Method for preparing gallium nitrate and flake silver powder through one-step method
By using the reduction reaction of metal Ga on AgNO3 in one-step, high-purity gallium nitrate and flake-shaped silver powder are generated, which solves the problems of environmental pollution and long production cycle in the traditional preparation process, and achieves efficient and environmentally friendly preparation of gallium nitrate and flake-shaped silver powder. .
Patent Information
- Application Number
- CN202411110834.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing environmental pollution caused by strong acids and alkalis during the preparation of gallium nitrate and the cumbersome preparation process and long cycles.
The reduction reaction of metal Ga on AgNO3 was performed by a one-step method to synchronize high-purity Ga(NO3)3 and sheet-like Ag. Ga after ultrasonication and surface treatment reacted with AgNO3 solution at a preset temperature, and then dried in vacuo after centrifugation. Ga(NO3)3 and flake silver powder.
The preparation steps are simplified, production time is significantly shortened, energy consumption and pollution emissions are reduced, and the production of high-purity gallium nitrate and high-quality sheet silver powder is achieved, meeting the needs of the high-tech field.
Smart Images

Figure HDA0004992147800000011 
Figure HDA0004992147800000012 
Figure HDA0004992147800000021
Abstract
Description
Technical Field
[0001] The invention relates to a one-step method for preparing gallium nitrate and flaky silver powder, belonging to the technical field of materials. Background Art
[0002] Gallium nitrate is a key raw material for the preparation of high-purity gallium oxide and is of great significance to the semiconductor industry. Moreover, in the field of biomedicine, gallium nitrate and its derivatives, such as gallic acid, show significant anti-tumor activity. In addition, in the field of energy, it is used as a conductive layer for the electrodes of solar panels, which can improve the conductivity and light absorption capacity, reduce energy loss, and improve conversion efficiency. At present, there are various preparation strategies for gallium nitrate, which can be summarized into three major pathways: through the reaction of gallium oxide with strong acids and bases, the solvation reaction of gallium and water, and the interaction of sponge gallium with strong acids and bases. However, although these methods can effectively synthesize gallium nitrate, they face significant challenges, especially the lengthy process of dissolving gallium oxide with concentrated nitric acid (which takes dozens of hours and is carried out under continuous heating and water replenishment conditions), which is not only inefficient and costly, but also accompanied by environmental problems such as nitric acid volatilization, posing a threat to the ecology.
[0003] As an important conductive material, flaky silver powder has shown wide application value in the fields of electronics and electrical industry, automobile industry, energy field, medical equipment, printing technology, etc. At present, most flaky silver powders are transformed from spherical or granular silver powders through complex ball milling process. This process not only requires inert gas protection to prevent oxidation, but also requires the use of lubricants and dispersants to finely control the particle size, accompanied by grading, polishing, modification and purification and other tedious processes. This series of high-precision operations not only relies on the support of high-end equipment, but also is accompanied by the extension of production cycle and significant increase in energy consumption and cost.
[0004] Therefore, the preparation of gallium nitrate and flaky silver powder in the prior art is very difficult. Summary of the invention
[0005] In view of the environmental pollution problems caused by strong acid and strong alkali in the traditional gallium nitrate preparation process, as well as the cumbersome and long cycle of flaky silver powder preparation process, the present invention proposes a one-step method for preparing gallium nitrate and flaky silver powder. The present invention utilizes the reduction characteristics of metal Ga to AgNO3, and directly generates high-purity Ga(NO3)3 and flaky Ag in the reaction between Ga and AgNO3 solution; that is, Ga that has been ultrasonically and surface-treated is added to the AgNO3 solution according to the molar ratio, and reacts at a preset temperature for 12 to 36 hours to obtain a suspension of Ga(NO3)3 and Ag; centrifugal separation is performed to obtain Ga(NO3)3 liquid and Ag solid; Ga(NO3)3 solution is evaporated and concentrated at a preset temperature and vacuum dried to obtain solid Ga(NO3)3, and Ag solid is vacuum dried to obtain flaky silver powder. This process not only simplifies the preparation steps and greatly shortens the production time, but also significantly reduces energy consumption, achieves zero pollution emissions in the production process, and shows extremely high environmental benefits and production efficiency.
[0006] A one-step method for preparing gallium nitrate and flaky silver powder, the specific steps are as follows:
[0007] (1) ultrasonically dispersing metal Ga in alcohol to obtain a metal Ga particle suspension with a particle size of 0.1 to 10 μm, and vacuum drying after standing to volatilize excess alcohol to obtain metal Ga particles;
[0008] (2) adding metal Ga particles to the AgNO3 solution, stirring and reacting at a temperature of 20 to 60°C for 12 to 36 hours to obtain a suspension of Ga(NO3)3 and Ag;
[0009] (3) The suspension of Ga(NO3)3 and Ag is centrifuged to obtain Ga(NO3)3 liquid and Ag solid; the Ag solid is vacuum dried to obtain flaky silver powder;
[0010] (4) The Ga(NO3)3 solution is evaporated and concentrated at a temperature of 40-60°C and vacuum dried to obtain solid Ga(NO3)3.
[0011] The temperature of the ultrasonic dispersion in step (1) is 30-40°C and the time is 0.5-2h; the vacuum drying temperature is 30-70°C.
[0012] The alcohol in step (1) is one or more of methanol, ethanol and isopropanol.
[0013] The concentration of the AgNO3 solution in step (2) is 0.1-2 mol / L, and the molar ratio of metal Ga to AgNO3 is 1:(3-5).
[0014] Preferably, the vacuum drying temperature in step (3) is 30-100°C.
[0015] Preferably, the evaporation concentration in step (4) is atmospheric pressure concentration or reduced pressure concentration, and the vacuum drying temperature is 30-60°C.
[0016] The mechanism of the one-step method for preparing gallium nitrate and flaky silver powder is as follows: by utilizing the strong reducing property of metal gallium (Ga) to silver (Ag), by precisely controlling the reaction conditions, metal gallium (Ga) and silver nitrate (AgNO3) solution are chemically reacted, and gallium acts as a reducing agent to effectively reduce silver ions (Ag + ) is reduced to metallic silver (Ag), and at the same time it is oxidized to gallium ions (Ga 3+ ), and finally directly generate gallium nitrate (Ga(NO3)3) and pure metallic silver (Ag) precipitate.
[0017] The beneficial effects of the present invention are:
[0018] (1) The present invention adopts a one-step reduction method to efficiently and directly prepare high-purity gallium nitrate (Ga(NO3)3) and high-quality flaky silver products. No other by-products are generated during the entire process, achieving 100% conversion efficiency from raw materials to products, greatly improving production purity and economic benefits;
[0019] (2) The reaction conditions of the present invention are mild, and no corrosive substances such as strong acids and strong bases need to be introduced throughout the process, nor does it require a complex high temperature and high pressure environment. The experimental steps are simple and clear, and the operation is convenient; it not only reduces production risks, but also significantly reduces environmental pollution, while ensuring an extremely high conversion rate;
[0020] (3) The gallium nitrate product prepared by the present invention has a purity of up to 99.9%, which meets the stringent requirements of high-tech fields such as semiconductors, optoelectronics and medicine for high-quality raw materials; at the same time, the average particle size of the prepared flaky silver powder is between 5 and 10 μm, which perfectly meets the specific requirements of many high-tech products for material morphology and performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a SEM image of the flaky silver powder prepared in Example 1;
[0022] Figure 2 is a SEM image of the flaky silver powder prepared in Example 2;
[0023] Figure 3 This is the SEM image of the flaky silver powder prepared in Example 3. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0025] Example 1: A one-step method for preparing gallium nitrate and flaky silver powder, the specific steps are as follows:
[0026] (1) adding 1 g of metal Ga to ethanol, ultrasonically dispersing at 30° C. for 2 h to obtain a metal Ga particle suspension with a particle size of 0.5-2 μm, standing for 30 min, and vacuum drying at 40° C. to evaporate excess ethanol to obtain metal Ga particles;
[0027] (2) adding metal Ga particles to a 2 mol / L AgNO3 solution, stirring and reacting at 30°C for 24 h to obtain a suspension of Ga(NO3)3 and Ag; the molar ratio of the metal Ga to AgNO3 is 1:3;
[0028] (3) The suspension of Ga(NO3)3 and Ag is centrifuged to obtain Ga(NO3)3 liquid and Ag solid; the Ag solid is vacuum dried at a temperature of 60°C to obtain flaky silver powder;
[0029] (4) The Ga(NO3)3 solution was concentrated by evaporation at 60°C under normal pressure, and then vacuum dried at 40°C to obtain a solid Ga(NO3)3 product;
[0030] The SEM image of the flaky silver powder in this embodiment is shown in Figure 1 ,from Figure 1 It can be seen that the flaky silver powder with uniform particle size distribution was successfully obtained, and the average particle size of the flaky silver powder was about 8 to 10 μm;
[0031] The solid-state Ga(NO3)3 product of this embodiment is tested by an inductively coupled plasma spectrometer (ICP), and the purity of the solid-state Ga(NO3)3 product is as high as 99.98%.
[0032] Example 2: A one-step method for preparing gallium nitrate and flaky silver powder, the specific steps are as follows:
[0033] (1) adding 0.5 g of metal Ga to methanol, and ultrasonically dispersing the mixture for 1.0 h at 40° C. to obtain a metal Ga particle suspension having a particle size of 0.3 to 5 μm. After standing for 30 min, the mixture was vacuum dried at 40° C. to evaporate excess ethanol to obtain metal Ga particles;
[0034] (2) adding metal Ga particles to a 1.5 mol / L AgNO3 solution, stirring and reacting at 40°C for 24 h to obtain a suspension of Ga(NO3)3 and Ag; the molar ratio of the metal Ga to AgNO3 is 1:3.5;
[0035] (3) The suspension of Ga(NO3)3 and Ag is centrifuged to obtain Ga(NO3)3 liquid and Ag solid; the Ag solid is vacuum dried at a temperature of 80°C to obtain flaky silver powder;
[0036] (4) The Ga(NO3)3 solution was concentrated by evaporation at 50°C under normal pressure, and then vacuum dried at 40°C to obtain solid Ga(NO3)3;
[0037] The SEM image of the flaky silver powder in this embodiment is shown in Figure 2 ,from Figure 2 It can be seen that the particle size of the prepared flaky silver powder is basically the same, and the particle size of the flaky silver powder is 8-9 μm;
[0038] The solid-state Ga(NO3)3 product of this embodiment is tested by an inductively coupled plasma spectrometer (ICP), and the purity of the solid-state Ga(NO3)3 product is as high as 99.90%.
[0039] Example 3: A one-step method for preparing gallium nitrate and flaky silver powder, the specific steps are as follows:
[0040] (1) 1.0 g of metal Ga was added to isopropanol, and ultrasonic dispersion was performed at 35° C. for 1.5 h to obtain a metal Ga particle suspension with a particle size of 1 to 3 μm. After standing for 30 min, vacuum drying was performed at 40° C. to evaporate excess ethanol to obtain metal Ga particles;
[0041] (2) adding metal Ga particles to a 1.0 mol / L AgNO3 solution, stirring and reacting at 60°C for 24 h to obtain a suspension of Ga(NO3)3 and Ag; the molar ratio of the metal Ga to AgNO3 is 1:4;
[0042] (3) The suspension of Ga(NO3)3 and Ag is centrifuged to obtain Ga(NO3)3 liquid and Ag solid; the Ag solid is vacuum dried at a temperature of 90°C to obtain flaky silver powder;
[0043] (4) The Ga(NO3)3 solution is evaporated and concentrated at normal pressure at 40°C, and then vacuum dried at 40°C to obtain solid Ga(NO3)3;
[0044] The SEM image of the flaky silver powder in this embodiment is shown in Figure 3 ,from Figure 3 It can be seen that the particle size of the prepared flaky silver powder is relatively uniform, and the particle size of the flaky silver powder is about 5 to 8 μm;
[0045] According to the inductively coupled plasma spectrometer (ICP) test of the solid-state Ga(NO3)3 product of this embodiment, the purity of the solid-state Ga(NO3)3 product is as high as 99.84%.
[0046] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A one-step method for preparing gallium nitrate and flaky silver powder, characterized in that: The specific steps are as follows: (1) ultrasonically dispersing metal Ga in alcohol to obtain a metal Ga particle suspension with a particle size of 0.1 to 10 μm, and vacuum drying after standing to volatilize excess alcohol to obtain metal Ga particles; (2) adding metal Ga particles to the AgNO3 solution and reacting at a temperature of 20 to 60°C for 12 to 36 hours to obtain a suspension of Ga(NO3)3 and Ag; (3) The suspension of Ga(NO3)3 and Ag is centrifuged to obtain Ga(NO3)3 liquid and Ag solid; the Ag solid is vacuum dried to obtain flaky silver powder; (4) The Ga(NO3)3 solution is evaporated and concentrated at a temperature of 40-60°C and vacuum dried to obtain solid Ga(NO3)3.
2. The method for preparing gallium nitrate and flaky silver powder in one step according to claim 1, characterized in that: The temperature of ultrasonic dispersion in step (1) is 30-40°C and the time is 0.5-2h; the vacuum drying temperature is 30-70°C.
3. The method for preparing gallium nitrate and flaky silver powder in one step according to claim 1, characterized in that: In step (1), the alcohol is one or more of methanol, ethanol and isopropanol.
4. The method for preparing gallium nitrate and flaky silver powder in one step according to claim 1, characterized in that: Step (2) The concentration of the AgNO3 solution is 0.1-2 mol / L, and the molar ratio of metal Ga to AgNO3 is 1:(3-5).
5. The method for preparing gallium nitrate and flaky silver powder in one step according to claim 1, characterized in that: The vacuum drying temperature in step (3) is 30-100°C.
6. The method for preparing gallium nitrate and flaky silver powder in one step according to claim 1, characterized in that: The evaporation concentration in step (4) is concentration under normal pressure or under reduced pressure, and the vacuum drying temperature is 30 to 60°C.
Citation Information
Patent Citations
Liquid-phase synthesis method of room-temperature liquid metal core-shell composite material as well as product and application thereof
CN117505871A
How to select and recover valuable metals from OLED waste
KR1020180063474A