chip to cut off the annular protrusion (for example, refer to patent document 3).
[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-173487
[0007] Patent Document 2: Japanese Patent Application Publication No. 2011-61137
[0008] Patent Document 3: Japanese Patent Application Publication No. 2012-54275
[0009] In the case of removing the annular protrusion by any method, an annular frame is attached to the outer periphery of the adhesive tape attached to the wafer. At this time, the wafer is accommodated in the opening formed in the annular frame. Then, when the wafer is processed to form the disconnection groove, processing chips are generated from the wafer and the like and fly around. A part of the scattered processing chips will adhere to the adhesive tape exposed in the opening of the annular frame. In addition, sometimes during the transportation or processing of the wafer, a part of the processing chips will fly again and adhere to the wafer, which becomes a problem.
[0010] In addition, after the annular convex portion is cut off by forming a break groove on the wafer, the cut annular convex portion is peeled off from the adhesive tape. However, since the annular convex portion is strongly adhered to the adhesive tape having the paste layer before being separated from the wafer, a large force is required to peel the annular convex portion from the adhesive tape. In addition, a large force is applied to the annular convex portion, and the annular convex portion may break, and the fragments may fly to the wafer.
[0011] Therefore, it is considered to stick an adhesive tape having a paste layer whose adhesive force is reduced by ultraviolet irradiation on the wafer and the annular frame. In this case, when the annular convex portion cut from the wafer is peeled off from the adhesive tape, ultraviolet rays are irradiated to the adhesive tape in the area overlapping with the annular convex portion to reduce the adhesive force of the paste layer. At this time, a shielding member is used so as not to irradiate the ultraviolet rays to the area overlapping with the circular concave portion.
[0012] However, in order to irradiate the area overlapping the annular protrusion with ultraviolet light with sufficient intensity, the size of the area that can be shielded by the shielding member is limited. Therefore, ultraviolet light is also irradiated to the adhesive tape in the area overlapping the outer periphery of the circular concave portion, and the adhesive force of the adhesive tape in this area is reduced. When the wafer is divided in the portion where the adhesive force of the adhesive tape is reduced, the wafer cannot be fully supported in this portion, so the processing becomes low-quality. Therefore, it is necessary to reduce the area on the front side of the wafer for device formation, and productivity is reduced. Summary of the invention
[0013] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a wafer processing method for processing a wafer having an annular convex portion with high quality and high productivity.
[0014] According to one embodiment of the present invention, a method for processing a chip is provided, wherein the chip has an annular protrusion on the outer peripheral portion of the back side, and a circular recess is formed in the area of the back side surrounded by the annular protrusion, wherein the method for processing the chip includes the following steps: a chip unit forming step, wherein a sheet without a paste layer is fixed on the front side of the chip and an annular frame is fixed on the outer peripheral portion of the sheet to form a chip unit; a holding step, wherein after the chip unit forming step, the chip is held by a holding workbench via the sheet; a disconnecting step, wherein after the holding step, a disconnecting groove is formed in the circular recess of the chip to separate the annular protrusion from the chip; and a removing step, wherein after the disconnecting step, the annular protrusion is removed from the sheet.
[0015] Preferably, in the wafer unit forming step, the sheet is heated and pressed to be thermocompressed onto the wafer, thereby fixing the sheet onto the wafer.
[0016] In a wafer processing method according to one embodiment of the present invention, a wafer unit is formed by fixing a sheet having no paste layer to a wafer and an annular frame. The sheet has no paste layer, so even if processing chips generated when forming a break groove on the wafer come into contact with the sheet, the processing chips will not adhere to the sheet. Furthermore, even if fragments generated by the damage of the annular convex portion when removing the annular convex portion from the sheet come into contact with the sheet, the fragments will not adhere to the sheet. In addition, the processing chips and fragments that come into contact with the sheet can be easily removed from the sheet by washing.
[0017] In addition, unlike the case where the adhesive tape is strongly adhered to by the paste layer, the annular convex portion is easier to remove when it is fixed to a sheet without a paste layer. Therefore, no large force is applied to the removed annular convex portion, and it is not easy to be damaged or fragmented. Therefore, the processing chips and fragments that come into contact with the sheet will not be transferred to the wafer (device chip) to reduce the quality of the device chip.
[0018] Furthermore, there is no need to irradiate the wafer with ultraviolet rays in order to remove the annular convex portion from the wafer, nor is there a need to narrow the region for device formation on the front surface of the wafer on the premise of irradiating ultraviolet rays. Therefore, the productivity of device chips is also improved.
[0019] Therefore, according to one embodiment of the present invention, there is provided a wafer processing method for processing a wafer having an annular convex portion with high quality and high productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 (A) is a perspective view schematically showing the back side of a wafer, Figure 1 (B) is a perspective view schematically showing the front side of the wafer.
[0021] Figure 2 (A) is a cross-sectional view schematically showing a thermal compression bonding device, Figure 2 (B) is a cross-sectional view schematically showing a thermocompression bonding device in the first stage of the wafer unit forming step.
[0022] Figure 3 (A) is a cross-sectional view schematically showing a thermocompression bonding device in the second stage of the wafer unit forming step, Figure 3 (B) is a cross-sectional view schematically showing the thermocompression bonding device in the third stage of the wafer unit forming step.
[0023] Figure 4 : is a cross-sectional view schematically showing the thermocompression bonding device in the fourth stage of the wafer unit forming step.
[0024] Figure 5 is a perspective view schematically showing a wafer unit.
[0025] Figure 6 (A) is a perspective view schematically showing a wafer unit in a holding step, Figure 6 (B) is a cross-sectional view schematically showing the wafer unit in the holding step.
[0026] Figure 7 (A) is a perspective view schematically showing a wafer unit in a breaking step, Figure 7 (B) is a cross-sectional view schematically showing the wafer unit in the breaking step.
[0027] Figure 8 (A) is a perspective view schematically showing a wafer unit in a removal step, Figure 8 (B) is a cross-sectional view schematically showing the wafer unit in the removal step.
[0028] Fig. 9 It is a flowchart showing the flow of each step of the wafer processing method according to the embodiment.
[0029] Description of symbols
[0030] 11: wafer; 11a: front side; 11b: back side; 13: annular convex part; 15: circular concave part; 17: step difference part; 19: predetermined dividing line; 21: device; 23: peripheral remaining area; 25: device forming area; 27: sheet; 29: annular frame; 29a: opening; 31: wafer unit; 33: disconnection groove; 2: hot pressing device; 4: upper chamber; 6: lower chamber; 8: first concave part; 10: second concave part; 12: first opening; 14: second opening; 16, 18: internal space; 20: first decompression unit; 22: second decompression unit; 24: exhaust part; 26: exhaust part; 28: first solenoid valve; 30: first Two solenoid valves; 32: holding table; 34: holding surface; 34a: circular convex portion; 34b: annular support portion; 36: heater; 38: cutting device; 40: holding table; 42: frame; 44: porous component; 46: holding surface; 48: fixture; 50: cutting unit; 52: spindle housing; 54: spindle; 56: cutting tool; 58: cutting blade; 60: removal unit; 62: arm; 64: bottom plate; 66: removal claw unit; 68: direct-acting mechanism; 70: advance and retract rod; 72: moving block; 74: rod for rotating axis; 76: bearing; 78: removal claw; 78a: upper claw; 78b: lower claw; 78c: connecting portion. DETAILED DESCRIPTION
[0031] An embodiment of one aspect of the present invention will be described with reference to the drawings. Figure 1 (A) is a perspective view schematically showing the back side 11b of the wafer 11. Figure 1 (B) is a perspective view schematically showing the front surface 11a side of the wafer 11. First, the wafer 11 processed by the wafer processing method of the present embodiment will be described.
[0032] The wafer 11 is a disk-shaped single crystal substrate formed of a semiconductor material such as silicon (Si) or silicon carbide (SiC). However, the shape, structure, size, etc. of the wafer 11 are not limited. Figure 1 As shown in FIG. 1B , a plurality of planned dividing lines 19 are set in a grid pattern on the front surface 11 a of the wafer 11. In each region partitioned by the plurality of planned dividing lines 19, a device 21 such as an IC or LSI is formed.
[0033] The peripheral region surrounding the region where the plurality of devices 21 are formed on the front surface 11a of the wafer 11 is referred to as the peripheral surplus region 23. The region where the plurality of devices 21 are formed on the front surface 11a of the wafer 11 surrounded by the peripheral surplus region 23 is referred to as the device formation region 25.
[0034] When the wafer 11 having a plurality of devices 21 formed thereon is ground and thinned from the back side 11b and the wafer 11 is divided along the predetermined dividing line 19, a plurality of thin device chips each having a device 21 are obtained. The division of the wafer 11 is performed, for example, by a cutting device having an annular cutting blade. However, the rigidity of the wafer 11 thinned by grinding is reduced and it is easy to break, and handling such as transportation is not easy.
[0035] Therefore, if Figure 1 As shown in (A), a region corresponding to the device forming region 25 where a plurality of devices 21 are formed in the back surface 11b of the wafer 11 is ground to form a circular concave portion 15, and the periphery of the circular concave portion 15 is left as an annular convex portion 13. The annular convex portion 13 has the function of reinforcing the thinned circular concave portion 15 during the conveyance of the wafer 11, etc. Thus, the rigidity of the wafer 11 is maintained, and it is not easy to cause warping, cracking, etc., and it is easy to handle.
[0036] However, when the wafer 11 having the annular protrusion 13 on the back side 11b is to be directly divided along the planned dividing line 19 by a cutting device, the thick annular protrusion 13 cannot be cut off by the breaking groove formed in the wafer 11 in the same manner as the thin circular concave portion 15. In other words, the annular protrusion 13 becomes an obstacle to dividing the wafer 11 into individual chips.
[0037] Therefore, the annular convex portion 13 needs to be removed from the wafer 11 before dividing the wafer 11. In the wafer processing method of this embodiment, a sheet without a paste layer is fixed to the entire area of the front surface 11a of the wafer 11 by a method such as thermocompression bonding. The wafer 11 is held via the sheet by a holding table of the dividing device.
[0038] Next, the sheet fixed to the wafer 11 will be described. Figure 3 (A) and the like include cross-sectional views schematically showing the sheet 27. Figure 5 The sheet 27 is schematically shown in FIG. 1 and FIG. 2 . The sheet 27 has a diameter larger than the outer diameter of the wafer 11 and has no paste layer. The sheet 27 is a thermoplastic sheet.
[0039] The outer periphery of the sheet 27 is disposed on a metal annular frame 29 (see Figure 5 The sheet 27 is, for example, a flexible resin sheet such as a polyolefin sheet or a polyester sheet, but the material of the sheet 27 is not limited thereto.
[0040] Here, the polyolefin-based sheet is a sheet of a polymer synthesized using olefin as a monomer. The polyolefin-based sheet used for the sheet 27 is, for example, a polyethylene sheet, a polypropylene sheet, a polystyrene sheet, or other sheet that is transparent or translucent to visible light.
[0041] The polyester sheet is a polymer sheet 27 synthesized from dicarboxylic acid (a compound having two carboxyl groups) and diol (a compound having two hydroxyl groups) as monomers. The polyester sheet used for the sheet 27 is, for example, a sheet 27 transparent or translucent to visible light, such as a polyethylene terephthalate sheet or a polyethylene naphthalate sheet.
[0042] From another point of view, the sheet 27 without a paste layer fixed to the wafer 11 by thermocompression bonding has a storage elastic modulus of 1×10 6 Pa~1×10 9 Pa and the storage modulus when heated is 1×10 6 Pa~1×10 7 Thermoplastic resin Pa. Here, the heating time refers to the temperature when the sheet 27 is thermocompressed to the wafer 11. For example, when the sheet 27 is polyolefin, the temperature can be set to 80°C to 100°C.
[0043] Among them, the storage modulus of the thermoplastic resin used as the constituent material of the sheet 27 can be evaluated using a viscoelasticity measuring device "DMA 7100" produced by Hitachi High-Technologies Co., Ltd. This viscoelasticity measuring device applies periodic deformation to a sample and measures the stress or strain generated thereby, thereby being able to calculate the temperature dependence and frequency dependence of storage modulus, loss modulus, loss tangent (tan δ), etc. as the viscoelastic properties of the sample.
[0044] The storage modulus of the thermoplastic resin measured by the viscoelasticity measuring device can be measured, for example, under the conditions of a heating rate of 2°C / min, a measurement temperature range of from room temperature to 200°C, and a deformation frequency of 1 Hz. However, the measurement conditions of the storage modulus are not limited thereto. In addition, the storage modulus can also be measured using other measuring devices.
[0045] The sheet 27 does not have a paste layer (adhesive layer) and does not have sufficient adhesiveness, so it cannot be directly attached to the wafer 11 and the ring frame 29 in this state. The sheet 27 has thermoplasticity, and when heated to a temperature near the melting point while the sheet 27 and the wafer 11 are bonded together under a predetermined pressure, it can be partially melted and fixed to the wafer 11. That is, the sheet 27 can be thermally pressed to the wafer 11.
[0046] In addition, if Figure 5 As shown, the outer periphery of the sheet 27 is fixed to the metal annular frame 29. The annular frame 29 has an opening (through hole) 29a having a diameter larger than that of the wafer 11. For example, the sheet 27 is fixed to the annular frame 29 before the wafer 11. The method of fixing the sheet 27 to the annular frame 29 is, for example, thermocompression bonding. For example, the sheet 27 is thermocompressed together with the wafer 11 to the annular frame 29. Alternatively, the sheet 27 is bonded to the annular frame 29 by bonding with an adhesive material or the like.
[0047] When the wafer 11, the sheet 27 and the annular frame 29 are finally integrated, a wafer unit 31 is formed (see Figure 5 When the wafer unit 31 is formed, the wafer 11 is handled by the sheet 27, so the handling of the wafer 11 becomes easy. In addition, when the wafer 11 that becomes a part of the wafer unit 31 is divided, the formed individual device chips continue to be supported by the sheet 27, so the handling of the device chips also becomes easy.
[0048] Next, the thermocompression bonding device 2 used when the sheet 27 is fixed to the wafer 11 in the wafer processing method of the present embodiment will be described. However, in the wafer processing method of the present embodiment, the thermocompression bonding device 2 may not be used when the sheet 27 is fixed to the wafer 11. Figure 2 (A) to Figure 4 A cross-sectional view schematically showing the thermocompression bonding device 2 is included.
[0049] Figure 2 (A) is a cross-sectional view schematically showing an example of a thermocompression bonding device 2. The thermocompression bonding device 2 is, for example, a chamber-shaped unit having a space inside which can accommodate a wafer 11, and has a function of thermocompression bonding the sheet 27 to the front surface 11a of the wafer 11. The thermocompression bonding device 2 has a concave lower chamber 6 opened upward and a concave upper chamber 4 disposed above the lower chamber 6 and opened downward.
[0050] The upper chamber 4 of the thermocompression bonding device 2 has a first recessed portion 8 connected to the first decompression unit 20 and having a first opening 12. The lower chamber 6 has a second recessed portion 10 connected to the second decompression unit 22 and having a second opening 14. The first decompression unit 20 and the second decompression unit 22 are, for example, vacuum pumps such as rotary pumps. However, the first decompression unit 20 and the second decompression unit are not limited thereto.
[0051] The thermocompression bonding device 2 has a holding table 32 disposed in the second recess 10 to hold the wafer 11. The upper chamber 4 and the lower chamber 6 can be closed by aligning the first opening 12 of the upper chamber 4 and the second opening 14 of the lower chamber 6.
[0052] The thermocompression bonding device 2 is described in more detail. The first opening 12 of the upper chamber 4 and the second opening 14 of the lower chamber 6 have an inner diameter larger than the diameter of the wafer 11. In addition, the first recess 8 of the upper chamber 4 and the second recess 10 of the lower chamber 6 have an outer diameter smaller than the inner diameter of the annular frame 29 provided on the outer periphery of the sheet 27.
[0053] For example, the upper chamber 4 can be raised and lowered. The second opening 14 of the lower chamber 6 is of the same shape as the first opening 12 of the upper chamber 4, and when the upper chamber 4 is lowered toward the lower chamber 6 in a manner that the first opening 12 overlaps with the second opening 14, a space isolated from the outside can be formed inside the upper chamber 4 and the lower chamber 6.
[0054] A table-shaped holding table 32 for supporting the wafer 11 is provided in the lower chamber 6. The wafer 11 is placed on the holding table 32 with the back surface 11b on which the annular convex portion 13 and the circular concave portion 15 are formed facing downward.
[0055] The upper surface of the holding table 32 is a holding surface 34 that supports and holds the wafer 11 from the back surface 11b side. The holding table 32 may also include a suction path (not shown) communicating with the holding surface 34 and a suction source (not shown) connected to the suction path. In this case, when the suction force generated by the suction source is applied to the wafer 11 placed on the holding surface 34 of the holding table 32 through the suction path, the wafer 11 can be held by suction using the holding table 32.
[0056] The holding table 32 mainly includes a circular protrusion 34 a that supports the circular recess 15 on the back surface 11 b of the wafer 11 , and an annular support portion 34 b that is disposed on the outer periphery of the circular protrusion 34 a and mainly supports the annular protrusion 13 of the wafer 11 .
[0057] The planar shape of the upper surface of the circular protrusion 34a is a shape that can accommodate the circular recess 15 of the wafer 11, and is a shape slightly smaller than the circular recess 15. The annular support portion 34b has a width (the distance between the inner periphery and the outer periphery) that is larger than the width (the distance between the inner periphery and the outer periphery) of the annular protrusion 13 of the wafer 11. The height difference between the upper surface of the annular support portion 34b and the upper surface of the circular protrusion 34a is equivalent to the height difference between the circular recess 15 and the annular protrusion 13 of the wafer 11. That is, the difference is based on the step difference portion 17 (see Figure 1 (B)) is appropriately determined based on the height.
[0058] A spacer (not shown) is disposed on the upper surface of the annular support portion 34b. The spacer is formed of an elastic member such as a resin layer, and its thickness varies in accordance with the deviation of the height difference between the circular concave portion 15 and the annular convex portion 13 of the wafer 11 (the height of the step portion 17). That is, the holding table 32 can appropriately hold the wafer 11 in accordance with the deviation of the height difference between the circular concave portion 15 and the annular convex portion 13 of the wafer 11.
[0059] The height of the holding table 32 is adjusted so that the front surface 11a of the wafer 11 is substantially the same height as the second opening 14 of the lower chamber 6 when the wafer 11 is placed on the holding surface 34. Alternatively, the height of the holding table 32 is adjusted so that the second opening 14 of the lower chamber 6 is higher than the front surface 11a of the wafer 11.
[0060] An exhaust section 24 is connected to the top or side wall of the upper chamber 4. The exhaust section 24 is an exhaust path connected to the first recess 8 of the upper chamber 4 at one end and connected to the first decompression unit 20 at the other end. A first electromagnetic valve 28 (e.g., an electromagnetic valve) for switching the connection state between the upper chamber 4 and the first decompression unit 20 is provided on the exhaust path of the exhaust section 24. That is, when the first electromagnetic valve 28 is actuated, the connection state between the upper chamber 4 and the first decompression unit 20 and the disconnection state in which they are disconnected from each other are switched.
[0061] An exhaust portion 26 is connected to the bottom wall or the side wall of the lower chamber 6. The exhaust portion 26 is an exhaust path connected to the second recess 10 of the lower chamber 6 at one end and connected to the second decompression unit 22 at the other end. A second electromagnetic valve 30 (e.g., an electromagnetic valve) for switching the connection state between the lower chamber 6 and the second decompression unit 22 is provided on the exhaust path of the exhaust portion 26. That is, when the second electromagnetic valve 30 is actuated, the connection state of the lower chamber 6 and the second decompression unit 22 and the disconnection state of being disconnected from each other are switched.
[0062] When the first solenoid valve 28 is operated to connect the first decompression unit 20 and the upper chamber 4, the internal space 16 of the upper chamber 4 can be decompressed. In addition, when the second solenoid valve 30 is operated to connect the second decompression unit 22 and the lower chamber 6, the internal space 18 of the lower chamber 6 can be decompressed.
[0063] The thermocompression bonding device 2 has a heating unit for heating the wafer 11 placed on the holding table 32 and the sheet 27 placed on the wafer 11. For example, a heater 36 that can function as a heating unit is provided inside the holding table 32. The heater 36 is, for example, an electric heating wire. When the heater 36 is operated, the wafer 11 is heated, and the sheet 27 is heated through the wafer 11.
[0064] However, the heating unit of the thermal compression bonding device 2 is not limited thereto. For example, a heating unit (not shown) that supplies hot air to the internal space 16 of the upper chamber 4 may be provided in the first recess 8 of the upper chamber 4. The heating unit includes, for example, a blower that generates air flow and a heater that can heat the air. The wafer 11 is placed on the holding table 32 and the sheet 27 is arranged on the wafer 11. When hot air is supplied to the sheet 27 from the heating unit, the sheet 27 can be heated.
[0065] Next, a cutting device for removing the annular convex portion 13 of the wafer 11 in the wafer processing method of the present embodiment will be described. Figure 7 (A) includes a perspective view schematically showing a cutting device, Figure 7 (B) includes a cross-sectional view schematically showing a cutting device.
[0066] The cutting device 38 includes a holding table 40 that holds the wafer 11 (wafer unit 31 ) and a cutting unit 50 that cuts the wafer 11 held by the holding table 40 .
[0067] The holding table 40 includes a porous member 44 having a circular upper surface of the same size as the front surface 11a of the wafer 11, and a frame 42 that accommodates the porous member 44 so that the porous member 44 is exposed upward. The frame 42 has a storage recess on the upper surface for accommodating the porous member 44. A suction path (not shown) is formed inside the frame 42, one end of which is connected to the porous member 44, and the other end is connected to a suction source (not shown) such as an ejector.
[0068] When the wafer 11 (wafer unit 31) is placed on the holding table 40 and the suction source is activated, negative pressure is applied to the wafer 11 through the suction path and the porous member 44. That is, the wafer 11 is sucked and held on the holding table 40 via the sheet 27. The upper surface of the holding table 40 serves as a holding surface 46.
[0069] In addition, a rotation drive source such as a motor (not shown) is connected to the holding table 40, and the rotation drive source rotates the holding table 40 around a rotation axis that is substantially parallel to the holding surface 46. In addition, a plurality of clamps 48 may be provided around the holding table 40 to hold and fix the annular frame 29 that supports the wafer 11 via the sheet 27.
[0070] A cutting unit 50 for cutting the wafer 11 is disposed above the holding table 40. The cutting unit 50 has a cylindrical spindle 54 disposed in a direction substantially parallel to the holding surface 46 of the holding table 40. An annular cutting tool 56 for cutting the wafer 11 is mounted at the front end (one end) of the spindle 54.
[0071] In addition, the base end portion (the other end side) of the spindle 54 is rotatably accommodated in the spindle housing 52. A rotational drive source (not shown) such as a motor is accommodated in the spindle housing 52, and the rotational drive source (not shown) is connected to the base end portion of the spindle 54. The cutting tool 56 is rotated by the power transmitted from the rotational drive source via the spindle 54.
[0072] As the cutting tool 56 mounted on the front end of the spindle 54, for example, a hub-type cutting tool (hub tool) is used. The hub tool is composed of an annular base made of metal or the like and an annular cutting blade 58 formed along the outer periphery of the base. In addition, the cutting blade 58 of the hub-type cutting tool is composed of an electroformed grinder, and the electroformed grinder has abrasive grains made of diamond or the like fixed by a bonding material such as a nickel plating layer.
[0073] However, a washer-type cutting tool (waster tool) can also be used as the cutting tool 56. The washer tool is composed of an annular cutting edge 58 obtained by fixing abrasive grains through a bonding material composed of metal, ceramic, resin, etc. Regardless of whether it is a hub type or a washer type, the cutting tool 56 can cut the wafer 11 using the annular cutting edge 58.
[0074] The cutting unit 50 is connected to a moving unit (not shown) to adjust the position of the cutting tool 56 cutting into the wafer 11. The cutting unit 50 is connected to a lifting unit (not shown) to change the height position of the lower end of the annular cutting blade 58.
[0075] Next, a description will be given of a removal unit for removing the annular convex portion 13 cut from the wafer 11 from the sheet 27 in the wafer processing method of the present embodiment. Figure 8 (B) includes a cross-sectional view schematically showing the removal unit 60. Figure 8 (A) includes a perspective view schematically showing a part of the structure of the removal unit 60.
[0076] The removal unit 60 has a cylindrical arm 62 disposed substantially parallel to the height direction. The arm 62 can be moved in the height direction and in the horizontal direction by, for example, a ball screw type height direction moving mechanism (not shown) and a horizontal direction moving mechanism (not shown), respectively.
[0077] The center portion of the disk-shaped bottom plate 64 is connected to the lower end portion of the arm portion 62 so as to be rotatable relative to the arm portion 62. A rotation drive source (not shown) such as a motor is built into the arm portion 62. The rotation drive source rotates the bottom plate 64 in a predetermined direction.
[0078] A plurality of removal claw units 66 are provided on the upper portion of the bottom plate 64. Each removal claw unit 66 includes a direct-acting mechanism 68. The direct-acting mechanism 68 includes a ball screw mechanism (not shown) for advancing and retracting the advancing and retracting rod 70.
[0079] The advance / retract rod 70 includes a nut portion (not shown) connected in a manner that allows sliding relative to the guide portion of the direct-acting mechanism 68. The nut portion is connected to a ball screw (not shown) of the direct-acting mechanism 68 in a rotatable manner. The direct-acting mechanism 68 is used to advance / retract the nut portion, so that the advance / retract rod 70 advances / retracts along the length direction. In this embodiment, a plurality of advance / retract rods 70 are provided. The positions of the plurality of advance / retract rods 70 are point-symmetrical with the arm portion 62 as the center.
[0080] A longitudinal end (base end) of a rectangular parallelepiped moving block 72 is fixed to the front end of the reciprocating rod 70. The reciprocating rod 70 is fixed to the moving block 72 so that the longitudinal direction of the reciprocating rod 70 and the longitudinal direction of the moving block 72 are perpendicular to each other in a horizontal plane.
[0081] A cylindrical rotating shaft rod 74 is fixed to the other end (front end) of the moving block 72 so as to extend vertically downward. A removal claw 78 is rotatably connected to the lower end of the rotating shaft rod 74 via a bearing 76 .
[0082] The removal claw 78 includes a disc-shaped upper claw 78a and a lower claw 78b, and a cylindrical connecting portion 78c connecting the center portions of the upper claw 78a and the lower claw 78b. The upper claw 78a and the lower claw 78b are fixed by the connecting portion 78c.
[0083] In this embodiment, if Figure 8 As shown in (A), the three removal claws 78 are arranged at approximately equal intervals and separated from each other along the circumferential direction of the bottom plate 64, and the three lower claws 78b are used to peel the annular protrusion 13 from the sheet 27 and support the peeled annular protrusion 13 at three points. However, in the removal unit 60, the number of the removal claws 78 is not limited to three, and the removal unit 60 may have the removal claws 78 in the number of four or more.
[0084] Next, each step of the wafer processing method of the present embodiment will be described in detail. The wafer processing method of the present embodiment is implemented as a part of a device chip manufacturing method of dividing the wafer 11 into device chips, for example. Fig. 9 This is a flowchart showing the flow of each step of a wafer processing method (device chip manufacturing method). Hereinafter, the wafer processing method of this embodiment will be described, and the following description is also a description of each step of the device chip manufacturing method.
[0085] In the wafer processing method of the present embodiment, first, a wafer unit forming step S10 is performed. In the wafer unit forming step S10, a sheet 27 having no paste layer is fixed on the front surface 11a of the wafer 11, and an annular frame 29 is fixed to the outer peripheral portion of the sheet 27, thereby forming a wafer unit 31. The wafer unit forming step S10 is described in stages below.
[0086] Figure 2 (B) is a cross-sectional view schematically showing the thermal compression bonding device 2 and the wafer 11 in the first stage of the wafer unit forming step S10. In the first stage of the wafer unit forming step S10, the back side 11b of the wafer 11 is oriented downward, and the wafer 11 is moved above the holding table 32 so that the back side 11b of the wafer 11 faces the holding surface 34 of the holding table 32.
[0087] Then, the wafer 11 is placed on the holding surface 34 of the holding table 32, and the suction source of the holding table 32 is operated to hold the wafer 11 by suction. More specifically, the circular concave portion 15 on the back side 11b of the wafer 11 is placed on the circular convex portion 34a of the holding table 32, and the annular convex portion 13 on the back side 11b of the wafer 11 is placed on the annular support portion 34b of the holding table 32, and the wafer 11 is held by suction by the holding table 32. At this time, the front side 11a of the wafer 11 is exposed upward, and the front side 11a is the surface to be thermally pressed with the sheet 27.
[0088] Next, as the second stage of the wafer unit forming step S10 , the sheet 27 is sandwiched between the upper chamber 4 and the lower chamber 6 of the thermocompression bonding device 2 , and the internal space 16 of the upper chamber 4 and the internal space 18 of the lower chamber 6 are sealed. Figure 3 (A) is a cross-sectional view schematically showing the thermocompression bonding device 2 in the second stage of the wafer unit forming step S10.
[0089] Alternatively, the ring frame 29 may be fixed in advance to the outer periphery of the sheet 27 (see Figure 5 The fixing of the sheet 27 to the annular frame 29 is performed by thermocompression bonding by heating the sheet 27 and pressing it onto the annular frame 29. Alternatively, thermocompression bonding of the sheet 27 to the annular frame 29 and thermocompression bonding of the sheet 27 to the wafer 11 may be performed simultaneously.
[0090] Alternatively, the sheet 27 may be fixed to the annular frame 29 by bonding the annular frame 29 and the sheet 27 with the adhesive material sandwiched therebetween. Alternatively, the sheet 27 may have a paste layer only on the outer periphery and be bonded to the annular frame 29 via the paste layer.
[0091] In the second stage of the wafer unit forming step S10, a frame unit is placed in the lower chamber 6, and the frame unit includes: an annular frame 29 having an opening 29a in the center capable of accommodating the wafer 11; and a sheet 27 whose outer periphery is fixed to the annular frame 29. At this time, the second opening 14 of the lower chamber 6 is blocked by the sheet 27. In addition, at this time, the position of the annular frame 29 is adjusted so that the annular frame 29 does not overlap with the first opening 12 and the second opening 14.
[0092] Then, the upper chamber 4 is lowered, and the sheet 27 of the wafer unit 31 is clamped by the first opening 12 of the first recess 8 and the second opening 14 of the second recess 10 inside the opening 29a of the annular frame 29, and the first recess 8 and the second recess 10 are closed. At this time, the internal space 16 of the upper chamber 4 is sealed by the sheet 27 and the first recess 8. In addition, the internal space 18 of the lower chamber 6 is sealed by the sheet 27 and the second recess 10.
[0093] Next, as the third stage of the wafer unit forming step S10 , the first recess 8 is depressurized by the first depressurizing unit 20 , and the second recess 10 is depressurized by the second depressurizing unit 22 . Figure 3 (B) is a cross-sectional view schematically showing the thermocompression bonding device 2 in the third stage of the wafer unit forming step S10.
[0094] In the third stage of the wafer unit forming step S10, the first electromagnetic valve 28 is operated to connect the first decompression unit 20 and the upper chamber 4. Then, the internal space 16 of the first recessed portion 8 of the upper chamber 4 is exhausted through the exhaust portion 24 by the first decompression unit 20, and the internal space 16 is decompressed. Then, the second electromagnetic valve 30 is operated to connect the second decompression unit 22 and the lower chamber 6. Then, the internal space 18 of the second recessed portion 10 of the lower chamber 6 is exhausted through the exhaust portion 26 by the second decompression unit 22, and the internal space 18 is decompressed.
[0095] Next, as the fourth stage of the wafer unit forming step S10, the pressure of the first recess 8 is increased to bring the sheet 27 into contact with the front surface 11a of the wafer 11. For example, the sheet 27 is pressed into contact with the wafer 11 by utilizing the pressure difference between the upper and lower portions of the sheet 27. Figure 4 1 is a cross-sectional view schematically showing the thermocompression bonding device 2 in the fourth stage of the wafer unit forming step S10 .
[0096] In the fourth stage of the wafer unit forming step S10, first, the first decompression unit 20 stops decompressing the upper chamber 4. That is, the first electromagnetic valve 28 is operated to release the connection between the first decompression unit 20 and the upper chamber 4. At this time, the second electromagnetic valve 30 is not operated, and the connection between the second decompression unit 22 and the lower chamber 6 is maintained. In this case, the pressure of the internal space 16 of the upper chamber 4 gradually rises.
[0097] The thermocompression bonding device 2 may connect the upper chamber 4 to the outside air via the exhaust portion 24. In this case, when the upper chamber 4 is connected to the outside air, air rapidly flows into the internal space 16, and the pressure of the internal space 16 of the upper chamber 4 rapidly rises.
[0098] When the pressure of the internal space 16 of the upper chamber 4 is higher than the pressure of the internal space 18 of the lower chamber 6, the sheet 27 separating the internal space 16 and the internal space 18 receives a downward force.
[0099] In the fourth stage of the wafer unit forming step S10, the sheet 27 is pushed downward to contact the front surface 11a of the wafer 11. Alternatively, at the start time of the fourth stage of the wafer unit forming step S10, the sheet 27 is already in contact with the front surface 11a of the wafer 11, and the sheet 27 is pushed toward the wafer 11 in the fourth stage.
[0100] When the fourth stage of the wafer unit forming step S10 is completed, a force sufficient to fix the sheet 27 to the wafer 11 is not applied between the sheet 27 and the wafer 11. Therefore, in order to fix the sheet 27 to the wafer 11, the sheet 27 is heated and thermally pressed onto the front surface 11a of the wafer 11.
[0101] Next, as the fifth stage of the wafer unit forming step S10, the heating means of the thermocompression bonding apparatus 2 is operated to heat the sheet 27. For example, when the thermocompression bonding apparatus 2 has a heater 36 as the heating means, the heater 36 is operated to heat the sheet 27 together with the wafer 11.
[0102] When the sheet 27 is heated to a temperature near the melting point while the sheet 27 is pressed toward the wafer 11 by the pressure difference between the internal space 16 of the first recess 8 and the internal space 18 of the second recess 10, the sheet 27 is thermocompressed onto the wafer 11. After the sheet 27 is thermocompressed, the heating unit (heater 36) is stopped to stop heating the sheet 27.
[0103] In addition, when performing thermal compression bonding, it is preferred to heat the sheet 27 to a temperature below the melting point. This is because when the heating temperature exceeds the melting point, the sheet 27 may melt and the shape of the sheet may not be maintained. In addition, it is preferred to heat the sheet 27 to a temperature above the softening point. This is because when the heating temperature does not reach the softening point, thermal compression bonding cannot be properly performed. That is, it is preferred to heat the sheet 27 to a temperature above the softening point and below the melting point.
[0104] In addition, a part of the sheet 27 may not have a clear softening point. Therefore, when performing thermocompression bonding, it is preferable to heat the sheet 27 to a temperature that is 20° C. lower than the melting point and is equal to or lower than the melting point.
[0105] For example, when the polyolefin sheet used as the sheet 27 is a polyethylene sheet, the heating temperature is preferably 120° C. to 140° C. Also, when the polyolefin sheet is a polypropylene sheet, the heating temperature is preferably 160° C. to 180° C. Also, when the polyolefin sheet is a polystyrene sheet, the heating temperature is preferably 220° C. to 240° C.
[0106] For example, when the polyester sheet used as the sheet 27 is a polyethylene terephthalate sheet, the heating temperature is 250° C. to 270° C. Also, when the polyester sheet is a polyethylene naphthalate sheet, the heating temperature is 160° C. to 180° C. However, the heating temperature of the sheet 27 is not limited thereto.
[0107] The heating unit is stopped to stop heating the sheet 27, the second electromagnetic valve 30 is operated to disconnect the second decompression unit 22 and the lower chamber 6, the pressure of the internal space 18 of the lower chamber 6 is restored to atmospheric pressure, and then the upper chamber 4 is raised. Figure 5 As shown, a wafer unit 31 is obtained in which the sheet 27, the wafer 11 and the ring frame 29 are integrated. Thus, the wafer unit forming step S10 is completed.
[0108] In the wafer processing method of the present embodiment, after the wafer unit forming step S10 , the holding step S20 is performed in which the wafer 11 is held by the holding table 40 of the cutting device 38 via the sheet 27 . Figure 6 (A) is a perspective view schematically showing the wafer unit 31 in the holding step S20, Figure 6 (B) is a cross-sectional view schematically showing the wafer unit 31 in the holding step S20.
[0109] In the holding step S20, the wafer unit 31 is unloaded from the thermal compression bonding device 2 and placed on the holding table 40 of the cutting device 38. At this time, the position of the wafer 11 is adjusted so that the front surface 11a side of the wafer 11 faces the holding surface 46 and the center of the holding surface 46 coincides with the center of the front surface 11a of the wafer 11.
[0110] Then, the suction source (not shown) of the holding table 40 is operated, and the wafer 11 is sucked and held by the holding table 40 via the sheet 27. In addition, the annular frame 29 of the wafer unit 31 is gripped by the clamp 48 disposed on the outer peripheral side of the holding table 40. As a result, the back side 11b of the wafer 11 is exposed upward.
[0111] In the wafer processing method of the present embodiment, after the holding step S20 , the breaking step S30 is performed in which a breaking groove is formed in the circular recessed portion 15 of the wafer 11 to separate the annular protruding portion 13 from the wafer 11 . Figure 7 (A) is a perspective view schematically showing the cutting device 38 in the breaking step S30, Figure 7 (B) is a cross-sectional view schematically showing the cutting device 38 in the breaking step S30. Figure 8 (A) and Figure 8 (B) schematically shows the breaking groove 33 formed in the wafer 11.
[0112] The position where the break groove 33 is formed on the wafer 11 is set to a circular area centered on the center of the circular recess 15. In particular, the cutting edge 58 does not cut into the Figure 1 The position of the breaking groove 33 is adjusted by the step difference portion 17 between the annular convex portion 13 and the circular concave portion 15 shown in (A). In the breaking step S30, first, the cutting unit 50 is moved so that the cutting edge 58 of the cutting tool 56 is positioned above the area where the breaking groove 33 is to be formed.
[0113] Next, the rotation drive source provided inside the spindle housing 52 is operated to start the rotation of the cutting tool 56, and the cutting unit 50 is lowered to make the cutting blade 58 cut into the wafer 11. Then, the cutting unit 50 is lowered until the lower end of the cutting blade 58 reaches the height position of the sheet 27, and the holding table 40 starts to rotate. Then, when the holding table 40 rotates more than one circle, the circular breaking groove 33 is formed on the wafer 11, and the annular convex portion 13 is separated from the wafer 11. In other words, the annular convex portion 13 is separated from the circular concave portion 15.
[0114] When the wafer 11 is cut by the cutting unit 50, cutting chips and frictional heat are generated from the wafer 11 and the cutting edge 58 of the cutting tool 56. Therefore, when the cutting tool 56 cuts into the wafer 11, cutting water composed of pure water or the like is supplied to the cutting tool 56 and the wafer 11. Then, the cutting chips and frictional heat generated by the cutting of the wafer 11 are taken into the cutting water and removed.
[0115] Here, when a dicing tape having a paste layer is used instead of the sheet 27 in a different wafer processing method from the present embodiment, when the cutting water that has taken in the cutting chips reaches the dicing tape, the cutting chips may adhere to the paste layer. In this case, the cutting chips may be separated from the dicing tape in a subsequent process, and the cutting chips may reach the wafer 11 and adhere to it. When the cutting chips adhere to the wafer 11, the quality of the device chip formed from the wafer 11 is reduced, which becomes a problem.
[0116] In contrast, in the wafer processing method of the present embodiment, the sheet 27 does not have a paste layer. Therefore, even if the cutting water that has taken in the cuttings reaches the sheet 27, the cuttings are unlikely to adhere to the sheet 27. In addition, even if the cuttings adhere to the sheet 27, the cuttings can be easily removed from the sheet 27. Therefore, the cuttings are unlikely to transfer from the sheet 27 to the wafer 11, and the quality of the device chip is unlikely to be degraded due to the cuttings.
[0117] In the wafer processing method of the present embodiment, after the breaking step S30 , the removing step S40 of removing the annular convex portion 13 cut from the wafer 11 from the sheet 27 is performed. Figure 8 (A) is a perspective view schematically showing the wafer unit 31 in the removal step S40, Figure 8 (B) is a cross-sectional view schematically showing the wafer unit 31 and the removal unit 60 in the removal step S40.
[0118] Figure 8 (B) of FIG. 4 includes a cross-sectional view schematically showing the annular protrusion 13 when it is removed from the sheet 27 by the removal step S40. After the annular protrusion 13 is separated from the wafer 11, the annular protrusion 13 is lifted and peeled off from the sheet 27. As a result, the portion of the wafer 11 that was previously the circular recess 15 remains on the sheet 27. That is, a wafer unit 31 is obtained in which the wafer 11, the sheet 27, and the annular frame 29 are integrated with the annular protrusion 13 removed. Then, when the wafer 11 is divided, individual device chips are obtained.
[0119] The removal step S40 is performed, for example, by the function of the removal unit 60. The removal unit 60 is, for example, assembled in the cutting device 38. However, the removal unit 60 may not be assembled in the cutting device 38, and the removal step S40 may be performed outside the cutting device 38. Hereinafter, the removal step S40 will be described by taking the case where the removal unit 60 is assembled in the cutting device 38 and the removal step S40 is performed on the holding table 40 by the removal unit 60 as an example.
[0120] For example, Figure 8 (A) and Figure 8 As shown in (B), after the disconnection step S30, the removal step S40 is performed on the holding table 40. In the removal step S40, first, the bottom plate 64 of the removal unit 60 is arranged above the wafer 11. Then, the bottom plate 64 is lowered in a state where the removal claws 78 protrude outward so that the removal claws 78 are located at a position further outward than the wafer 11.
[0121] The arm 62 is lowered until the lower claw 78b of the removal claw 78 is located at the boundary between the sheet 27 and the annular protrusion 13, and then the lowering is stopped. Next, the removal claw 78 is moved toward the inner side of the bottom plate 64. At this time, the lower claw 78b is moved, for example, 1.6 mm inward from the outer peripheral edge of the wafer 11. In the removal step S40, the removal claw 78 is inserted into the boundary between the sheet 27 and the annular protrusion 13 in a state where the plurality of removal claws 78 are arranged approximately equally and spaced apart from each other along the circumferential direction of the wafer 11.
[0122] Next, while the bottom plate 64 is rotated with the arm 62 as the rotation axis so that the plurality of removal claws 78 rotate along the outer periphery of the wafer 11, the arm 62 and the bottom plate 64 are raised so that the plurality of removal claws 78 move upward. In addition, the rotation speed of the removal claws 78 is set to 10° / s, for example, and it takes 14 seconds for each removal claw 78 to rotate 140°. In addition, the rising speed of the removal claws 78 is, for example, 0.14 mm / s. The annular convex portion 13 is separated from the sheet 27, and the annular convex portion 13 is removed from the sheet 27 (wafer unit 31).
[0123] In this embodiment, since the actions of rotating the plurality of removal claws 78 around the wafer 11 and moving the plurality of removal claws 78 upward are performed simultaneously, the time required to remove the annular protrusion 13 from the sheet 27 can be shortened compared to when each action is performed separately.
[0124] Furthermore, since the annular projection 13 is moved in a predetermined direction away from the sheet 27 as the removal claw 78 rotates, there is an advantage that the annular projection 13 does not adhere to the sheet 27 again.
[0125] In addition, the removal claw 78 has an upper claw 78a in addition to the lower claw 78b. The annular convex portion 13 peeled off from the sheet 27 may rise violently sometimes, but by providing the upper claw 78a, the rise of the annular convex portion 13 can be stopped within the range of the upper claw 78a and the lower claw 78b. Thus, the annular convex portion 13 can be prevented from falling.
[0126] When the annular protrusion 13 is removed from the sheet 27, an excessive load may be applied to the annular protrusion 13, and the annular protrusion 13 may be cracked or damaged. In addition, the generated chips and fragments may fall between the wafer 11 of the wafer unit 31 and the annular frame 29 toward the sheet 27.
[0127] However, since the sheet 27 does not have a paste layer, scraps and fragments do not adhere to the sheet 27. For example, when the wafer unit 31 is cleaned by a cleaning device, such scraps and fragments are extremely easily removed and do not remain on the sheet 27.
[0128] In addition, unlike the case where the adhesive tape is strongly adhered by the paste layer, the annular convex portion 13 is inherently easy to remove when it is fixed to the sheet 27 without the paste layer. Therefore, a large force is not applied to the removed annular convex portion 13, and it is not easy to be damaged or fragmented. Therefore, the fragments will not be scattered and attached to the device chips formed by dividing the wafer 11, and the quality of the device chips can be prevented from being degraded.
[0129] Furthermore, it is not necessary to irradiate the sheet 27 with ultraviolet rays in order to remove the annular convex portion from the sheet 27, nor is it necessary to narrow the region for device formation on the front surface 11a of the wafer 11 on the premise of irradiating ultraviolet rays. Therefore, the productivity of device chips is also improved.
[0130] In addition, in the above embodiment, the case where the cutting groove 33 is formed on the wafer 11 using the cutting device 38 equipped with the cutting tool 56 in the breaking step S30 is described, but one embodiment of the present invention is not limited to this. That is, in the breaking step S30, a laser processing device (not shown) that can irradiate a laser beam to the wafer 11 and perform laser processing on the wafer 11 may also be used.
[0131] For example, a laser beam containing a wavelength component absorbed by the wafer 11 is irradiated to the area in the wafer 11 where the disconnect groove 33 is to be formed, and the wafer 11 is ablated. Alternatively, a laser beam containing a wavelength component that transmits the wafer 11 is focused on the area in the wafer 11 where the disconnect groove 33 is to be formed, and a modified layer is formed along the area in the wafer 11, and the wafer 11 is divided using the modified layer as the division starting point.
[0132] In these cases as well, according to the wafer processing method of one embodiment of the present invention, the annular convex portion 13 of the wafer 11 that has been cut off from the wafer 11 can be easily removed from the sheet 27. At this time, a large load is not applied to the annular convex portion 13, and even if the annular convex portion 13 is damaged and fragments fall onto the sheet 27, the fragments can be easily removed from the sheet 27. Therefore, the fragments will not adhere to the device chip later, and a high-quality device chip can be formed.
[0133] Furthermore, the structures, methods, and the like according to the above-described embodiments and modifications may be implemented with appropriate changes without departing from the scope of the purpose of the present invention. The above-described embodiments and modifications may also be combined as appropriate.
Claims
1. A method for processing a wafer, wherein the wafer has an annular convex portion on the outer periphery of the back side, and a circular concave portion is formed in an area of the back side surrounded by the annular convex portion, wherein: The wafer processing method comprises the following steps: a wafer unit forming step of fixing a sheet having no paste layer on the front surface of the wafer and fixing a ring-shaped frame on the outer peripheral portion of the sheet to form a wafer unit; A holding step of holding the wafer via the sheet using a holding table after the wafer unit forming step; a breaking step of forming a breaking groove in the circular concave portion of the wafer to separate the annular protrusion from the wafer after the holding step; as well as A removing step, after the breaking step, removing the annular protrusion from the sheet.
2. The wafer processing method according to claim 1, characterized in that: In the wafer unit forming step, the sheet is heated and pressed to be thermocompressed onto the wafer, thereby fixing the sheet onto the wafer.