Preparation method and application of modified molecular sieve
By adding metal precursors to the molecular sieve and subjecting hydrothermal synthesis, subsequent alkali treatment and silanization treatment, a modified molecular sieve catalyst was prepared, which solved the low yield problem caused by the self-polymerization of molecular sieve in furfuryl alcohol etherification reaction, and achieved Highly efficient production of alkoxyfuryl ether, supporting the large-scale application of alkoxyfuran ether.
Patent Information
- Application Number
- CN202310603572.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The existing molecular sieves have low yields of alkoxyfuryl ether due to the autopolymerization reaction in catalytic furoxyl ether, which increases production cost and separation difficulty, and limits the large-scale application of alkoxyfuryl ether.
A metal precursor was added to the tetraethyl orthosilicate molecular sieve by hydrothermal method to perform in-situ synthesis of metal-doped MFI molecular sieve, and a modified molecular sieve catalyst was prepared by alkali treatment and silanization treatment to improve its catalytic performance.
The yield of alkoxyfuryl ether was significantly improved, especially when the catalytic synthesis of furfuryl alcohol ether was achieved, achieving a yield of 85%, overcoming the difficulty of yield below 60% in the prior art. , supports the large-scale application of alkoxyfuran ether.
Smart Images

Figure CN119018907A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a preparation method and application of a modified molecular sieve, and belongs to the field of chemistry and chemical engineering. Background Art
[0002] Alkoxy furan ethers are considered to be a new type of bio-based fuel additive due to their advantages such as high energy density, high octane number and good fuel miscibility. At present, alkoxy furan ethers are mainly prepared by acid-catalyzed etherification of furan alcohol and alkyl alcohol. Common furan alcohols include: 5-hydroxymethylfurfural, 2,5-furan dimethanol and furfuryl alcohol. Among them, furfuryl alcohol is an important bio-based chemical, which can be obtained by selective hydrogenation of bio-based platform chemical furfural. Compared with 5-hydroxymethylfurfural and its derivative 2,5-furan dimethanol, furfuryl alcohol has the advantages of low price and large production capacity. Molecular sieves, as a solid acid catalyst, are widely used in the fields of fine chemicals and petrochemicals. In recent years, molecular sieves have shown excellent catalytic performance in catalyzing the reaction of 5-hydroxymethylfurfural, 2,5-furan dimethanol with methanol, ethanol, butanol, etc., and obtained an alkoxy furan ether yield of more than 90%. However, due to the active performance of furfuryl alcohol, it is very easy to undergo self-polymerization during the reaction, resulting in the yield of alkoxy furfuryl ether on molecular sieves generally being less than 60%. This not only greatly increases the difficulty of subsequent separation, but also significantly increases the production cost. Therefore, the development of a molecular sieve catalyst that can efficiently catalyze the etherification of furfuryl alcohol to prepare alkoxyfurfuryl ethers is of great significance for the large-scale application of alkoxyfurfuryl ethers. Summary of the invention
[0003] According to one aspect of the present application, a method for preparing a modified molecular sieve is provided, wherein a metal precursor is added to a synthesis stock solution of tetraethyl orthosilicate molecular sieve, a metal-doped MFI molecular sieve is synthesized in situ by a hydrothermal method, and then the metal-doped MFI molecular sieve is sequentially subjected to an alkali treatment and a silanization treatment to prepare a modified molecular sieve catalyst.
[0004] This application adopts the following technical solutions:
[0005] A method for preparing a modified molecular sieve comprises the following steps:
[0006] S1, subjecting a mixed solution containing tetraethyl orthosilicate, a metal precursor, tetrapropylammonium hydroxide and water to a hydrothermal reaction and calcining I to obtain a metal-doped MFI molecular sieve;
[0007] S2, treating the metal-doped MFI molecular sieve with alkali, exchanging with ammonium, and calcining II to obtain the modified molecular sieve.
[0008] Optionally, the step S1 includes:
[0009] S11, adding a metal precursor and tetrapropylammonium hydroxide to an aqueous solution of tetraethyl orthosilicate in sequence to obtain a mixed solution;
[0010] S12, placing the mixed solution in step S11 into a closed reactor, performing a hydrothermal reaction, and calcining I to obtain a metal-doped MFI molecular sieve.
[0011] Optionally, the step S2 further comprises a silanization treatment after calcination II.
[0012] Optionally, the mixed solution preparation process in step S11 includes continuing stirring until complete dissolution.
[0013] Optionally, the weight ratio of tetraethyl orthosilicate, tetrapropylammonium hydroxide and water is 1:(1.2-2.3):(1.5-3).
[0014] Optionally, the weight ratio of tetraethyl orthosilicate, tetrapropylammonium hydroxide and water is 1:(1.65-1.75):(1.7-1.8).
[0015] Optionally, the metal precursor is selected from at least one of tin tetrachloride, zirconium tetrachloride and titanium tetrachloride.
[0016] Optionally, the molar ratio of the metal element to the silicon element in the metal precursor and tetraethyl orthosilicate is 0.01 to 0.03:1.
[0017] Optionally, the molar ratio of the metal element to the silicon element in the metal precursor and tetraethyl orthosilicate is selected from any value of 0.01:1, 0.015:1, 0.02:1, 0.025:1, 0.03:1, or any range between the two.
[0018] Optionally, the conditions of the hydrothermal reaction are: reaction temperature of 170-190° C., and reaction time of 60-84 h.
[0019] Optionally, the hydrothermal reaction is to crystallize the mixed solution at the above temperature, and after the crystallization is completed, wait for cooling to room temperature, take out the product in the hydrothermal kettle, filter, wash, dry in sequence, and then calcine I.
[0020] Optionally, the drying condition is drying at 890-120° C. for 10-14 hours.
[0021] Optionally, the calcination conditions of I are: calcination at 500-600° C. for 4-6 hours.
[0022] Optionally, in step S2, the alkali treatment comprises: immersing the metal-doped MFI molecular sieve in an aqueous alkali solution, and heating at 75 to 85° C. for 0.5 to 1.5 h to obtain the alkali-treated molecular sieve.
[0023] Optionally, the alkaline treatment further comprises continuous stirring.
[0024] Optionally, the alkali treatment further comprises hot filtering, washing and drying the heated reaction solution.
[0025] Optionally, the weight ratio of the metal-doped MFI molecular sieve to the alkali is 2 to 3:1.
[0026] Optionally, the weight ratio of the metal-doped MFI molecular sieve to the alkali is selected from any value of 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3:1, or any range therebetween.
[0027] Optionally, the concentration of the aqueous solution of the base is 0.015 to 0.025 g / mL.
[0028] Optionally, the base is selected from at least one of sodium hydroxide and potassium hydroxide.
[0029] Optionally, in step S2, the ammonium exchange treatment and calcination II comprises: immersing the alkali-treated molecular sieve in an aqueous solution of ammonium, heating at 75 to 85° C. for 0.5 to 1.5 h, and calcining to obtain a hydrogen-type alkali-treated modified molecular sieve.
[0030] Optionally, the weight ratio of the alkali-treated molecular sieve to ammonium is 1:0.5-0.6.
[0031] Optionally, the concentration of the aqueous solution of ammonium is 0.01 to 0.015 g / mL.
[0032] Optionally, the concentration of the aqueous solution of ammonium is selected from any value of 0.01 g / mL, 0.011 g / mL, 0.012 g / mL, 0.013 g / mL, 0.014 g / mL, 0.015 g / mL, or any range therebetween.
[0033] Optionally, the ammonium is at least one of ammonium chloride, ammonium nitrate and ammonium sulfate.
[0034] Optionally, the calcination conditions of II are: calcination at 500-600° C. for 6-8 hours.
[0035] Optionally, the ammonium exchange treatment further comprises hot filtering, washing and drying the heated reaction solution, wherein the washing solvent is anhydrous ethanol and the drying temperature is 100-120°C.
[0036] Optionally, the silanization treatment comprises: immersing the modified molecular sieve obtained in step S2 into a silane modifier solution, and refluxing at 20 to 40° C. for 8 to 12 hours;
[0037] Optionally, the weight ratio of the hydrogen-type alkali-treated modified molecular sieve to the silane modifier is 1:0.1 to 0.15.
[0038] Optionally, the weight ratio of the hydrogen-type alkali-treated modified molecular sieve to the silane modifier is any value among 1:0.1, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15, or any range value therebetween.
[0039] Optionally, the solvent of the silane modifier is an organic solvent;
[0040] Optionally, the solvent of the silane modifier is selected from at least one of toluene, p-xylene, m-xylene and o-xylene;
[0041] Optionally, the silane modifier is selected from at least one of octadecyltrichlorosilane and dimethyloctadecylchlorosilane.
[0042] Optionally, the concentration of the silane modifier is 0.003-0.009 g / mL.
[0043] According to another aspect of the present application, a modified molecular sieve prepared according to the aforementioned preparation method is provided, wherein the particle size of the modified molecular sieve is 200 to 500 nm.
[0044] According to another aspect of the present application, there is also provided a modified molecular sieve prepared by the aforementioned preparation method, and the use of at least one of the aforementioned modified molecular sieves as a catalyst in catalyzing the etherification of furfuryl alcohol to synthesize alkoxyfurfuryl ether.
[0045] Optionally, the following steps are included:
[0046] The modified molecular sieve is contacted with a mixed solution of furfuryl alcohol and alkyl alcohol, and heated for reaction to obtain alkoxy furfuryl ether.
[0047] Optionally, the weight ratio of the modified molecular sieve, furfuryl alcohol, and alkyl alcohol is 1:(1-3):(15-40);
[0048] Optionally, the conditions for the heating reaction are: reaction temperature is 100-120° C., and reaction time is 1-6 h;
[0049] Optionally, the alkyl alcohol is selected from n-butanol, and the alkoxy furfuryl ether is selected from n-butyl furfuryl ether.
[0050] The beneficial effects of this application include:
[0051] The modified molecular sieve prepared by the preparation method of the modified molecular sieve provided in the present application can be used as a molecular sieve catalyst for catalyzing the etherification of furfuryl alcohol to prepare alkoxyfurfuryl ethers, can achieve high-selectivity etherification of furfuryl alcohol, greatly improve the yield of alkoxyfurfuryl ethers, and the catalyst can be applied multiple times. In particular, when the modified molecular sieve is used in catalyzing the etherification of furfuryl alcohol to synthesize n-butylfurfuryl ether, an 85% yield of n-butylfurfuryl ether can be obtained, which overcomes the difficulty that the yield of alkoxyfurfuryl ether catalyzed by furfuryl alcohol in the prior art is generally lower than 60%, and is of great significance for the large-scale application of alkoxyfurfuryl ethers. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 XRD diagrams of samples 1# to 4# metal-doped MFI molecular sieves in Examples 1 to 4 of the present application;
[0053] Figure 2 This is the TEM image of sample 1#Sn-doped MFI molecular sieve in Example 1 of the present application. DETAILED DESCRIPTION
[0054] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0055] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0056] Example 1
[0057] Weigh 0.46g SnCl 4 ·5H 2 O was dissolved in 10 mL of deionized water, and after dissolution, it was added to a beaker containing 28 g of tetraethyl orthosilicate (TEOS) and stirred for 30 minutes. Then, 48 g of tetrapropylammonium hydroxide (TPAOH) was weighed and slowly added dropwise to the above solution, and stirring was continued for 1 hour. Finally, 40 mL of deionized water was added and stirred for more than 30 minutes. The obtained gel was transferred to a 250 mL polytetrafluoroethylene hydrothermal autoclave and crystallized in an oven at 180°C for 72 hours. After crystallization, it was cooled to room temperature, the solid material was taken out and washed with deionized water 3 times, and dried in an oven at 100°C for 12 hours. The dried solid was placed in a muffle furnace and calcined at 550°C for 5 hours. After cooling, it was taken out and ground to obtain a 1% Sn metal-doped MFI molecular sieve, named sample 1#. The XRD pattern is shown in Figure 1 As shown, the TEM image at 200nm scale is Figure 2 shown.
[0058] Example 2
[0059] Weigh 0.92g SnCl 4 ·5H 2O was dissolved in 20 mL of deionized water, and after dissolution, it was added to a beaker containing 28 g of tetraethyl orthosilicate (TEOS) and stirred for 30 minutes. Then, 50 g of tetrapropylammonium hydroxide (TPAOH) was weighed and slowly added dropwise to the above solution, and stirring was continued for 1 hour. Finally, 40 mL of deionized water was added and stirred for more than 30 minutes. The obtained gel was transferred to a 250 mL polytetrafluoroethylene hydrothermal autoclave and crystallized in an oven at 180°C for 72 hours. After crystallization, it was cooled to room temperature, the solid material was taken out and washed with deionized water 3 times, and dried in an oven at 100°C for 12 hours. The dried solid was placed in a muffle furnace and calcined at 550°C for 5 hours. After cooling, it was taken out and ground to obtain a 2% Sn metal-doped MFI molecular sieve, named sample 2#. The XRD pattern is shown in Figure 1 shown.
[0060] Example 3
[0061] Weigh 0.3g ZrCl 4 Dissolve in 10mL deionized water, add to a beaker containing 28g tetraethyl orthosilicate (TEOS) after dissolution, and stir for 30 minutes. Then, weigh 50g tetrapropylammonium hydroxide (TPAOH) and slowly add it dropwise to the above solution, and continue stirring for 1 hour. Finally, add 40mL deionized water and stir for more than 30 minutes. The obtained gel is transferred to a 250mL polytetrafluoroethylene hydrothermal autoclave and crystallized in an oven at 180°C for 72 hours. After crystallization, cool to room temperature, take out the solid material and wash it 3 times with deionized water, and dry it in an oven at 100°C for 12 hours. The dried solid is placed in a muffle furnace and calcined at 550°C for 5 hours. After cooling, take it out and grind it to obtain a 1% Zr metal-doped MFI molecular sieve, named sample 3#. The XRD pattern is as shown below Figure 1 shown.
[0062] Example 4
[0063] Weigh 0.25g TiCl 4 Dissolve in 10mL deionized water, add to a beaker containing 28g tetraethyl orthosilicate (TEOS) after dissolution, and stir for 30 minutes. Then, weigh 50g tetrapropylammonium hydroxide (TPAOH) and slowly add it dropwise to the above solution, and continue stirring for 1 hour. Finally, add 40mL deionized water and stir for more than 30 minutes. The obtained gel is transferred to a 250mL polytetrafluoroethylene hydrothermal autoclave and crystallized in an oven at 180°C for 72 hours. After crystallization, cool to room temperature, take out the solid material and wash it 3 times with deionized water, and dry it in an oven at 100°C for 12 hours. The dried solid is placed in a muffle furnace and calcined at 550°C for 5 hours. After cooling, take it out and grind it to obtain a 1% Zr metal-doped MFI molecular sieve, named sample 4#. The XRD pattern is as shown below Figure 1 shown.
[0064] Example 5
[0065] Weigh 2g of sodium hydroxide and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 5g of sample 1# and add it to the three-necked flask, and stir and treat it at 80°C for 1h. The reaction solution is hot filtered, washed, and dried to obtain an alkali-treated molecular sieve.
[0066] Weigh 1.08g of ammonium chloride and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 2g of alkali-treated molecular sieve and add it to the three-necked flask, and stir for 1h. Finally, the reaction solution was hot filtered and washed, dried at 100°C for 12h, and calcined at 550°C for 7h to obtain a hydrogen-type alkali-treated modified molecular sieve, named sample 5#.
[0067] Example 6
[0068] Weigh 2g of sodium hydroxide and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 5g of sample 2# and add it to the three-necked flask, and stir and treat it at 80°C for 1h. The reaction solution is hot filtered, washed, and dried to obtain an alkali-treated molecular sieve.
[0069] Weigh 1.08g of ammonium chloride and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 2g of alkali-treated molecular sieve and add it to the three-necked flask, stirring for 1h. Finally, the reaction solution was hot filtered and washed, dried at 100°C for 12h, and calcined at 550°C for 7h to obtain a hydrogen-type alkali-treated modified molecular sieve, named sample 6#.
[0070] Example 7
[0071] Weigh 2g of sodium hydroxide and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 5g of sample 3# and add it to the three-necked flask, and stir and treat it at 80°C for 1h. The reaction solution is hot filtered, washed, and dried to obtain an alkali-treated molecular sieve.
[0072] Weigh 1.08g of ammonium chloride and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 2g of alkali-treated molecular sieve and add it to the three-necked flask, and stir for 1h. Finally, the reaction solution was hot filtered and washed, dried at 100°C for 12h, and calcined at 550°C for 7h to obtain a hydrogen-type alkali-treated modified molecular sieve, named sample 7#.
[0073] Example 8
[0074] Weigh 2g of sodium hydroxide and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 5g of sample 4# and add it to the three-necked flask, and stir and treat it at 80°C for 1h. The reaction solution is hot filtered, washed, and dried to obtain an alkali-treated molecular sieve.
[0075] Weigh 1.08g of ammonium chloride and add it to a three-necked flask containing 100mL of deionized water, and heat it to 80°C in an oil bath. Then, weigh 2g of alkali-treated molecular sieve and add it to the three-necked flask, and stir for 1h. Finally, the reaction solution was hot filtered and washed, dried at 100°C for 12h, and calcined at 550°C for 7h to obtain a hydrogen-type alkali-treated modified molecular sieve, named sample 8#.
[0076] Example 9
[0077] Weigh 0.6g of octadecyltrichlorosilane into a beaker containing 100mL of toluene, stir evenly and pour into a flask. Then, weigh 5g of sample 5# into the flask and stir and reflux at 30°C for 10h. Finally, the reaction mixture was filtered, washed with anhydrous ethanol 3 times, and dried at 110°C for 12h to obtain a silanized modified molecular sieve, named sample 9#.
[0078] Example 10
[0079] Weigh 0.6g of octadecyltrichlorosilane into a beaker containing 100mL of toluene, stir evenly and pour into a flask. Then, weigh 5g of sample 6# into the flask and stir and reflux at 30°C for 10h. Finally, the reaction mixture was filtered, washed with anhydrous ethanol 3 times, and dried at 110°C for 12h to obtain a silanized modified molecular sieve, named sample 10#.
[0080] Embodiment 11
[0081] Weigh 0.6g of octadecyltrichlorosilane into a beaker containing 100mL of toluene, stir evenly and pour into a flask. Then, weigh 5g of sample 7# into the flask and stir and reflux at 30°C for 10h. Finally, the reaction mixture was filtered, washed with anhydrous ethanol 3 times, and dried at 110°C for 12h to obtain a silanized modified molecular sieve, named sample 11#.
[0082] Example 12
[0083] Weigh 0.6g of octadecyltrichlorosilane into a beaker containing 100mL of toluene, stir evenly and pour into a flask. Then, weigh 5g of sample 8# into the flask and stir and reflux at 30°C for 10h. Finally, the reaction mixture was filtered, washed with anhydrous ethanol 3 times, and dried at 110°C for 12h to obtain a silanized modified molecular sieve, named sample 12#.
[0084] Comparative Example 1
[0085] Weigh 28g of tetraethyl orthosilicate (TEOS) and add it to a beaker, stir for 30 minutes. Then, weigh 48g of tetrapropylammonium hydroxide (TPAOH) and slowly add it dropwise to the above solution, and continue stirring for 1 hour. Finally, add 40mL of deionized water and stir for more than 30 minutes. The obtained gel was transferred to a 250mL polytetrafluoroethylene hydrothermal autoclave and crystallized in an oven at 180°C for 72 hours. After crystallization, wait for cooling to room temperature, take out the solid material and wash it with deionized water 3 times, and dry it in an oven at 100°C for 12 hours. The dried solid was placed in a muffle furnace, calcined at 550°C for 5 hours, taken out after cooling and ground to obtain a pure MFI molecular sieve, named sample 13#.
[0086] Test Example 1
[0087] 30 mL of n-butanol and 1.5 g of furfuryl alcohol were added to a 100 mL three-necked flask, and the flask was placed in an oil bath, heated and stirred under condensation reflux, and after the reaction temperature reached 110°C, 0.75 g of catalyst samples 1# to 13# were added, and the timing was started. After a certain reaction time, the flask was placed in ice water for rapid cooling, and then transferred to a 500 mL volumetric flask, the volume was fixed with anhydrous ethanol, and the concentrations of furfuryl alcohol and n-butyl furfuryl ether were detected by liquid chromatography, and then the furfuryl alcohol conversion rate and n-butyl furfuryl ether yield were calculated, and the results are shown in Table 1.
[0088] For the catalyst with obviously reduced performance, it was first dried in an oven at 110°C for 12 hours, and then calcined in a muffle furnace at 550°C for 5 hours. Subsequently, the calcined catalyst was silanized again, and the silanized catalyst was continuously used to catalyze the furfuryl alcohol etherification reaction.
[0089] Table 1. Performance of different molecular sieves in etherification of furfuryl alcohol and n-butanol
[0090] catalyst Reaction time Furfuryl alcohol conversion Yield of n-butyl furfuryl ether 1 3h 71% 58% 1 6h 90% 69% 2 1h 62% 50% 2 3h 82% 73% 2 6h 95% 76% 3 3h 59% 45% 3 6h 80% 63% 4 3h 45% 30% 4 6h 75% 56% 5 3h 90% 76% 6 3h 92% 81% 7 3h 79% 72% 8 3h 55% 40% 9 3h 99% 83% 10 3h 99% 86% 11 3h 92% 80% 12 3h 81% 69% 13 3h 5% 0%
[0091] As shown in Table 1, when the metal-doped MFI molecular sieves (1-4#) catalyze the etherification reaction of furfuryl alcohol and n-butanol, although prolonging the reaction time can promote the conversion of furfuryl alcohol, the highest yield of n-butyl furfuryl ether is only 76%, and a large amount of furfuryl alcohol is still converted into by-products. After alkali treatment, the conversion activity of catalysts (5-8#) is significantly improved, and the yield of n-butyl furfuryl ether is also increased to more than 80%. After silanization modification of the alkali-treated molecular sieves, the activity of catalysts (9-12#) is further accelerated, and the yield of n-butyl furfuryl ether on catalyst 10# reaches more than 85%. On sample 13#, the conversion rate of furfuryl alcohol is only 5% after 3h of reaction, and no n-butyl furfuryl ether is generated. It is difficult for pure MFI molecular sieves to catalyze the etherification of furfuryl alcohol. These results indicate that metal-doped molecular sieves can catalyze the etherification reaction of furfuryl alcohol and n-butanol. Their activity comes from the acidic sites generated by metal doping. Alkali treatment and silanization modification can significantly inhibit the occurrence of side reactions and achieve highly selective etherification of furfuryl alcohol.
[0092] Test Example 2
[0093] 30mL of n-butanol and 1.5g of furfuryl alcohol were added to a 100mL three-necked flask, and the flask was placed in an oil bath, heated and stirred under condensation reflux, and after the reaction temperature reached 110°C, 0.75g of 10# catalyst was added and timing was started. After a certain reaction time, the flask was placed in ice water for rapid cooling, and then transferred to a 500mL volumetric flask, fixed to volume with anhydrous ethanol, and the concentrations of furfuryl alcohol and n-butyl furfuryl ether were detected by liquid chromatography, and then the furfuryl alcohol conversion rate and n-butyl furfuryl ether yield were calculated.
[0094] The catalyst was applied 5 times, and the results are shown in Table 2, wherein the filtered catalyst was first ultrasonically cleaned once with anhydrous ethanol, and then ultrasonically cleaned twice with deionized water after filtration, and then placed in an oven at 110°C to dry for 12 hours, and finally continued to be used to catalyze the furfuryl alcohol etherification reaction.
[0095] Table 2. Stability of 10# sample catalyzing the etherification reaction of furfuryl alcohol and n-butanol
[0096] Number of applications Reaction time Furfuryl alcohol conversion Yield of n-butyl furfuryl ether 1 3h 99% 86% 2 3h 98% 84% 3 3h 92% 80% 4 3h 88% 72% 5 3h 99% 85%
[0097] Note: Before the fifth application, the catalyst was calcined and silanized in sequence.
[0098] Table 2 shows the stability of the 10# sample in catalyzing the reaction of furfuryl alcohol and n-butanol. As the number of applications increases, the performance of the catalyst decreases, but the yield of n-butyl furfuryl ether remains above 80%. However, in the fourth application, both the furfuryl alcohol conversion rate and the yield of n-butyl furfuryl ether decreased significantly, which may be due to the macromolecular byproducts formed by the self-polymerization of furfuryl alcohol covering the active center of the catalyst. After calcination and silanization treatment, the performance of the catalyst was restored, indicating that the catalyst has good stability.
[0099] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a modified molecular sieve, characterized in that: The steps include: S1, subjecting a mixed solution containing tetraethyl orthosilicate, a metal precursor, tetrapropylammonium hydroxide and water to a hydrothermal reaction and calcining I to obtain a metal-doped MFI molecular sieve; S2, treating the metal-doped MFI molecular sieve with alkali, exchanging with ammonium, and calcining II to obtain the modified molecular sieve.
2. The preparation method according to claim 1, characterized in that: The step S2 further comprises performing a silanization treatment after calcination II.
3. The preparation method according to claim 1, characterized in that: The weight ratio of tetraethyl orthosilicate, tetrapropylammonium hydroxide and water is 1:(1.2-2.3):(1.5-3); Preferably, the metal precursor is selected from at least one of tin tetrachloride, zirconium tetrachloride and titanium tetrachloride; Preferably, the molar ratio of the metal element to the silicon element in the metal precursor and tetraethyl orthosilicate is 0.01 to 0.03:1; Preferably, the conditions of the hydrothermal reaction are: reaction temperature is 170-190°C, reaction time is 60-84h; Preferably, the calcination conditions of the method I are: calcination at 500-600° C. for 4-6 hours.
4. The preparation method according to claim 1, characterized in that: In the step S2, the alkali treatment comprises: immersing the metal-doped MFI molecular sieve in an aqueous alkali solution, heating at 75 to 85° C. for 0.5 to 1.5 hours, to obtain an alkali-treated molecular sieve; Preferably, the weight ratio of the metal-doped MFI molecular sieve to the base is 2 to 3:1; Preferably, the alkali is selected from at least one of sodium hydroxide and potassium hydroxide.
5. The preparation method according to claim 4, characterized in that: In the step S2, the ammonium exchange treatment and roasting II comprises: immersing the alkali-treated molecular sieve in an aqueous solution of ammonium, heating at 75 to 85° C. for 0.5 to 1.5 h, and roasting to obtain a hydrogen-type alkali-treated modified molecular sieve; Preferably, the weight ratio of the alkali-treated molecular sieve to ammonium is 1:0.5-0.6; Preferably, the concentration of the aqueous solution of ammonium is 0.01 to 0.015 g / mL; Preferably, the ammonium is at least one selected from ammonium chloride, ammonium nitrate and ammonium sulfate; Preferably, the calcination conditions II are: calcination at 500-600° C. for 6-8 hours.
6. The preparation method according to claim 2, characterized in that: The silanization treatment comprises: immersing the modified molecular sieve obtained in step S2 into a silane modifier solution, and refluxing at 20 to 40° C. for 8 to 12 hours; Preferably, the weight ratio of the hydrogen-type alkali-treated modified molecular sieve to the silane modifier is 1:0.1 to 0.15; Preferably, the solvent of the silane modifier is an organic solvent.
7. The modified molecular sieve prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The particle size of the modified molecular sieve is 200-500 nm.
8. Use of at least one of the modified molecular sieve prepared by the preparation method according to any one of claims 1 to 6 and the modified molecular sieve according to claim 7 as a catalyst in catalyzing the etherification of furfuryl alcohol to synthesize alkoxyfurfuryl ether.
9. The use according to claim 8, characterized in that: The steps include: The modified molecular sieve is contacted with a mixed solution of furfuryl alcohol and alkyl alcohol, and heated for reaction to obtain alkoxy furfuryl ether.
10. The use according to claim 9, characterized in that: The weight ratio of the modified molecular sieve, furfuryl alcohol and alkyl alcohol is 1:(1-3):(15-40); Preferably, the conditions for the heating reaction are: reaction temperature is 100-120°C, and reaction time is 1-6h; Preferably, the alkyl alcohol is selected from n-butanol, and the alkoxy furfuryl ether is selected from n-butyl furfuryl ether.