Composite antistatic film and preparation method thereof

By adopting a composite antistatic film structure in the PET film, the combination of toughened modified PET resin and antistatic PET resin, combined with graphitized carbon nanotubes and bioxazoline chain extenders, the PET film forming process is solved. The problems of interruption and poor antistatic properties have achieved high-efficiency molding and excellent antistatic properties.

CN119017811AActive Publication Date: 2024-11-26SHENZHEN MINDA TECH CO LTD

Patent Information

Application Number
CN202411137489.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing PET films are prone to breaking and have poor antistatic properties during the molding process, resulting in low molding efficiency and easy dust adhesion on the surface.

Method used

A composite antistatic film structure is adopted, including a core layer and an outer layer. The core layer is made of toughened modified PET resin, and the outer layer is made of antistatic PET resin, using end-hydroxygraphitized carbon nanotubes and bisoxazole respectively. The linear chain extenders improve compatibility and antistatic properties, and increase melt viscosity by isocyanate-capped polyurethane prepolymer, small molecule diol chain extenders and double-ended hydroxypropyl silicone oil to prevent foaming and delamination.

Benefits of technology

The toughness and antistatic properties of the composite antistatic film are improved, the molding efficiency and dust resistance are enhanced, the cost is reduced, and the problems of fracture and later foaming and layering of the composite film are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017811A_ABST
    Figure CN119017811A_ABST
Patent Text Reader

Abstract

The invention discloses a composite antistatic film and a preparation method thereof, and relates to the field of automobile part film materials. The composite antistatic film comprises a core layer and an outer layer, the core layer is made of toughened modified PET resin, and the outer layer is made of antistatic PET resin; the toughened modified PET resin is prepared from 100 parts by weight of first PET resin, 24.3 to 30.8 parts by weight of hydroxyl-terminated polyurethane resin, 1.0 to 1.5 parts by weight of first hydroxyl graphitized carbon nanotubes and 8.8 to 10.4 parts by weight of a first bisoxazoline chain extender; the antistatic PET resin is prepared from 100 parts by weight of second PET resin, 0.85 to 1.0 part by weight of second hydroxyl graphitized carbon nanotubes and 3.5 to 4.8 parts by weight of a second bisoxazoline chain extender. The composite antistatic film has both toughness and antistatic property, the forming efficiency of the composite antistatic film can be improved, rapid export of static electricity can be promoted, and the dustproof property of the composite antistatic film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of automotive parts film materials, and in particular to a composite antistatic film and a preparation method thereof. Background Art

[0002] PET (polyethylene terephthalate) film is usually obtained by stretching after melt extrusion of PET resin, toughening agent and release agent. PET film has excellent physical and mechanical properties in a wide temperature range, and has good resistance to organic solvents, weather resistance and scratch resistance, and can protect auto parts from being scratched. However, the existing PET film mainly has the following two shortcomings: the first is that the film-forming property of PET resin is poor, and in the process of producing PET film, PET film is prone to fracture, and the molding efficiency is low. Although the addition of toughening agent can improve the film-forming property of PET resin, the existing toughening agent is usually acrylonitrile-butadiene-styrene copolymer or styrene-butadiene thermoplastic elastomer, and acrylonitrile-butadiene-styrene copolymer or styrene-butadiene thermoplastic elastomer has poor compatibility with PET resin, and the improvement effect is limited. The second is that the antistatic property of PET film is poor, and dust is easily attached to the surface. Summary of the invention

[0003] In order to improve the problem of easy breakage and poor antistatic property of PET film during the molding process in the related art, the present application provides a composite antistatic film and a preparation method thereof.

[0004] In the first aspect, the present application provides a composite antistatic film using the following technical solution: A composite antistatic film comprises a core layer and an outer layer composited on the upper and lower surfaces of the core layer, wherein the core layer is made of a toughened modified PET resin, and the outer layer is made of an antistatic PET resin; wherein, based on the raw materials, the toughened modified PET resin comprises 100 parts by weight of a first PET resin, 24.3-30.8 parts by weight of a hydroxyl-terminated polyurethane resin, 1.0-1.5 parts by weight of a first hydroxyl graphitized carbon nanotube, and 8.8-10.4 parts by weight of a first bis-oxazoline chain extender; The antistatic PET resin comprises 100 parts by weight of a second PET resin, 0.85-1.0 parts by weight of a second hydroxy graphitized carbon nanotube and 3.5-4.8 parts by weight of a second bis-oxazoline chain extender.

[0005] The composite antistatic film in the present application comprises at least a core layer and an outer layer composited on the upper and lower surfaces of the core layer. The difference between the core layer and the outer layer is that the raw material ratio is different and terminal hydroxyl polyurethane resin is added to the core layer.

[0006] The core layer is made of toughened modified PET resin, in which the terminal hydroxyl polyurethane resin is used to improve toughness, the first hydroxyl graphitized carbon nanotube is used to improve antistatic property, and the first bis-oxazoline chain extender can react with the hydroxyl groups on the first PET resin, the terminal hydroxyl polyurethane resin and the first hydroxyl graphitized carbon nanotube to improve the compatibility among the first PET resin, the terminal hydroxyl polyurethane resin and the first hydroxyl graphitized carbon nanotube, which is beneficial to obtain a core layer with good toughness and good antistatic property, and can improve the molding efficiency of the composite antistatic film.

[0007] The outer layer is made of antistatic PET resin. In the antistatic PET resin, the second hydroxy graphitized carbon nanotubes are used to improve the antistatic property. The second bis-oxazoline chain extender can react with the hydroxyl groups on the second PET resin and the second hydroxy graphitized carbon nanotubes to improve the compatibility between the second PET resin and the second hydroxy graphitized carbon nanotubes, which is conducive to obtaining an outer layer with good antistatic performance.

[0008] The outer layer may or may not contain a hydroxyl-terminated polyurethane resin, and not containing a hydroxyl-terminated polyurethane resin is beneficial to reducing costs, and the composite antistatic film has better stiffness. In addition, in the present application, the core layer and the outer layer can form a complete static conductive network, promote the rapid conduction of static electricity, and improve the dustproofness of the composite antistatic film.

[0009] Optionally, the first PET resin and the second PET resin are made of American DuPont PT2251 or Korean SKBR8040.

[0010] Optionally, based on the raw materials, the hydroxyl-terminated polyurethane resin includes 58-64 parts by weight of isocyanate-terminated polyurethane prepolymer, 5.5-6.0 parts by weight of small molecule diol chain extender and 8.5-10.8 parts by weight of double-terminated hydroxypropyl silicone oil; the isocyanate-terminated polyurethane prepolymer is prepared from 30-40 parts by weight of polyester diol, 12.8-16.4 parts by weight of diisocyanate and 0.01-0.015 parts by weight of catalyst.

[0011] In the present application, the terminal hydroxyl polyurethane resin is prepared by using isocyanate-terminated polyurethane prepolymer, small molecule diol chain extender and double-terminated hydroxypropyl silicone oil, wherein the isocyanate-terminated polyurethane prepolymer is chain extended by the small molecule diol chain extender and the double-terminated hydroxypropyl silicone oil, which is beneficial to improve the problem of foaming and stratification of the composite antistatic film in the later stage caused by the increase of melt viscosity of the toughened modified PET resin, the inability to discharge bubbles in the melt in time, or the existence of local extrusion unevenness during the melt extrusion process.

[0012] Optionally, the small molecule diol chain extender is at least one of propylene glycol, 1,4-butanediol, and neopentyl glycol.

[0013] Optionally, the molecular weight of the polyester diol is 1000-2000.

[0014] In the present application, the molecular weight of the polyester diol is controlled within the range of 1000-2000, which is beneficial to further improve the toughness of the hydroxyl-terminated polyurethane resin.

[0015] Optionally, the diisocyanate is at least one of isophorone diisocyanate, hexamethylene diisocyanate, toluene diisocyanate and diphenylmethane diisocyanate.

[0016] Optionally, the catalyst is at least one of dibutyltin dilaurate and stannous octoate.

[0017] Optionally, the method for preparing the hydroxyl-terminated polyurethane resin comprises the following steps: The polyester diol is heated to 45-55°C, and then diisocyanate and a catalyst are added, and the temperature is raised to 70-75°C under nitrogen protection for reaction for 3-4 hours to obtain an isocyanate-terminated polyurethane prepolymer; Add a small molecule diol chain extender and a double-terminated hydroxypropyl silicone oil to the isocyanate-terminated polyurethane prepolymer, continue the reaction at 80-85° C. for 3-4 hours, then evacuate, cool, and granulate to obtain a hydroxyl-terminated polyurethane resin.

[0018] In the present application, the above method is used to prepare the hydroxy-terminated polyurethane resin, which has the characteristics of simple steps and good product stability.

[0019] Optionally, the diameter of the first hydroxyl-graphitized carbon nanotube and the second hydroxyl-graphitized carbon nanotube is 10-30 nm, and the length is 10-30 μm.

[0020] In the present application, the diameter of the first hydroxy graphitized carbon nanotube and the second hydroxy graphitized carbon nanotube are controlled to be 10-30 nm and the length is 10-30 μm, which is conducive to the uniform dispersion of the first hydroxy graphitized carbon nanotube and the second hydroxy graphitized carbon nanotube.

[0021] Optionally, the first bisoxazoline chain extender and the second bisoxazoline chain extender are at least one of bisoxazoline and 2,2'-(1,3-phenylene)-bisoxazoline.

[0022] Optionally, the thickness ratio of the core layer to the outer layer is 1:(1-1.5).

[0023] In the second aspect, the present application provides a method for preparing a composite antistatic film using the following technical solution: A method for preparing a composite antistatic film comprises the following steps: The first PET resin, the hydroxyl-terminated polyurethane resin, the first hydroxyl-graphitized carbon nanotube and the first bis-oxazoline chain extender are mixed, melt-extruded and pelletized at 245-260° C. to obtain a toughened modified PET resin; The second PET resin, the second hydroxy graphitized carbon nanotubes and the second bis-oxazoline chain extender are mixed, melt-extruded at 245-260° C., and pelletized to obtain an antistatic PET resin; The toughened modified PET resin is put into extruder A, and the temperature of extruder A is set to 265-280° C.; The antistatic PET resin is fed into the extruder B, and the temperature of the extruder B is set to 265-280° C.; The die distributor is connected to extruders A and B, wherein the melt of extruder B is evenly distributed to the upper and lower flow channels through the die distributor, and the melt of extruder A is distributed to the middle flow channel through the die distributor, and the fluids in the three flow channels are co-extruded and cast from the die lip to obtain a cast sheet; The cast sheet is stretched to obtain a composite antistatic film.

[0024] In the present application, the composite antistatic film prepared by the above method can obtain a composite antistatic film with good toughness and good antistatic properties.

[0025] In summary, this application at least includes the following beneficial effects: (1) The composite antistatic film in the present application at least includes a core layer and an outer layer composited on the upper and lower surfaces of the core layer. The core layer is made of a toughened modified PET resin, in which a terminal hydroxyl polyurethane resin is used to improve toughness, a first hydroxyl graphitized carbon nanotube is used to improve antistatic properties, a first bis-oxazoline chain extender can react with the first PET resin, the terminal hydroxyl polyurethane resin, and the hydroxyl groups on the first hydroxyl graphitized carbon nanotube, improve the compatibility between the first PET resin, the terminal hydroxyl polyurethane resin, and the first hydroxyl graphitized carbon nanotube, and is conducive to obtaining a core layer with good toughness and good antistatic properties, and can improve the molding efficiency of the composite antistatic film. The outer layer is made of an antistatic PET resin, in which a second hydroxyl graphitized carbon nanotube is used to improve antistatic properties, a second bis-oxazoline chain extender can react with the second PET resin and the hydroxyl groups on the second hydroxyl graphitized carbon nanotube, improve the compatibility between the second PET resin and the second hydroxyl graphitized carbon nanotube, and is conducive to obtaining an outer layer with good antistatic properties. The outer layer may or may not contain hydroxyl-terminated polyurethane resin. Not containing hydroxyl-terminated polyurethane resin is beneficial to reducing costs and making the composite antistatic film more stiff. It promotes the rapid discharge of static electricity and improves the dustproofness of the composite antistatic film. (2) In the present application, the hydroxyl-terminated polyurethane resin is prepared by using isocyanate-terminated polyurethane prepolymer, small molecule diol chain extender and double-terminated hydroxypropyl silicone oil, wherein the isocyanate-terminated polyurethane prepolymer is chain extended by the small molecule diol chain extender and the double-terminated hydroxypropyl silicone oil, which is beneficial to improve the problem of foaming and stratification of the composite antistatic film in the later stage caused by the increase of melt viscosity of the toughened modified PET resin, the inability to discharge the bubbles in the melt in time, or the existence of local extrusion unevenness during the melt extrusion process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the structure of a composite antistatic film according to an embodiment of the present application.

[0027] Description of reference numerals: 1. Core layer; 2. Outer layer. DETAILED DESCRIPTION

[0028] The present application is further described below in conjunction with specific experiments.

[0029] Preparation Example [Preparation Example 1] A hydroxyl-terminated polyurethane resin comprises, in terms of raw materials, 58 kg of isocyanate-terminated polyurethane prepolymer, 5.5 kg of propylene glycol and 10.8 kg of double-terminated hydroxypropyl silicone oil HX-10 (Huaxiang Kejie), wherein the isocyanate-terminated polyurethane prepolymer is prepared from 30 kg of polycaprolactone diol with a molecular weight of 2000, 12.8 kg of isophorone diisocyanate and 0.01 kg of dibutyltin dilaurate.

[0030] In this preparation example, the preparation method of the hydroxyl-terminated polyurethane resin comprises the following steps: The polycaprolactone diol was heated to 45°C, and then isophorone diisocyanate and dibutyltin dilaurate were added, and the temperature was raised to 70°C under nitrogen protection for 4 hours to obtain an isocyanate-terminated polyurethane prepolymer; Propylene glycol and double-terminated hydroxypropyl silicone oil were added to the isocyanate-terminated polyurethane prepolymer according to the ratio, and the reaction was continued at 80° C. for 4 hours, and then vacuumed, cooled, and granulated to obtain a hydroxyl-terminated polyurethane resin.

[0031] [Preparation Example 2] A terminal hydroxyl polyurethane resin, calculated on the basis of raw materials, comprises 64kg of isocyanate-terminated polyurethane prepolymer, 6.0kg of 1,4-butanediol and 8.5kg of double-terminated hydroxypropyl silicone oil HX-20 (Huaxiang Kejie), wherein the isocyanate-terminated polyurethane prepolymer is prepared from 40kg of polycaprolactone diol with a molecular weight of 2000, 16.4kg of diphenylmethane diisocyanate and 0.015kg of dibutyltin dilaurate.

[0032] In this preparation example, the preparation method of the hydroxyl-terminated polyurethane resin comprises the following steps: The polycaprolactone diol was heated to 55°C, and then diphenylmethane diisocyanate and dibutyltin dilaurate were added, and the temperature was raised to 75°C under nitrogen protection for reaction for 3 hours to obtain an isocyanate-terminated polyurethane prepolymer; 1,4-Butanediol and double-terminated hydroxypropyl silicone oil were added to the isocyanate-terminated polyurethane prepolymer according to the ratio, and the reaction was continued at 85°C for 3 hours, and then vacuumed, cooled, and granulated to obtain a hydroxyl-terminated polyurethane resin.

[0033] [Preparation Example 3] A hydroxy-terminated polyurethane resin, which differs from [Preparation Example 1] in that the double-terminated hydroxypropyl silicone oil is replaced by an equal amount of propylene glycol.

[0034] [Preparation Example 4] A hydroxy-terminated polyurethane resin, which differs from [Preparation Example 1] in that propylene glycol is replaced by an equal amount of double-terminated hydroxypropyl silicone oil. Example

[0035] [Example 1] A composite antistatic film, referring to Figure 1 , including a core layer 1 and an outer layer 2 compounded on the upper and lower surfaces of the core layer 1, the thickness ratio of the core layer 1 to the outer layer 2 is 1:1.5, the thickness of the core layer 1 is 5μm, and the core layer 1 is made of toughened modified PET resin, and the outer layer 2 is made of antistatic PET resin. Among them, in terms of raw materials, the toughened modified PET resin includes 100kg of the first PET resin, 24.3kg of the terminal hydroxyl polyurethane resin prepared in [Preparation Example 1], 1.0kg of the first hydroxyl graphitized carbon nanotubes and 8.8kg of the first bis-oxazoline chain extender, and the antistatic PET resin includes 100kg of the second PET resin, 1.0kg of the second hydroxyl graphitized carbon nanotubes and 4.8kg of the second bis-oxazoline chain extender.

[0036] In this embodiment, the first PET resin and the second PET resin are both made of DuPont PT2251 from the United States; the first hydroxyl graphitized carbon nanotube and the second hydroxyl graphitized carbon nanotube are both made of hydroxyl graphitized carbon nanotube CNT224 produced by China Science and Technology Research Institute, and the diameter of the hydroxyl graphitized carbon nanotube CNT224 is 10-20nm and the length is 10-30μm; the first bis-oxazoline chain extender and the second bis-oxazoline chain extender are both made of disoxizoline.

[0037] In this embodiment, the preparation method of the composite antistatic film comprises the following steps: The first PET resin, the hydroxyl-terminated polyurethane resin, the first hydroxyl-graphitized carbon nanotube and the first bis-oxazoline chain extender are mixed, melt-extruded and pelletized at 245° C. to obtain a toughened modified PET resin; The second PET resin, the second hydroxy graphitized carbon nanotubes and the second bis-oxazoline chain extender are mixed, melt-extruded at 245° C., and pelletized to obtain an antistatic PET resin; The toughened modified PET resin was fed into extruder A, and the temperature of extruder A was set to 265°C; The antistatic PET resin was fed into the extruder B, and the temperature of the extruder B was set to 265°C; The die distributor is connected to extruders A and B, wherein the melt of extruder B is evenly distributed to the upper and lower flow channels through the die distributor, and the melt of extruder A is distributed to the middle flow channel through the die distributor, and the fluids in the three flow channels are co-extruded and cast from the die lip to obtain a cast sheet; The cast sheet was stretched, and the transverse stretching ratio and the longitudinal stretching ratio were both 3 times to obtain a composite antistatic film.

[0038] [Example 2] A composite antistatic film, referring to Figure 1 , including a core layer 1 and an outer layer 2 compounded on the upper and lower surfaces of the core layer 1, the thickness ratio of the core layer 1 to the outer layer 2 is 1:1.5, the thickness of the core layer 1 is 5μm, and the core layer 1 is made of toughened modified PET resin, and the outer layer 2 is made of antistatic PET resin. Among them, in terms of raw materials, the toughened modified PET resin includes 100kg of the first PET resin, 30.8kg of the terminal hydroxyl polyurethane resin prepared in [Preparation Example 2], 1.5kg of the first hydroxyl graphitized carbon nanotubes and 10.4kg of the first bis-oxazoline chain extender, and the antistatic PET resin includes 100kg of the second PET resin, 0.85kg of the second hydroxyl graphitized carbon nanotubes and 3.5kg of the second bis-oxazoline chain extender.

[0039] In this embodiment, the first PET resin and the second PET resin are both made of Korean SK BR8040; the first hydroxyl graphitized carbon nanotube and the second hydroxyl graphitized carbon nanotube are both made of hydroxyl graphitized carbon nanotube CNT225 produced by China Science and Technology Research Institute, and the diameter of the hydroxyl graphitized carbon nanotube CNT225 is 20-30nm and the length is 10-30μm; the first bis-oxazoline chain extender and the second bis-oxazoline chain extender are both made of 2,2'-(1,3-phenylene)-bis-oxazoline.

[0040] In this embodiment, the preparation method of the composite antistatic film comprises the following steps: The first PET resin, the hydroxyl-terminated polyurethane resin, the first hydroxyl-graphitized carbon nanotube and the first bis-oxazoline chain extender are mixed, melt-extruded and pelletized at 260° C. to obtain a toughened modified PET resin; The second PET resin, the second hydroxy graphitized carbon nanotubes and the second bis-oxazoline chain extender are mixed, melt-extruded at 260° C., and pelletized to obtain an antistatic PET resin; The toughened modified PET resin was fed into extruder A, and the temperature of extruder A was set at 280°C; The antistatic PET resin was fed into the extruder B, and the temperature of the extruder B was set to 280°C; The die distributor is connected to extruders A and B, wherein the melt of extruder B is evenly distributed to the upper and lower flow channels through the die distributor, and the melt of extruder A is distributed to the middle flow channel through the die distributor, and the fluids in the three flow channels are co-extruded and cast from the die lip to obtain a cast sheet; The cast sheet was stretched, and the transverse stretching ratio and the longitudinal stretching ratio were both 3 times to obtain a composite antistatic film.

[0041] [Example 3] A composite antistatic film, which differs from [Example 1] in that: the terminal hydroxyl polyurethane resin is replaced by an equal amount of the terminal hydroxyl polyurethane resin prepared in [Preparation Example 3].

[0042] [Example 4] A composite antistatic film, which differs from [Example 1] in that: the terminal hydroxyl polyurethane resin is replaced by an equal amount of the terminal hydroxyl polyurethane resin prepared in [Preparation Example 4].

[0043] Comparative Example [Comparative Example 1] A composite antistatic film, which differs from [Example 1] in that: In the toughened and modified PET resin, the terminal hydroxyl polyurethane resin is replaced by an equal amount of the first PET resin.

[0044] [Comparative Example 2] A composite antistatic film, which differs from [Example 1] in that: In the toughened and modified PET resin, the hydroxyl-terminated polyurethane resin is replaced by an equal amount of styrene-butadiene thermoplastic elastomer T171.

[0045] [Comparative Example 3] A composite antistatic film, which differs from [Example 1] in that: In the toughened modified PET resin, the first bis-oxazoline chain extender is replaced by an equal amount of diphenylmethane diisocyanate, and in the antistatic PET resin, the second bis-oxazoline chain extender is replaced by an equal amount of diphenylmethane diisocyanate.

[0046] [Comparative Example 4] A composite antistatic film, which differs from [Example 1] in that: In the toughened modified PET resin, the first bis-oxazoline chain extender is replaced by an equal amount of the first PET resin, and in the antistatic PET resin, the second bis-oxazoline chain extender is replaced by an equal amount of the second PET resin.

[0047] Performance testing 1. Elongation at break: Referring to GB / T 13022-1991 "Test method for tensile properties of plastic films", the composite antistatic films prepared in the embodiments and comparative examples of the present application were made into standard test pieces, and the elongation at break of the composite antistatic films in the embodiments and comparative examples was tested according to the standard. The test speed was 100 mm / min, and the elongation at break of the composite antistatic films in the embodiments and comparative examples was recorded.

[0048] 2. Stability: Take 10 rolls of the composite antistatic film in each embodiment and comparative example (all without interlayer blistering problem), store them under the same environmental conditions for 180 days, observe whether there is blistering between the layers of the composite antistatic film, and record the number of rolls of the composite antistatic film with interlayer blistering.

[0049] 3. Surface resistance: The surface resistance of the composite antistatic film prepared in each embodiment and comparative example of the present application was measured with reference to GB / T 33398-2016 "Measurement method for surface resistance of optically functional film polyethylene terephthalate (PET) film".

[0050] Table 1 Sample Elongation at break / % Number of foam rolls / roll Surface resistance / Ω Example 1 58.6 0 <![CDATA[2.5*10 6 ]]> Example 2 54.9 0 <![CDATA[2.9*10 6 ]]> Example 3 56.8 4 <![CDATA[2.7*10 6 ]]> Example 4 49.5 2 <![CDATA[2.8*10 6 ]]> Comparative Example 1 22.8 0 <![CDATA[2.7*10 6 ]]> Comparative Example 2 28.9 0 <![CDATA[2.6*10 6 ]]> Comparative Example 3 39.9 0 <![CDATA[2.9*10 6 ]]> Comparative Example 4 32.1 0 <![CDATA[4.3*10 7 ]]> The difference between Comparative Example 1 and Example 1 is that the hydroxyl-terminated polyurethane resin in Comparative Example 1 is replaced by an equal amount of the first PET resin. Combining the data in Table 1, it can be seen that after the hydroxyl-terminated polyurethane resin is replaced by the first PET resin, the elongation at break of the composite antistatic film is significantly reduced, which is not conducive to improving the molding efficiency of the composite antistatic film.

[0051] The difference between Comparative Example 2 and Example 1 is that the hydroxyl-terminated polyurethane resin in Comparative Example 2 is replaced by an equal amount of styrene-butadiene thermoplastic elastomer. Combining the data in Table 1, it can be seen that after the hydroxyl-terminated polyurethane resin is replaced by styrene-butadiene thermoplastic elastomer, the elongation at break of the composite antistatic film is also significantly reduced, which is not conducive to improving the molding efficiency of the composite antistatic film.

[0052] The difference between Comparative Example 3 and Example 1 is that the first bis-oxazoline chain extender and the second bis-oxazoline chain extender in Comparative Example 3 are replaced by diphenylmethane diisocyanate in equal amounts. Combining the data in Table 1, it can be seen that after the bis-oxazoline chain extender is replaced by diphenylmethane diisocyanate, the elongation at break of the composite antistatic film decreases, but is better than the composite antistatic film in Comparative Example 2.

[0053] The difference between Comparative Example 4 and Example 1 is that no bisoxazoline chain extender is added to the toughened modified PET resin and the antistatic PET resin in Comparative Example 4. Combined with the data in Table 1, it can be seen that when no bisoxazoline chain extender is added, the elongation at break of the composite antistatic film decreases, and the surface resistance of the composite antistatic film tends to increase, and the antistatic performance is weakened.

[0054] The difference between Example 3 and Example 1 is that no double-terminal hydroxypropyl silicone oil is added when synthesizing the terminal hydroxyl polyurethane resin in Example 3. Combined with the data in Table 1, it can be seen that when the double-terminal hydroxypropyl silicone oil is not added when synthesizing the terminal hydroxyl polyurethane resin, some composite antistatic films are prone to local blistering between layers after long-term storage. The reason is that the melt viscosity of the toughened modified PET resin increases, the bubbles in the melt cannot be discharged in time, or there is a problem of local uneven extrusion during the melt extrusion process, which leads to the problem of blistering and stratification in the composite antistatic film in the later stage.

[0055] The difference between Example 4 and Example 1 is that propylene glycol is not added when synthesizing the hydroxyl-terminated polyurethane resin in Example 4. Combined with the data in Table 1, it can be seen that when propylene glycol is not added when synthesizing the hydroxyl-terminated polyurethane resin, the toughness of the composite antistatic film is reduced, and some composite antistatic films will also have blistering and stratification problems in the later stage.

[0056] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A composite antistatic film, characterized in that: The invention comprises a core layer (1) and an outer layer (2) composited to the upper and lower surfaces of the core layer (1), wherein the core layer (1) is made of a toughened modified PET resin, and the outer layer (2) is made of an antistatic PET resin; wherein, based on the raw materials, the toughened modified PET resin comprises 100 parts by weight of a first PET resin, 24.3-30.8 parts by weight of a hydroxyl-terminated polyurethane resin, 1.0-1.5 parts by weight of a first hydroxyl graphitized carbon nanotube, and 8.8-10.4 parts by weight of a first bis-oxazoline chain extender; The antistatic PET resin comprises 100 parts by weight of a second PET resin, 0.85-1.0 parts by weight of a second hydroxy graphitized carbon nanotube and 3.5-4.8 parts by weight of a second bis-oxazoline chain extender.

2. A composite antistatic film according to claim 1, characterized in that: The first PET resin and the second PET resin are American DuPont PT2251 or Korean SK BR8040.

3. A composite antistatic film according to claim 1, characterized in that: In terms of raw materials, the hydroxyl-terminated polyurethane resin includes 58-64 parts by weight of isocyanate-terminated polyurethane prepolymer, 5.5-6.0 parts by weight of small molecule diol chain extender and 8.5-10.8 parts by weight of double-terminated hydroxypropyl silicone oil; the isocyanate-terminated polyurethane prepolymer is prepared from 30-40 parts by weight of polyester diol, 12.8-16.4 parts by weight of diisocyanate and 0.01-0.015 parts by weight of catalyst.

4. A composite antistatic film according to claim 3, characterized in that: The small molecule diol chain extender is at least one of propylene glycol, 1,4-butanediol and neopentyl glycol.

5. The composite antistatic film according to claim 3, characterized in that: The molecular weight of the polyester diol is 1000-2000.

6. A composite antistatic film according to any one of claims 3 to 5, characterized in that: The preparation method of the hydroxyl-terminated polyurethane resin comprises the following steps: The polyester diol is heated to 45-55°C, and then diisocyanate and a catalyst are added, and the temperature is raised to 70-75°C under nitrogen protection for reaction for 3-4 hours to obtain an isocyanate-terminated polyurethane prepolymer; Add a small molecule diol chain extender and a double-terminated hydroxypropyl silicone oil to the isocyanate-terminated polyurethane prepolymer, continue the reaction at 80-85° C. for 3-4 hours, then evacuate, cool, and granulate to obtain a hydroxyl-terminated polyurethane resin.

7. The composite antistatic film according to claim 1, characterized in that: The diameter of the first hydroxy graphitized carbon nanotube and the second hydroxy graphitized carbon nanotube is 10-30 nm, and the length is 10-30 μm.

8. The composite antistatic film according to claim 1, characterized in that: The first bisoxazoline chain extender and the second bisoxazoline chain extender are at least one of bisoxazoline and 2,2'-(1,3-phenylene)-bisoxazoline.

9. The composite antistatic film according to claim 1, characterized in that: The thickness ratio of the core layer (1) to the outer layer (2) is 1:(1-1.5).

10. The method for preparing a composite antistatic film according to any one of claims 1 to 9, characterized in that: The following steps are involved: The first PET resin, the hydroxyl-terminated polyurethane resin, the first hydroxyl-graphitized carbon nanotube and the first bis-oxazoline chain extender are mixed, melt-extruded and pelletized at 245-260° C. to obtain a toughened modified PET resin; The second PET resin, the second hydroxy graphitized carbon nanotubes and the second bis-oxazoline chain extender are mixed, melt-extruded at 245-260° C., and pelletized to obtain an antistatic PET resin; The toughened modified PET resin is put into extruder A, and the temperature of extruder A is set to 265-280° C.; The antistatic PET resin is fed into the extruder B, and the temperature of the extruder B is set to 265-280° C.; The die distributor is connected to extruders A and B, wherein the melt of extruder B is evenly distributed to the upper and lower flow channels through the die distributor, and the melt of extruder A is distributed to the middle flow channel through the die distributor, and the fluids in the three flow channels are co-extruded and cast from the die lip to obtain a cast sheet; The cast sheet is stretched to obtain a composite antistatic film.

Citation Information

Patent Citations

  • Antistatic PET film

    CN106183304A

  • High-performance antistatic polyester material and preparation method thereof

    CN111004478A

  • Optical protective film

    JP2007105928A

Cited By

  • Antistatic film and preparation method thereof

    CN119286031A

  • Antistatic film and preparation method thereof

    CN119286031B