Preparation method of gas-sensitive material and gas-sensitive material
Through the hydrothermal reaction between porous graphene and zinc oxide composite, the problem of insufficient performance of a single zinc oxide gas-sensitive material is solved, and more efficient gas-sensitive performance and simplified preparation process are achieved.
Patent Information
- Application Number
- CN202411113110.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing single zinc oxide gas-sensitive materials have high working temperature, low sensitivity, long response recovery time, complex preparation steps and low efficiency, resulting in poor gas-sensitive performance.
Porous graphene and zinc oxide composite materials are used to prepare porous graphene/zinc oxide gas-sensitive materials by ultrasonic dispersing porous graphene ethanol aqueous solution and dissolved with zinc chloride and sodium hydroxide, which simplifies the preparation process and improves the Material properties.
Reduces operating temperature, improves sensitivity, shortens response recovery time, improves gas-sensitive performance, and simplifies preparation steps, reducing equipment complexity and production costs.
Smart Images

Figure CN119018929A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of material technology, and in particular, to a method for preparing a gas-sensitive material and a gas-sensitive material. Background Art
[0002] The combustion of fossil fuels such as coal and oil, the leakage of various waste gases in industrial production and manufacturing, and the release of harmful gases from indoor furniture and building materials in daily life not only pollute the environment but also endanger human health. Therefore, it is urgent to develop gas sensing technology and develop gas sensing equipment to effectively and real-time monitor gases that threaten the human environment and health.
[0003] In the related art, in practical applications, a single zinc oxide gas-sensitive material is generally prepared. However, a single zinc oxide gas-sensitive material has certain limitations, such as high operating temperature, low sensitivity, long response recovery time, poor gas-sensitive performance, complex preparation steps and low preparation efficiency. Summary of the invention
[0004] The purpose of the present disclosure is to provide a method for preparing a gas-sensitive material and a gas-sensitive material, thereby overcoming, at least to a certain extent, the problems of complicated preparation steps, low preparation efficiency and poor gas-sensitive performance of the gas-sensitive material caused by the limitations and defects of the relevant technology.
[0005] According to one aspect of the present disclosure, a method for preparing a gas-sensitive material is provided, comprising: using porous graphene as a starting material, ultrasonically dispersing a porous graphene ethanol aqueous solution to obtain a first solution; using zinc chloride as a zinc source and sodium hydroxide as a precipitant, dissolving the zinc source and the precipitant in the ethanol aqueous solution in sequence to obtain a suspension; adding the suspension dropwise to the first solution to obtain a mixed solution; transferring the mixed solution to a reactor for a hydrothermal reaction, and cooling to room temperature after the hydrothermal reaction for centrifugation, washing and freeze-drying to obtain a porous graphene / zinc oxide gas-sensitive material.
[0006] In an exemplary embodiment of the present disclosure, the molar ratio of the precipitant to the zinc source is 10:1 to 20:1.
[0007] In an exemplary embodiment of the present disclosure, the reaction temperature of the hydrothermal reaction is 120 to 160° C., and the reaction time of the hydrothermal reaction is 6 to 18 hours.
[0008] In an exemplary embodiment of the present disclosure, the freeze-drying time is 48 to 60 hours.
[0009] In an exemplary embodiment of the present disclosure, the size of the zinc oxide gas-sensitive material in the porous graphene / zinc oxide gas-sensitive material is 1 to 2.5 μm, and the zinc oxide gas-sensitive material is uniformly distributed on the surface of the porous graphene.
[0010] In an exemplary embodiment of the present disclosure, zinc chloride is used as a zinc source and sodium hydroxide is used as a precipitant, and the zinc source and the precipitant are sequentially dissolved in an ethanol aqueous solution to obtain a suspension, including: dissolving the zinc source in the ethanol aqueous solution, stirring to obtain a second suspension; dissolving the precipitant in the ethanol aqueous solution, stirring and adding dropwise to the second suspension to obtain a third suspension, and using the third suspension as the suspension.
[0011] In an exemplary embodiment of the present disclosure, the method further includes: preparing the gas-sensitive material into a slurry, coating the slurry on a ceramic tube to assemble into a gas-sensitive element; and performing a gas-sensitive performance test on the gas-sensitive element to determine the gas-sensitive response and response time.
[0012] In an exemplary embodiment of the present disclosure, the operating temperature of the gas-sensing performance test is 200-300°C.
[0013] In an exemplary embodiment of the present disclosure, the gas used in the gas-sensitive performance test is acetone.
[0014] According to one aspect of the present disclosure, a gas-sensitive material is provided. The gas-sensitive material is prepared according to any one of the above-mentioned methods for preparing a gas-sensitive material.
[0015] In the technical solution provided in the embodiments of the present disclosure, on the one hand, porous graphene is used as the starting material, zinc chloride is used as the zinc source, and sodium hydroxide is used as the precipitant, and an ethanol aqueous solution is added to obtain a suspension, and the suspension is further added dropwise to the first solution represented by the porous graphene dispersion to obtain a mixed solution, and the mixed solution is transferred to a reactor for hydrothermal reaction, cooled to room temperature, centrifuged and washed, and freeze-dried to obtain a porous graphene / zinc oxide gas-sensitive material. Compared with a single zinc oxide, the porous graphene / zinc oxide gas-sensitive material in the embodiments of the present disclosure reduces the operating temperature, improves the sensitivity, reduces the response recovery time, and effectively improves its gas-sensitive performance. On the other hand, only a simple hydrothermal reaction is required to prepare the porous graphene / zinc oxide gas-sensitive material, the operation steps are simple, and no complicated instruments and equipment are required, thereby reducing the preparation complexity and improving the preparation efficiency.
[0016] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0018] Figure 1 A flow chart schematically illustrates a method for preparing a gas-sensitive material in an embodiment of the present disclosure.
[0019] Figure 2 The XRD pattern of the porous graphene / zinc oxide gas sensing material is schematically shown.
[0020] Figure 3 The SEM image of the porous graphene / zinc oxide gas-sensitive material prepared according to Example 1 is schematically shown.
[0021] Figure 4 The response recovery curve obtained by assembling the porous graphene / zinc oxide gas-sensitive material prepared in Example 1 into a gas-sensitive element and testing is schematically shown.
[0022] Figure 5 The SEM image of the porous graphene / zinc oxide gas-sensitive material prepared according to Example 2 is schematically shown.
[0023] Figure 6 The response recovery curve obtained by assembling the porous graphene / zinc oxide gas-sensitive material prepared in Example 2 into a gas-sensitive element is schematically shown.
[0024] Figure 7 The SEM image of the porous graphene / zinc oxide gas-sensitive material prepared according to Example 3 is schematically shown.
[0025] Figure 8 The porous graphene / zinc oxide gas-sensitive material prepared according to Example 3 is assembled into a gas-sensitive element and tested in accordance with different operating temperatures. The gas-sensitive response line graph is schematically shown.
[0026] Fig. 9 The porous graphene / zinc oxide gas-sensitive material prepared according to Example 3 is schematically shown as a bar graph of the gas-sensitive response corresponding to different gases when assembled into a gas-sensitive element for testing.
[0027] Fig.10 The response recovery curve obtained by assembling the porous graphene / zinc oxide gas-sensitive material prepared in Example 3 into a gas-sensitive element is schematically shown.
[0028] Fig.11 The SEM image of the porous graphene / zinc oxide gas-sensitive material prepared according to Example 4 is schematically shown.
[0029] Fig.12 The response recovery curve obtained by assembling the porous graphene / zinc oxide gas-sensitive material prepared in Example 4 into a gas-sensitive element is schematically shown.
[0030] Fig.13 The SEM image of the porous graphene / zinc oxide gas-sensitive material prepared according to Example 5 is schematically shown.
[0031] Fig.14 The response recovery curve obtained by assembling the porous graphene / zinc oxide gas-sensitive material prepared in Example 5 into a gas-sensitive element is schematically shown. DETAILED DESCRIPTION
[0032] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0033] The terms "a", "an", "the" and "said" used in this specification are used to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components, etc. in addition to the listed elements / components, etc.; the terms "first" and "second" etc. are used only as labels and are not intended to limit the quantity of their objects.
[0034] With the rapid development of industry and technology, while material life is greatly satisfied, people have higher and higher requirements for their own safety and the quality of the surrounding environment. The combustion of fossil fuels such as coal and oil, the leakage of various waste gases in industrial production and manufacturing processes, and the release of harmful gases in indoor furniture and building materials in daily life not only pollute the environment but also endanger human health. Therefore, there is an urgent need to develop gas sensing technology and develop gas sensing equipment to effectively and in real time monitor gases that threaten human environment and health. As the core component of gas sensing equipment, gas-sensitive materials greatly affect the gas-sensitive properties of materials and are currently a hot topic of research.
[0035] Zinc oxide is a traditional and common metal oxide-based semiconductor gas-sensitive material with the advantages of stable physical and chemical properties, non-toxicity, and relatively low price. Many studies have been devoted to its morphology control, and nanobelts, nanorods, nanotubes, hollow spheres, etc. have been synthesized. However, in practical applications, single zinc oxide gas-sensitive materials still have certain limitations, such as high operating temperature, low sensitivity, and long response recovery time.
[0036] In order to solve the above technical problems, the present disclosure provides a method for preparing a gas-sensitive material in an embodiment, which is used to prepare a porous graphene / zinc oxide gas-sensitive material. Figure 1 As shown in , it mainly includes the following steps:
[0037] In step S110, porous graphene is used as a starting material, and an ethanol aqueous solution of porous graphene is ultrasonically dispersed to obtain a first solution;
[0038] In step S120, zinc chloride is used as a zinc source and sodium hydroxide is used as a precipitant, and the zinc source and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension;
[0039] In step S130, the suspension is added dropwise to the first solution to obtain a mixed solution;
[0040] In step S140, the mixed solution is transferred to a reactor for a hydrothermal reaction, and after the hydrothermal reaction, the mixed solution is cooled to room temperature for centrifugation, washing, and freeze-drying to obtain a porous graphene / zinc oxide gas-sensitive material.
[0041] In the disclosed embodiment, on the one hand, porous graphene is used as the starting material, zinc chloride is used as the zinc source, and sodium hydroxide is used as the precipitant to prepare a suspension, the suspension is added dropwise to the first solution to obtain a mixed solution, the mixed solution is transferred to a reactor for hydrothermal reaction, cooled to room temperature, centrifuged and washed, and freeze-dried to obtain a porous graphene / zinc oxide gas-sensitive material. By introducing porous graphene and zinc oxide composite, compared with a single zinc oxide, porous graphene / zinc oxide gas-sensitive materials can overcome the problems of single metal oxide in the application of gas sensors, reduce operating temperature, improve sensitivity, reduce response recovery time, and effectively improve its gas-sensitive performance. On the other hand, only a simple hydrothermal reaction is required to prepare porous graphene / zinc oxide gas-sensitive materials, the operating steps are simple, and complex instruments and equipment are not required, so the preparation complexity is reduced and the preparation efficiency is improved.
[0042] Next, combine Figure 1 The preparation method of the gas-sensitive material in the embodiment of the present disclosure is described in detail.
[0043] In step S110, porous graphene is used as a starting material, and an ethanol aqueous solution of porous graphene is ultrasonically dispersed to obtain a first solution.
[0044] In the disclosed embodiments, porous graphene refers to a carbon material with nanoscale pores on a two-dimensional base surface. Porous graphene can be prepared by metal etching, and porous graphene is used as a starting material. After obtaining the porous graphene, a 50 vol% ethanol aqueous solution of porous graphene can be ultrasonically dispersed to obtain a first solution, which can be recorded as solution I. Compared with graphene, porous graphene with a vacancy structure has many unique properties due to the presence of defects, such as ultra-large surface area, abundant mass transfer channels, adjustable energy band gap and good mechanical stability, etc., which makes porous graphene have a wider range of applications in superelectrics, sensors, catalysis, electrochemical energy storage and seawater desalination.
[0045] In step S120, zinc chloride is used as a zinc source, sodium hydroxide is used as a precipitant, and the zinc source and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension.
[0046] In the disclosed embodiment, the zinc source can be dissolved in an ethanol aqueous solution, and the precipitant can be dissolved in the ethanol aqueous solution and added dropwise to the ethanol aqueous solution in which the zinc source is dissolved, and then rapidly stirred to obtain a final suspension. Among them, zinc chloride can be used as the zinc source, and sodium hydroxide can be used as the precipitant. In addition, other components can also be used as the zinc source and the precipitant, which are not specifically limited here.
[0047] For example, the zinc source can be dissolved in an ethanol aqueous solution, and the solution is stirred rapidly to obtain a second suspension; the precipitant is dissolved in an ethanol aqueous solution, stirred rapidly and added dropwise to the second suspension to obtain a third suspension, and the third suspension is used as the suspension. The ethanol aqueous solutions used to dissolve the zinc source and the precipitant can be stored in different containers, but their components can be exactly the same.
[0048] Specifically, zinc chloride can be used as a zinc source, dissolved in a 50 vol% ethanol aqueous solution in a first container, and stirred rapidly to obtain a second suspension, i.e., suspension II; sodium hydroxide can be used as a precipitant, dissolved in a 50 vol% ethanol aqueous solution in a second container, and stirred rapidly, and the stirred suspension can be added dropwise to the second suspension in the first container to obtain a third suspension, i.e., suspension III. Furthermore, the third suspension can be used as the final suspension.
[0049] In step S130, the suspension is added dropwise to the first solution to obtain a mixed solution.
[0050] In the disclosed embodiment, the suspension can be added dropwise to the first solution to obtain a mixed solution. For example, the suspension III can be added dropwise to the first solution represented by the porous graphene dispersion, that is, solution I, to obtain a mixed solution IV.
[0051] In the process of adding the suspension dropwise to the first solution, the precipitant and the zinc source can be added in different molar ratios. Specifically, the molar ratio of the precipitant to the zinc source is 10:1 to 20:1, which can be determined according to the content of the precipitant and the zinc source. For example, the molar ratio of the precipitant to the zinc source can be 10:1, 20:1, or other ratios. Based on this, the content of the zinc source and the precipitant can be adjusted, and the content of the zinc source and the precipitant can be, for example: 1 mmol of zinc source, 10 mmol of precipitant; 1 mmol of zinc source, 20 mmol of precipitant.
[0052] In step S140, the mixed solution is transferred to a reactor for a hydrothermal reaction, and after the hydrothermal reaction, the mixed solution is cooled to room temperature for centrifugation, washing, and freeze-drying to obtain a porous graphene / zinc oxide gas-sensitive material.
[0053] In the disclosed embodiments, the mixed solution IV can be transferred to a reactor for a hydrothermal reaction. A hydrothermal reaction is a chemical process in which water reacts with other substances as a solvent under high pressure and high temperature. The hydrothermal reaction is usually carried out in a closed reaction vessel, and the reaction temperature is usually above 100°C and the pressure is above normal pressure to increase the reaction rate and change the composition of the reaction products. In some embodiments, the reaction temperature of the hydrothermal reaction can be 120 to 160°C, and the reaction time of the hydrothermal reaction can be 6 to 18 hours, for example, 6 hours, 12 hours, and 18 hours, and the reaction time of 12 hours is used as an example for explanation. The reaction temperature and reaction time of the hydrothermal reaction can be adjusted according to actual needs. For example, the reaction temperature of the hydrothermal reaction can be 120°C, 140°C, or 160°C.
[0054] After the hydrothermal reaction, it can be cooled to room temperature and centrifuged, washed and freeze-dried to obtain a gas-sensitive material. The gas-sensitive material can be a porous graphene / zinc oxide gas-sensitive material, that is, a zinc oxide gas-sensitive material is generated on the surface of the porous graphene. Among them, the size of the zinc oxide gas-sensitive material in the porous graphene / zinc oxide gas-sensitive material is 1 to 2.5 μm, and the zinc oxide gas-sensitive material is evenly distributed on the surface of the porous graphene. Among them, the freeze-drying time can be 48 to 60 hours, for example, 48 hours, 55 hours, and 60 hours. 48 hours is used as an example for explanation here, and it can also be adjusted according to actual needs.
[0055] After the gas-sensitive material is prepared, the gas-sensitive material can be added to ultrapure water to form a slurry, which can be coated on a ceramic tube to be assembled into a gas-sensitive element, so as to perform a gas-sensitive performance test through the gas-sensitive element.
[0056] Next, the preparation method of the gas-sensitive material in the embodiment of the present disclosure is described in detail.
[0057] Example 1
[0058] The preparation method of the gas-sensitive material specifically comprises the following steps:
[0059] Step 1: Prepare porous graphene by simple metal etching method and use it as starting material, ultrasonically disperse porous graphene in 50 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., solution I;
[0060] Step 2: Using zinc chloride as a zinc source, weigh 1 mmol, dissolve it in a 50 vol% ethanol aqueous solution, and stir rapidly to obtain a second suspension, i.e., suspension II;
[0061] Step 3, using sodium hydroxide as a precipitant, weighing 10 mmol, dissolving it in a 50 vol% ethanol aqueous solution, rapidly stirring, and dropping it into the suspension II to obtain a third suspension, i.e., suspension III;
[0062] Step 4: Add the suspension III dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution IV; wherein the molar ratio of the precipitant sodium hydroxide to the zinc source zinc chloride is 10:1.
[0063] Step 5: Transfer the mixed solution IV to a reactor, perform a hydrothermal reaction at 100°C for 12 hours, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / zinc oxide gas-sensitive material. The gas-sensitive material is a flower cluster-shaped gas-sensitive material.
[0064] Step 6: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0065] Figure 2 A schematic diagram of X-ray diffraction testing of gas-sensitive materials is shown schematically in FIG. Figure 2As shown in the figure, the peaks at 2θ=10° and 26.5° in the spectrum correspond to the (001) and (002) crystal planes of graphene, and the peaks at 2θ=31.7°, 34.5°, 36.3°, 47.6°, 56.6°, 62.9°, 66.4°, 67.9° and 69.1° in the spectrum correspond to the (100), (002), (101), (102), (110), (103), (200), (112) and (201) crystal planes of zinc oxide, demonstrating the successful preparation of porous graphene / zinc oxide gas-sensitive materials.
[0066] Figure 3 The schematic diagram of the scanning electron microscope of the gas-sensitive material prepared in Example 1 is shown schematically in FIG. Figure 3 As shown in the figure, it can be seen that flower-like zinc oxide (about 1 μm in size) is distributed on the surface of the porous graphene, and there are some rod-like zinc oxide scattered around. This may be due to the fact that the flower-like structure is not fully developed due to the low hydrothermal temperature.
[0067] Next, the gas-sensitive material prepared in Example 1 was assembled into a gas-sensitive element to test the gas-sensitive performance. Figure 4 As shown in , when the working temperature is 260°C, the gas sensitive response of the gas sensitive material to 50ppm acetone gas is 9.3, and the response time is 11s.
[0068] Example 2
[0069] Compared with Example 1, the reaction temperature of the hydrothermal reaction is increased to 120° C. Based on this, the preparation method of the gas-sensitive material specifically includes the following steps:
[0070] Step 1: Prepare porous graphene by simple metal etching method and use it as starting material, ultrasonically disperse porous graphene in 50 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., solution I;
[0071] Step 2: Using zinc chloride as a zinc source, weigh 1 mmol, dissolve it in a 50 vol% ethanol aqueous solution, and stir rapidly to obtain a second suspension, i.e., suspension II;
[0072] Step 3, using sodium hydroxide as a precipitant, weighing 10 mmol, dissolving it in a 50 vol% ethanol aqueous solution, rapidly stirring, and dropping it into the suspension II to obtain a third suspension, i.e., suspension III;
[0073] Step 4: Add the suspension III dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution IV; wherein the molar ratio of the precipitant sodium hydroxide to the zinc source zinc chloride is 10:1.
[0074] Step 5: Transfer the mixed solution IV to a reactor, perform a hydrothermal reaction at 120°C for 12 hours, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / zinc oxide gas-sensitive material. The gas-sensitive material is a flower cluster-shaped gas-sensitive material.
[0075] Step 6: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0076] Figure 2 A schematic diagram of X-ray diffraction testing of gas-sensitive materials is shown schematically in FIG. Figure 2 As shown in the figure, there are obvious diffraction peaks of graphene and zinc oxide in the spectrum, which proves the successful preparation of porous graphene / zinc oxide gas-sensitive materials.
[0077] Figure 5 The schematic diagram of the gas-sensitive material prepared in Example 2 is shown schematically in FIG. Figure 5 As shown in the figure, it can be seen that flower-like zinc oxide (about 2 μm in size) is distributed on the surface of porous graphene, but the size of the flower-like zinc oxide is uneven. This may be due to the influence of hydrothermal conditions, and some flower-like structures are not fully developed.
[0078] Figure 6 FIG. 2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 2 into a gas-sensitive element for gas-sensitive performance testing. Figure 6 As shown, when the working temperature is 260°C, the gas sensitive response to 50ppm acetone gas is 14.1 and the response time is 8s.
[0079] Example 3
[0080] Compared with Example 1, the reaction temperature of the hydrothermal reaction is increased, and the reaction temperature of the hydrothermal reaction is 140° C. Based on this, the preparation method of the gas-sensitive material specifically includes the following steps:
[0081] Step 1: Prepare porous graphene by simple metal etching method and use it as starting material, ultrasonically disperse porous graphene in 50 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., solution I;
[0082] Step 2: Using zinc chloride as a zinc source, weigh 1 mmol, dissolve it in a 50 vol% ethanol aqueous solution, and stir rapidly to obtain a second suspension, i.e., suspension II;
[0083] Step 3, using sodium hydroxide as a precipitant, weighing 10 mmol, dissolving it in a 50 vol% ethanol aqueous solution, rapidly stirring, and dropping it into the suspension II to obtain a third suspension, i.e., suspension III;
[0084] Step 4: Add the suspension III dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution IV; wherein the molar ratio of the precipitant sodium hydroxide to the zinc source zinc chloride is 10:1.
[0085] Step 5: Transfer the mixed solution IV to a reactor, perform a hydrothermal reaction at 140°C for 12 hours, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / zinc oxide gas-sensitive material. The gas-sensitive material is a flower cluster-shaped gas-sensitive material.
[0086] Step 6: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0087] Figure 2 A schematic diagram of X-ray diffraction testing of gas-sensitive materials is shown schematically in FIG. Figure 2 As shown in the figure, there are obvious diffraction peaks of graphene and zinc oxide in the spectrum, which proves the successful preparation of porous graphene / zinc oxide gas-sensitive materials.
[0088] Figure 7 A schematic diagram of the gas-sensitive material prepared in Example 3 is shown schematically in FIG. Figure 7 As shown in the figure, it can be seen that flower-like zinc oxide (about 2.5 μm in size) is evenly distributed on the surface of the porous graphene, presenting a flower cluster structure.
[0089] Figure 8 FIG. 2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 3 into a gas-sensitive element for gas-sensitive performance testing. Figure 8 As shown, in the working temperature range of 200-300℃, the gas sensitive response test of acetone gas is carried out. Figure 8 As shown, it is found that when the working temperature is 260℃, the gas sensitive response value is the highest, which is 43.7. Therefore, the optimal working temperature of the gas sensor is 260℃.
[0090] like Fig. 9 The porous graphene / zinc oxide gas-sensitive material prepared in Example 3 was assembled into a gas-sensitive element and the gas-sensitive response values obtained by testing eight gases including 50 ppm acetone, isopropanol, and ethanol at the optimal working temperature of 260°C were found to have the best gas-sensitive response to acetone.
[0091] At the same time, its response recovery characteristics are tested, such as Fig.10 As shown, the response time is only 3s, which is faster than the response time of most gas-sensitive materials such as zinc oxide used in industrial applications.
[0092] Example 4
[0093] Compared with Example 1, the content of the precipitant is increased, the molar ratio of the precipitant sodium hydroxide and the zinc source zinc chloride is increased, and the reaction temperature of the hydrothermal reaction is increased. Among them, the molar ratio of the precipitant sodium hydroxide and the zinc source zinc chloride can be 20:1, and the reaction temperature of the hydrothermal reaction is 140°C. Based on this, the preparation method of the gas-sensitive material includes the following steps:
[0094] Step 1: Prepare porous graphene by simple metal etching method and use it as starting material, ultrasonically disperse porous graphene in 50 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., solution I;
[0095] Step 2: Using zinc chloride as a zinc source, weigh 1 mmol, dissolve it in a 50 vol% ethanol aqueous solution, and stir rapidly to obtain a second suspension, i.e., suspension II;
[0096] Step 3, using sodium hydroxide as a precipitant, weighing 20 mmol, dissolving it in a 50 vol% ethanol aqueous solution, rapidly stirring, and dropping it into the suspension II to obtain a third suspension, i.e., suspension III;
[0097] Step 4: Add the suspension III dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution IV; wherein the molar ratio of the precipitant sodium hydroxide to the zinc source zinc chloride is 20:1.
[0098] Step 5: Transfer the mixed solution IV to a reactor, perform a hydrothermal reaction at 140°C for 12 hours, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / zinc oxide gas-sensitive material. The gas-sensitive material is a flower cluster-shaped gas-sensitive material.
[0099] Step 6: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0100] Figure 2 A schematic diagram of X-ray diffraction testing of gas-sensitive materials is shown schematically in FIG. Figure 2 As shown in the figure, there are obvious diffraction peaks of graphene and zinc oxide in the spectrum, which proves the successful preparation of porous graphene / zinc oxide gas-sensitive materials.
[0101] Fig.11 The schematic diagram of the scanning electron microscope of the gas-sensitive material prepared in Example 4 is shown schematically in FIG. Fig.11 As shown in the figure, it can be seen that flower-like zinc oxide (about 2 μm in size) is distributed on the surface of porous graphene, some rod-like structures are randomly distributed, and a small amount of flower-like zinc oxide has a flake flower structure. This may be due to the increase in the ratio of precipitant sodium hydroxide to zinc source zinc chloride, resulting in abnormal development of the flower-like structure.
[0102] Fig.12 FIG. 4 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 4 into a gas-sensitive element for gas-sensitive performance testing. Fig.12 As shown, when the working temperature is 260°C, the gas-sensitive response to 50ppm acetone gas is 33.5, and the response time is 6s. Compared with Example 3, the gas-sensitive performance is reduced, which may be due to the abnormal development of flower-like zinc oxide, resulting in a decrease in the adsorption of acetone gas.
[0103] Example 5
[0104] Compared with Example 1, the reaction temperature of the hydrothermal reaction is increased, and the reaction temperature of the hydrothermal reaction is 160° C. Based on this, the preparation method of the gas-sensitive material includes the following steps:
[0105] Step 1: Prepare porous graphene by simple metal etching method and use it as starting material, ultrasonically disperse porous graphene in 50 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., solution I;
[0106] Step 2: Using zinc chloride as a zinc source, weigh 1 mmol, dissolve it in a 50 vol% ethanol aqueous solution, and stir rapidly to obtain a second suspension, i.e., suspension II;
[0107] Step 3, using sodium hydroxide as a precipitant, weighing 10 mmol, dissolving it in a 50 vol% ethanol aqueous solution, rapidly stirring, and dropping it into the suspension II to obtain a third suspension, i.e., suspension III;
[0108] Step 4: Add the suspension III dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution IV; wherein the molar ratio of the precipitant sodium hydroxide to the zinc source zinc chloride is 20:1.
[0109] Step 5: Transfer the mixed solution IV to a reactor, perform a hydrothermal reaction at 160°C for 12 hours, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / zinc oxide gas-sensitive material. The gas-sensitive material is a flower cluster-shaped gas-sensitive material.
[0110] Step 6: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0111] Figure 2 A schematic diagram of X-ray diffraction testing of gas-sensitive materials is shown schematically in FIG. Figure 2 As shown in the figure, there are obvious diffraction peaks of graphene and zinc oxide in the spectrum, which proves the successful preparation of porous graphene / zinc oxide gas-sensitive materials.
[0112] Fig.13 A schematic diagram of the gas-sensitive material prepared in Example 5 is shown schematically in FIG. Fig.13 As shown in the figure, it can be seen that the flower-like zinc oxide (size of about 2.5 μm) is randomly distributed on the surface of the porous graphene, and some flower-like structures are piled up and agglomerated, which is not conducive to the diffusion of the target gas, thereby reducing the gas sensing performance.
[0113] Fig.14 FIG. 5 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 5 into a gas-sensitive element for gas-sensitive performance testing. Fig.14 As shown, when the working temperature is 260°C, the gas sensitive response to 50ppm acetone gas is 20.2 and the response time is 5s.
[0114] The technical solution in the disclosed embodiment uses porous graphene as the starting material (prepared by a simple metal etching method), zinc chloride as a zinc source, sodium hydroxide as a precipitant, and a 50 vol% ethanol aqueous solution as a solvent. It is kept warm for 12 hours under hydrothermal conditions at 120-160°C, cooled to room temperature, centrifuged and washed, and freeze-dried to synthesize a cluster-shaped porous graphene / zinc oxide gas-sensitive composite material through a simple hydrothermal reaction; the flower-shaped zinc oxide (size of 1-2.5 μm) is evenly distributed on the surface of the porous graphene.
[0115] Flower cluster gas-sensitive materials were synthesized through a simple hydrothermal reaction. Compared with single zinc oxide and graphene / zinc oxide gas-sensitive materials, the porous structure of graphene and the flower-like structure of zinc oxide greatly increased the specific surface area of the composite material, and provided an effective diffusion channel for the adsorption and desorption of the target gas, greatly improving its gas-sensitive performance. The preparation process is simple, does not require complex instruments and equipment, and is easy to achieve industrial mass production.
[0116] In the flower-like gas-sensitive material prepared in the embodiment of the present disclosure, the size of the flower-like zinc oxide is about 200-500nm and is evenly distributed on the surface of the porous graphene. The size and distribution of the flower-like zinc oxide on the surface of the porous graphene can be controlled by adjusting the reaction temperature of the hydrothermal reaction and adjusting the molar ratio of the precipitant sodium hydroxide and the zinc source zinc chloride, which can better meet the requirements of the gas sensing field for gas-sensitive materials.
[0117] In this exemplary embodiment, a device is also provided. The device can be a device generated based on the gas-sensitive material, such as a mobile phone, a tablet computer, a laptop computer, a smart bracelet, a smart watch, a smart helmet, smart glasses, a vehicle, a robot, and any type of industrial equipment, etc., as long as it can contain the gas-sensitive material, and this exemplary embodiment does not specifically limit this.
[0118] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0119] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.
[0120] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A method for preparing a gas-sensitive material, characterized in that: include: Using porous graphene as a starting material, ultrasonically dispersing a porous graphene ethanol aqueous solution to obtain a first solution; Using zinc chloride as a zinc source and sodium hydroxide as a precipitant, the zinc source and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension; adding the suspension dropwise to the first solution to obtain a mixed solution; The mixed solution is transferred to a reactor for a hydrothermal reaction, and after the hydrothermal reaction, it is cooled to room temperature for centrifugation, washing and freeze-drying to obtain a porous graphene / zinc oxide gas-sensitive material.
2. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The molar ratio of the precipitant to the zinc source is 10:1 to 20:
1.
3. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The reaction temperature of the hydrothermal reaction is 120 to 160° C., and the reaction time of the hydrothermal reaction is 6 to 18 hours.
4. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The freeze-drying time is 48 to 60 hours.
5. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The size of the zinc oxide gas-sensitive material in the porous graphene / zinc oxide gas-sensitive material is 1 to 2.5 μm, and the zinc oxide gas-sensitive material is evenly distributed on the surface of the porous graphene.
6. The method for preparing a gas-sensitive material according to claim 1, characterized in that: Using zinc chloride as a zinc source and sodium hydroxide as a precipitant, the zinc source and the precipitant are sequentially dissolved in an ethanol aqueous solution to obtain a suspension, comprising: dissolving a zinc source in an ethanol aqueous solution and stirring to obtain a second suspension; The precipitant is dissolved in an ethanol aqueous solution, stirred and added dropwise to the second suspension to obtain a third suspension, and the third suspension is used as the suspension.
7. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The method further comprises: The gas-sensitive material is prepared into slurry, and coated on a ceramic tube to assemble into a gas-sensitive element; The gas sensing element is subjected to a gas sensing performance test to determine the gas sensing response and response time.
8. The method for preparing a gas-sensitive material according to claim 7, characterized in that: The working temperature of the gas-sensing performance test is 200-300°C.
9. The method for preparing a gas-sensitive material according to claim 7, characterized in that: The gas used in the gas-sensing performance test is acetone.
10. A gas-sensitive material, characterized in that: The gas-sensitive material is prepared according to the method for preparing a gas-sensitive material according to any one of claims 1 to 9.