Method for improving wear resistance of printed color film and application

By combining the BOPP film with surface modification coating, combined with water-based color ink printing, the whitening problem caused by friction in tobacco packaging is solved, and the wear resistance of the printed color film is improved and maintained. Its light transmission and gloss extend the service life.

CN119017857APending Publication Date: 2024-11-26CHINA TOBACCO YUNNAN IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110873.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The whitening phenomenon (frost) caused by friction in tobacco packaging affects its beauty and durability, and the wear resistance of the printed color film is insufficient, affecting the long-term storage and use of the product.

Method used

The composite BOPP film is used for pretreatment and surface modification coating, including low-temperature plasma surface activation and corona treatment, combined with water-based color ink printing, and a three-layer structure printed color film is formed to improve wear resistance.

Benefits of technology

It significantly improves the wear resistance of the printed color film, maintains light transmission and gloss, avoids the phenomenon of frosting, enhances the bonding ability of the surface modification coating agent to the film, and extends the service life of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992159650000061
    Figure BDA0004992159650000061
  • Figure BDA0004992159650000071
    Figure BDA0004992159650000071
  • Figure BDA0004992159650000081
    Figure BDA0004992159650000081
Patent Text Reader

Abstract

The invention discloses a method for improving wear resistance of a printed color film, the printed color film is a composite BOPP film, and the method comprises the following steps: (1) pretreating the outer surface and the inner surface of the composite BOPP film; (2) coating the outer surface and the inner surface of the composite BOPP film with a surface modification coating agent, and drying at high temperature; and (3) printing the outer surface of the composite BOPP film by using water-based color ink, and drying to obtain the printed color film. The invention also discloses application of the high-printing color film obtained by the method in a tobacco packaging film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tobacco, and particularly relates to a method for improving the wear resistance of a printed color film and a use thereof. Background Art

[0002] The cigarette packaging film is generally BOPP film. BOPP film undergoes biaxial stretching during the production process, so BOPP film has high tensile strength and high impact strength. It has excellent rigidity, toughness and transparency, outstanding tensile strength and impact strength, high stiffness and high transparency. BOPP film is colorless, odorless, tasteless and non-toxic, and is a commonly used packaging material in the tobacco industry.

[0003] Due to the characteristics of BOPP film, such as light weight, non-toxicity, high mechanical strength, good dimensional stability and good transparency, it is widely used in the packaging of candy, cigarettes, textiles, food, etc. However, some characteristics of BOPP film limit its application: (1) Biaxially oriented polypropylene film is a non-polar polymer with mainly methyl groups exposed on the surface, so its surface free energy is extremely low, resulting in poor adhesion and printing and dyeing properties; (2) The tertiary carbon atoms and methyl groups in the biaxially oriented polypropylene film molecules carry active H elements, which are prone to oxidative degradation reactions under the action of external oxygen and other conditions, which is not conducive to its long-term storage and use; (3) BOPP film is rubbed by packaging (or boxing), transportation, and distribution, resulting in whitening, which affects its appearance and performance.

[0004] At present, high-end cigarette products generally use printed color films for decorative packaging. Compared with traditional non-printed cigarette films, printed color films require large-area printing of multiple colors, and the printing process of printed color films is complicated. If the organic solvent used in printing causes erosion of the macromolecular chain of the printed color film (the cigarette film is generally BOPP); therefore, water-based ink is generally used, and the drying process of printing is about 40°C, which causes a certain degree of loss in the physical indicators of the printed color film, especially the loss of performance indicators such as wear resistance.

[0005] Cigarette packaging films may turn white due to friction caused by packing (or box), transportation, and distribution. The distribution position is not fixed, which is generally called "abrasion" in the industry. This phenomenon is particularly obvious on dark box skins. Especially when loaded into boxes for storage, the probability of "abrasion" is higher because the outer packaging needs to withstand friction between itself and the inner wall of the box during the packing process. The specific phenomenon is: when it is just packaged, it can achieve a beautiful effect of body-fitting brightness, but before sales, due to the friction between items, the surface of the items is scratched and the haze increases, which seriously affects the appearance of the items. Abrasion items destroy their original decoration effect and beauty, and make consumers feel bad. Therefore, it is of great significance to improve the wear resistance of BOPP film.

[0006] The present invention has been proposed to solve the above-mentioned problems. Summary of the invention

[0007] In order to improve the wear resistance of BOPP printed color film without losing its light transmittance (no change in haze) and glossiness, the present invention proposes a method for improving the wear resistance of printed color film. The obtained printed color film has improved wear resistance for tobacco packaging film without losing its light transmittance and glossiness.

[0008] The technical solution of the present invention is as follows:

[0009] The first aspect of the present invention discloses a method for improving the wear resistance of a printed color film, wherein the printed color film is a composite BOPP film, and the method comprises the following steps:

[0010] (1) Pre-treating the outer surface and inner surface of the composite BOPP film;

[0011] (2) coating the outer surface and inner surface of the composite BOPP film with a surface modification coating agent and drying at high temperature;

[0012] (3) Printing the outer surface of the composite BOPP film with water-based color ink, and obtaining the printed color film after drying.

[0013] Preferably, the composite BOPP film is three-layered, the surface layer is a blended film of copolymer PP and silicon dioxide, the core layer is a blended film of homopolymer PP, antistatic agent and hydrogenated petroleum resin, and the inner layer is a blended film of copolymer PP and phenyl-modified silicone.

[0014] Preferably, the silicon dioxide content in the surface layer is not higher than 0.15wt%; the antistatic agent in the core layer is a mixture of alkyl diethanolamine and monoglyceride, the antistatic agent content is 0.35%-0.45wt%, and the content of hydrogenated petroleum resin is 10-15wt%; the content of phenyl modified silicone in the inner layer is 0.10-0.20wt%.

[0015] Preferably, in step (1), the outer surface of the composite BOPP film is pretreated by low-temperature plasma surface activation treatment, and the gas used is CO2; the inner surface of the composite BOPP film is treated by corona treatment, and the voltage of the corona treatment is 2 to 100 kV and the frequency is 2 to 10 kHz.

[0016] Preferably, the surface modification coating composition of step (2) includes: water-based silane coupling agent, soluble aluminum salt, tetraethyl orthosilicate, solid acid and water, and the mass ratio thereof is (1-10): (10-30): (50-200): (5-10): (200-400).

[0017] Preferably, the silane coupling agent is one of methyltrichlorosilane (MTS) or aminosilane; and the solid acid is ethylenediaminetetraacetic acid.

[0018] Preferably, the preparation of the surface modification coating comprises the following steps: adding a water-based silane coupling agent, a soluble aluminum salt and a solid acid into water to dissolve them, then adding tetraethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed.

[0019] Preferably, the surface modification coating in step (2) is applied by spraying; the drying temperature is 80-100°C.

[0020] Preferably, the drying temperature after printing in step (3) is 40-60°C.

[0021] The second aspect of the present invention discloses the use of the high-printing color film obtained by the method as a tobacco packaging film.

[0022] Beneficial effects of the present invention:

[0023] 1. The method of the present invention improves the wear resistance of the printed color film, and the haze, glossiness and transparency are not affected or slightly improved. It is used for tobacco packaging film and has good machine suitability. Note: Haze refers to the ratio of the scattered light flux that deviates from the direction of the incident light through the sample to the transmitted light flux, expressed as a percentage. Wearability refers to the ability of the surface of the film to withstand damage under the action of external friction; it is generally expressed by the change in haze value, that is, the difference between the haze value of the film after a certain pressure, speed and number of frictions minus the original haze value before friction; the smaller the difference, the better the wear resistance, and vice versa.

[0024] 2. The method for improving the wear resistance of printed color film of the present invention adopts a composite BOPP film; the surface layer is a copolymerized PP and a silicon dioxide film, and the wear resistance is better than that of an ordinary BOPP film. The core layer is a blended film of homopolymerized PP, an antistatic agent and a hydrogenated petroleum resin. The refractive index of the hydrogenated petroleum resin is about 1.51, which is very close to the refractive index of BOPP (about 1.49). Both are non-polar materials with similar structures and good compatibility. The hydrogenated petroleum resin is an amorphous oligomer, and PP is a semi-crystalline polymer. The addition of the hydrogenated petroleum resin expands the amorphous region of the mixed material, significantly changes the aggregated structure of the PP polymer chain, partially dissolves the crystal structure of the PP, reduces the melting point of the PP (from 161-162°C to 140-150°C), and refines the crystal particles of the PP, thereby improving the transparency of the PP, and keeping the haze unchanged or reduced (light transmittance unchanged or improved). The inner layer is a blended film of copolymerized PP and phenyl-modified silicone, in which the kinematic viscosity of phenyl-modified silicone is 100-280mm 2 / s, which has a refractive index closer to that of PP, which improves the glossiness of the BOPP film surface and makes it more transparent.

[0025] 3. In order to improve the bonding performance between the surface modification coating and the surface of the composite BOPP film, the method of the present invention performs low-temperature plasma surface activation treatment on the outer surface of the composite BOPP film, and the gas used is CO2; the inner surface of the composite BOPP film is subjected to corona treatment, and the voltage of the corona treatment is 2-100kV and the frequency is 2-10kHz. Since the surface layer of the composite BOPP film of the present invention is a blended film of copolymerized PP and silica, after the CO2 low-temperature plasma surface activation treatment, the surface modification coating has a greater ability to bind to it, and after printing with water-based color ink, the color film has higher wear resistance. The inner layer is a blended film of copolymerized PP and phenyl-modified silicone. After the corona treatment with a voltage of 2-100kV and a frequency of 2-10kHz, the surface modification coating has a better ability to bind to it, and the coating formed later has a high peeling strength and will not have a "grinding" phenomenon; at the same time, because many active points will be formed on the surface after the corona treatment, these active points are tightly combined with the surface modification coating, and there is almost no gap on the entire BOPP surface, so the gas barrier property is improved. Through the analysis of the CO2 low-temperature plasma surface activation treatment of the composite BOPP film, polar groups such as -COOH and -OH were successfully introduced into the outer surface of the composite BOPP film, which significantly improved the surface free energy and the interface bonding ability between the outer surface of the composite BOPP film and the surface modification coating. The outer surface components of the composite BOPP film after the surface modification coating are mainly Al, Si and O elements, among which Al and Si elements are mainly Al 3+ and SiO2, so the wear resistance of the outer surface of the composite BOPP film is significantly improved.

[0026] 4. The surface modification coating of the present invention first dissolves the water-based silane coupling agent, soluble aluminum salt and solid acid in water, and then adds tetraethyl orthosilicate dropwise under high-speed stirring (the speed is generally 1000-5000rpm) to prepare a surface modification coating with good transparency and wear resistance for the first time. According to analysis, the particles in the surface modification coating are about 30nm and the particle size is uniform. Infrared spectroscopy analysis shows that Si-O-Al covalent bonds are formed in the prepared surface modification coating; transmittance analysis shows that Al 3+ It can effectively inhibit the cross-linking and aggregation of silica sol after hydrolysis of ethyl orthosilicate to produce whitening phenomenon, thereby not reducing the haze of BOPP film and maintaining excellent optical properties.

[0027] 5. The outer surface of the composite BOPP film of the present invention is treated with CO2 low-temperature plasma surface activation and then coated with a surface modification coating, and then the outer surface of the composite BOPP film is printed with water-based color ink, and the wear quality is small. This is because the polar groups such as -COOH and -OH generated on the outer surface after CO2 low-temperature plasma surface activation have good hydrophilicity, so that the outer surface has good bonding performance with the surface modification coating, and the coating is uniform; the printed color film obtained by printing the outer surface of the composite BOPP film with water-based color ink is firmly bonded to the surface modification coating. When the mass ratio of ethyl orthosilicate to soluble aluminum salt (AlCl3) is 10:1.5, the wear resistance effect is the best. DETAILED DESCRIPTION

[0028] The following is described in conjunction with the embodiments, and it should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. Other advantages, objectives and features of the present invention will be described in the subsequent embodiments, and to some extent are obvious to those skilled in the art, or those skilled in the art can be taught from the practice of the present invention.

[0029] In order to improve the wear resistance of BOPP printed color film without losing its light transmittance (no change in haze) and glossiness, the present invention proposes a method for improving the wear resistance of printed color film, and obtains a high-printed color film for tobacco packaging film with improved wear resistance without losing its light transmittance and glossiness.

[0030] The method for improving the wear resistance of a printed color film of the present invention is a composite BOPP film, and the method comprises the following steps: (1) pre-treating the outer surface and the inner surface of the composite BOPP film; the composite BOPP film is a three-layer film, the surface layer is a film of a copolymerized PP and a silicon dioxide blend, the silicon dioxide content is not higher than 0.15wt%; the core layer is a film of a homopolymerized PP, an antistatic agent and a hydrogenated petroleum resin blend, the antistatic agent is a mixture of alkyl diethanolamine and monoglyceride, the antistatic agent content is 0.35%-0.45wt%, and the hydrogenated petroleum resin content is 10-15wt%; the inner layer is a film of a copolymerized PP and a phenyl-modified silicone blend, the phenyl-modified silicone content is 0.10-0.20wt%; the outer surface of the composite BOPP film is pre-treated by a low-temperature plasma surface activation treatment, the gas used is CO2; the inner surface of the composite BOPP film is treated by a corona treatment, the voltage of the corona treatment is 2-100kV, and the frequency is 40-60Hz; The rate is 2 to 10 kHz; (2) coating the outer surface and the inner surface of the composite BOPP film with a surface modification coating agent, the coating is carried out by spraying, and the coating is dried at 80-100° C. The surface modification coating agent comprises: a water-based silane coupling agent, a soluble aluminum salt, tetraethyl orthosilicate, a solid acid and water, and the mass ratio thereof is (1-10): (10-30): (50-200): (5-10): (200-400); the silane coupling agent is methyltrichlorosilane ( MTS) or one of aminosilane; the solid acid is ethylenediaminetetraacetic acid; the preparation of the surface modification coating comprises the following steps: adding a water-based silane coupling agent, a soluble aluminum salt and a solid acid into water to dissolve, then adding tetraethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed; (3) using a water-based color ink to print the outer surface of the composite BOPP film, and obtaining the printed color film after drying; the drying temperature after printing is 40-60°C.

[0031] Embodiment 1: Method for improving the wear resistance of printed color film (shrink film).

[0032] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP and 0.10wt% silica; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP and 0.15wt% phenyl modified silicone;

[0033] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), soluble aluminum salt (aluminum chloride), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 5:15:100:10:200. Add 5g of aminosilane, 15g of aluminum chloride and 10g of ethylenediaminetetraacetic acid into 200g (ml) of water, mix and dissolve, add 100g of tetraethyl orthosilicate drop by drop at 3000rmp, and stir for 10min after the addition is completed; a white, transparent and slightly viscous surface modified coating is obtained;

[0034] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;

[0035] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;

[0036] The obtained printed color film was tested for abrasion resistance, light transmittance and glossiness, and the results are shown in Table 1 below:

[0037] The wear resistance shall be tested in accordance with the requirements of YC / T 315 Determination of wear resistance of cigarette packaging film.

[0038] The haze test shall be carried out in accordance with the provisions of GB / T2410 Transparent Plastics Transmittance and Haze Test Method.

[0039] The glossiness is tested in accordance with the provisions of GB / T8807 Plastic Mirror Gloss Test Method, with an incident angle of 45°. During the test, the plane formed by the incident and reflected light of the glossiness tester test window should be parallel to the longitudinal direction of the smoke film, the backing plate should be black and the glossiness should not exceed 0.2%.

[0040] Table 1 Test results of printed color film obtained in Example 1

[0041]

[0042] Machine suitability: The cigarette film samples undergoing machine suitability test should be stored for 24 hours under environmental conditions of temperature 22.0-27.0℃ and relative humidity 60%±5% before being tested on the machine. During the process, the normal operation of the packaging machine will not be affected by cigarette film quality defects, the effective operation rate of the equipment will be improved, and there will be no defects such as loose packs and wrinkles that affect the quality of cigarette strips, boxes and packaging.

[0043] Embodiment 2: Method for improving the wear resistance of printed color film (shrink film).

[0044] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP and 0.10wt% silica; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP and 0.15wt% phenyl modified silicone;

[0045] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), soluble aluminum salt (aluminum chloride), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 5:20:100:10:200. Add 5g of aminosilane, 20g of aluminum chloride and 10g of ethylenediaminetetraacetic acid into 200g (ml) of water, mix and dissolve, add 100g of tetraethyl orthosilicate drop by drop at 3000rmp, and stir for 10min after the addition is completed; a white, transparent and slightly viscous surface modified coating is obtained;

[0046] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;

[0047] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;

[0048] Similar to Example 1, the obtained printed color film was tested for abrasion resistance, light transmittance and glossiness. The results are shown in Table 2 below:

[0049] Table 2 Test results of printed color film obtained in Example 2

[0050]

[0051] The suitability for the machine is the same as that in Example 1.

[0052] Embodiment 3: Method for improving the wear resistance of printed color film (micro-shrinkage film).

[0053] The composite BOPP film has three layers: the surface layer is a blended film of copolymer PP and 0.08wt% silica; the core layer is a blended film of homopolymer PP, 0.40wt% antistatic agent (the mass ratio of alkyl diethanolamine and monoglyceride is 1:0.3) and 10wt% hydrogenated petroleum resin; the inner layer is a blended film of copolymer PP and 0.12wt% phenyl modified silicone;

[0054] The composition and preparation method of the modified coating: water-based silane coupling agent (aminosilane), soluble aluminum salt (aluminum chloride), tetraethyl orthosilicate, solid acid (ethylenediaminetetraacetic acid) and water, the mass ratio of which is 5:10:100:10:200. Add 5g of aminosilane, 10g of aluminum chloride and 10g of ethylenediaminetetraacetic acid into 200g (ml) of water and mix and dissolve, add 100g of tetraethyl orthosilicate drop by drop at 3000rmp, and stir for 10min after the addition is completed; a white, transparent and slightly viscous surface modified coating is obtained;

[0055] The outer surface of the composite BOPP film is pretreated by using CO2 low-temperature plasma surface activation treatment; then the surface modification coating is sprayed on the outer surface of the composite BOPP film, and after drying at 90° C., the outer surface of the composite BOPP film is printed with water-based color ink (commonly used in the market), and after drying at 50° C., the printed color film is obtained;

[0056] At the same time, the inner surface of the composite BOPP film was treated with 50 kV and 10 kHz corona treatment, and then the surface modification coating was sprayed on the outer surface of the composite BOPP film and dried at 90°C;

[0057] Similar to Example 1, the obtained printed color film was tested for abrasion resistance, light transmittance and glossiness. The results are shown in Table 3 below:

[0058] Table 3 Test results of printed color film obtained in Example 3

[0059]

[0060] The suitability for the machine is the same as that of Example 1.

[0061] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for improving the wear resistance of a printed color film, characterized in that: The printed color film is a composite BOPP film, and the method comprises the following steps: (1) Pre-treating the outer and inner surfaces of the composite BOPP film; (2) coating the outer surface and inner surface of the composite BOPP film with a surface modification coating agent and drying at high temperature; (3) Printing the outer surface of the composite BOPP film with water-based color ink, and obtaining the printed color film after drying.

2. The method according to claim 1, characterized in that The composite BOPP film is a three-layer film, the surface layer is a blended film of copolymer PP and silicon dioxide, the core layer is a blended film of homopolymer PP, antistatic agent and hydrogenated petroleum resin, and the inner layer is a blended film of copolymer PP and phenyl modified silicone.

3. The method according to claim 2, characterized in that The silicon dioxide content in the surface layer is not higher than 0.15wt%; the antistatic agent in the core layer is a mixture of alkyl diethanolamine and monoglyceride, the antistatic agent content is 0.35%-0.45wt%, and the content of hydrogenated petroleum resin is 10-15wt%; the content of phenyl modified silicone in the inner layer is 0.10-0.20wt%.

4. The method according to claim 1, characterized in that: In step (1), the outer surface of the composite BOPP film is pretreated by low-temperature plasma surface activation treatment, and the gas used is CO2; the inner surface of the composite BOPP film is treated by corona treatment, and the voltage of the corona treatment is 2 to 100 kV and the frequency is 2 to 10 kHz.

5. The method according to claim 1, characterized in that The surface modification coating composition of step (2) includes: water-based silane coupling agent, soluble aluminum salt, tetraethyl orthosilicate, solid acid and water, and the mass ratio thereof is (1-10): (10-30): (50-200): (5-10): (200-400).

6. The method according to claim 5, characterized in that The water-based silane coupling agent is one of methyltrichlorosilane (MTS) and aminosilane; and the solid acid is ethylenediaminetetraacetic acid.

7. The method according to claim 5, characterized in that The preparation of the surface modification coating comprises the following steps: adding a water-based silane coupling agent, a soluble aluminum salt and a solid acid into water to dissolve them, then adding ethyl orthosilicate dropwise under high-speed stirring, and obtaining the surface modification coating after the reaction is completed.

8. The method according to claim 1, characterized in that The surface modification coating in step (2) is applied by spraying; the drying temperature is 80-100°C.

9. The method according to claim 1, characterized in that: The drying temperature after printing in step (3) is 40-60°C.

10. Use of the high-printing color film obtained according to any one of the methods of claims 1 to 9 as tobacco packaging film.