Biomass-modified hydrophobic electronic conductive polymer gel material as well as preparation method and application thereof

By combining hydrophobic deep eutectic liquids with biomass materials to construct hydrophobic networks, the polymerization reaction problem of deep eutectic liquids as conductive polymer solvents is solved, the reaction rate and material properties are improved, and the application of flexible electronic devices is expanded.

CN119019609AActive Publication Date: 2024-11-26SHAANXI UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411373283.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-26
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

In the prior art, when deep eutectic liquids are used as solvents for conductive polymers, the solvent system is too viscous, which makes the polymerization reaction difficult to carry out and results in a low reaction rate, thus affecting the material properties.

Method used

A hydrophobic deep eutectic liquid is combined with biomass materials, and the biomass materials are modified by an acid anhydride modifier. Conjugated monomers are introduced for in-situ interfacial oxidative polymerization to form a conductive polymer with a large conjugated system, thus constructing a hydrophobic network.

Benefits of technology

It increases the polymerization rate, improves the electrical and mechanical properties of the material, and expands the application areas of flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019609A_ABST
    Figure CN119019609A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of gel materials, and relates to a biomass modified hydrophobic electronic conductive polymer gel material as well as a preparation method and application thereof. The hydrophobic deep eutectic liquid biomass material is prepared from the following raw materials in parts by mass: a hydrophobic deep eutectic liquid biomass material, an anhydride modifier, a conjugated monomer, a hydrophobic monomer, a doping agent, an oxidizing agent, a buffer solution and a surfactant, the hydrophobic deep eutectic liquid is composed of a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor. A three-dimensional hydrophilic network of traditional gel is changed into a hydrophobic network, an in-situ polymerization mode is adopted to construct a conductive network, a biomass material is adopted for modification, the'insoluble and non-meltable 'characteristic of a conductive polymer is effectively improved, and the network is successfully applied to a hydrogel flexible base material. The limitation of traditional hydrogel in practical application is solved, a new material choice is provided for manufacturing of flexible electronic devices, and further development and application of the flexible electronic technology are expected to be promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gel materials, and in particular relates to a biomass-modified hydrophobic electronic conductive polymer gel material and a preparation method and application thereof. Background Art

[0002] In recent years, the rapid development of flexible electronic technology has promoted the application of flexible strain sensors. These sensors are lightweight, flexible and portable, which makes them show great potential in many cutting-edge fields. Flexible strain sensors not only have good biocompatibility and conductivity, but also improve waterproof performance through hydrophobic treatment, so that they can maintain stable working state under various environmental conditions.

[0003] With the continuous advancement of technology, this material is expected to play an important role in the development of smart materials and technologies in the future. Especially in electronic skin, medical monitoring, human-computer interaction and artificial intelligence. The core competitiveness of these sensors lies in their ability to accurately and sensitively detect and respond to mechanical deformations such as stretching, compression and bending, thereby achieving real-time monitoring of changes in the external environment. In order to achieve high-performance strain sensing functions, material scientists and engineers are constantly exploring various strategies to optimize the structure and performance of sensors.

[0004] Biomass materials refer to organic substances derived from nature, such as cellulose, chitosan, sodium alginate, etc. These materials have good biocompatibility and degradability, and are suitable for use in biomedicine and environmental protection fields.

[0005] Constructing and regulating the conductive network is one of the key steps to improve the performance of strain sensors. The conductive network not only determines the conductivity of the sensor, but also directly affects its sensitivity, response speed and stability. Conductive polymers are a class of organic polymer materials with conductivity. They are polymers with a three-dimensional network cross-linking structure inside. They can maintain the integrity of their structure in both air and water. They have widely adjustable physical and chemical properties. They have high conductivity, good mechanical properties and easy processing. They show great potential in the field of flexible electronics. However, using water as a solvent alone will bring about problems such as low-temperature freezing and water loss, causing the material to become dry and brittle, the conductive filler to be lost, and the mechanical properties to be poor, which will lead to the loss of electrical properties.

[0006] A possible solution to overcome these limitations is to replace water with deep eutectic liquid. At present, some literature uses functionalized hydrophilic deep eutectic liquid as monomer and introduces photoinitiator technology to polymerize to form gel. This improves the problem of poor mechanical properties, but at the same time there are problems such as the solvent system being too viscous to participate in the polymerization reaction and the low reaction rate. Summary of the invention

[0007] The purpose of the present invention is to provide a biomass-modified hydrophobic electronic conductive polymer gel material and a preparation method thereof, which solves the problem that the solvent system is too viscous to participate in the polymerization reaction and the reaction rate is low when using deep eutectic liquid instead of water as the solvent of the conductive polymer.

[0008] The present invention is achieved through the following technical solutions:

[0009] A biomass-modified hydrophobic electronic conductive polymer gel material, wherein the raw materials thereof include the following components by weight:

[0010] 8-10 parts of hydrophobic deep eutectic liquid, 2-4 parts of biomass material, 1-4 parts of anhydride modifier, 2-4 parts of conjugated monomer, 1-3 parts of hydrophobic monomer, 0.08-0.1 parts of dopant, 3-5 parts of oxidant, 20-30 parts of buffer solution and 20-30 parts of surfactant;

[0011] The hydrophobic deep eutectic liquid is composed of a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor in a molar ratio of 1:(2-4).

[0012] Further, the hydrophobic hydrogen bond donor is trioctylmethylammonium bromide, n-octyltrimethylammonium bromide, tetra-n-octylammonium bromide, octadecyltrimethylammonium bromide or dioctyldimethylammonium chloride;

[0013] The hydrophobic hydrogen bond acceptor is ethylparaben, methylparaben, diloxanide furoate or diethyl maleate.

[0014] Furthermore, the biomass material is one or more of heparin, maltodextrin, cassava starch, carboxymethyl chitosan, gelatin, gum arabic, konjac and hydroxypropyl deacetylated chitosan.

[0015] Furthermore, the anhydride modifier is angelic anhydride, NA-anhydride, crotonic anhydride, itaconic anhydride, maleic anhydride or 2,3-dimethylmaleic anhydride.

[0016] Further, the conjugated monomer is 1-(3-sulfopropyl)-2-vinylpyridine hydroxide inner salt, 3-(2-nitrovinyl)pyridine, 1-vinyl-3-butylimidazolium bromide or 1-vinyl-3-ethylimidazolium bromide;

[0017] The hydrophobic monomer is isooctyl acrylate, ethyl acrylate, octadecyl methacrylate or hydroxyethyl acrylate.

[0018] Further, the cross-linking agent is MBA;

[0019] The initiator is ammonium persulfate, potassium persulfate or BPO.

[0020] Further, the doping agent is tannic acid, p-toluenesulfonic acid, aminosulfonic acid, citric acid, lactic acid or formic acid;

[0021] The oxidant is peracetic acid, perchloric acid, hypochlorous acid, ammonium persulfate, potassium dichromate, hydrogen peroxide, potassium permanganate or ferric permanganate.

[0022] Further, the buffer solution is a Tris buffer solution, a phosphate buffer, a disodium hydrogen phosphate-sodium dihydrogen phosphate buffer or an imidazole-hydrochloride buffer;

[0023] The surfactant is dodecyl dimethyl betaine, carboxylate type imidazoline, sodium coconut sulfate, sodium lauryl sulfate or cocamidopropyl betaine.

[0024] The present invention also discloses a method for preparing a biomass-modified hydrophobic electronic conductive polymer gel material, comprising:

[0025] 1) mixing a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor in a molar ratio of 1:(2-4) and freeze-drying to obtain a hydrophobic deep eutectic liquid;

[0026] 2) dissolving 2-4 parts of biomass material in 20-30 parts of buffer solution, adjusting the pH to 6-8, and then dropping 3-5 parts of anhydride modifier, reacting at 0-5°C to obtain a modified biomass material;

[0027] 3) mixing the modified biomass material with 2-4 parts of a conjugated monomer and 0.08-0.1 parts of a dopant, adding 3-5 parts of an oxidant dropwise at a temperature of 0-3° C., centrifuging, washing, purifying, and freeze-drying after the reaction to obtain a conductive polymer modified by the biomass material;

[0028] 4) Add 8-10 parts of deep eutectic liquid to 20-30 parts of surfactant and disperse by ultrasonic dispersion, then add 1-3 parts of hydrophobic monomer, 0.08-0.1 parts of cross-linking agent and 2-4 parts of biomass material modified conductive polymer prepared in step 3), pass protective gas, add 0.1-0.3 parts of initiator dropwise, react at 65-80° C. for 30 minutes, and obtain the biomass-modified hydrophobic electronic conductive polymer gel material.

[0029] The invention also discloses the application of the biomass-modified hydrophobic electronic conductive polymer gel material in the preparation of a flexible sensor.

[0030] Compared with the prior art, the present invention has the following beneficial technical effects:

[0031] The present invention discloses a biomass-modified hydrophobic electronic conductive polymer gel material, and its raw materials include a hydrophobic deep eutectic liquid, a biomass material, an anhydride modifier, and the like. The hydrophobic deep eutectic liquid is to provide a hydrophobic environment for the subsequent polymerization reaction to inhibit the material from losing electrical properties due to water loss, so that each monomer undergoes polymerization reaction in the same phase, thereby increasing the reaction rate; the anhydride modifier can introduce a propylene structure into the structure of the biomass material to obtain a modified biomass material, and introduce a conductive polymer monomer into its structure, and then adopt in-situ interfacial oxidation polymerization to form a functionalized biomass material. A conductive polymer with a large conjugated system is formed by polymerizing conjugated monomers, and a dopant is used to dope it, thereby regulating the mechanical properties and improving its electrical properties; the present invention uses a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor to synthesize a hydrophobic deep eutectic liquid, which provides a powerful environment for the introduction of hydrophobic monomers, and then introduces hydrophobic monomers, thereby expanding the application field in information transmission.

[0032] In order to overcome the limitation of traditional gels that swell and absorb water, resulting in the leakage of conductive media, the present invention changes the three-dimensional hydrophilic network of traditional gels into a hydrophobic network. The conductive network is constructed by in-situ polymerization, and modified by biomass materials to effectively improve the "insoluble and infusible" characteristics of the conductive polymer, and this network is successfully applied to hydrogel flexible substrates. The development of biomass-modified hydrophobic conductive polymer coating electronic gel materials not only solves the limitations of traditional hydrogels in practical applications, but also provides new material options for the manufacture of flexible electronic devices, which is expected to promote the further development and application of flexible electronic technology.

[0033] Furthermore, the hydrogen bond acceptor used by the hydrophobic deep eutectic liquid is an organic salt skeleton, which can further form a quaternary ammonium salt structure to coordinately improve the electrical properties.

[0034] The invention provides a preparation method of a biomass-modified hydrophobic electronic conductive polymer gel material, which comprises the following steps: firstly, introducing a hydrophobic deep eutectic liquid to provide a hydrophobic environment for a subsequent polymerization reaction, inhibiting the material from losing electrical properties due to water loss, so that each monomer undergoes a polymerization reaction in the same phase, and improving the reaction rate; mixing an anhydride modifier with the biomass material, introducing a double bond, and obtaining a modified biomass material; mixing the modified biomass material, a conjugated monomer, a dopant, and an oxidant, polymerizing the conjugated monomer to form a conductive polymer with a large conjugated system, adopting an anhydride modifier to structurally graft conductive polymer monomers onto the biomass material, and then adopting in-situ interfacial oxidation polymerization to obtain a conductive polymer modified by the biomass material; finally, introducing the conductive polymer modified by the biomass material into a deep eutectic liquid system, and grafting the functionalized biomass material into a hydrophobic monomer molecular chain by a free radical polymerization method, and forming a long-range ordered conductive material.

[0035] The present invention directly modifies the functional groups (amino groups, hydroxyl groups) on the biomass material by acid anhydride to obtain the modified biomass material; the modified biomass material is grafted with a conductive polymer material, and the conductive polymer modified by the biomass material is further synthesized by an in-situ chemical oxidation polymerization method. The free radical polymerized matrix gel material is combined with the conductive polymer modified by the biomass material to create a new type of flexible conductive composite material. This material not only retains the soft properties of the hydrogel, but also introduces the electrical properties of the conductive medium, which makes it show significant advantages in the development of flexible electronic devices.

[0036] The present invention introduces conductive polymers, which can effectively improve both electrical properties and mechanical properties. Secondly, by combining conductive polymers with biomass materials to form a double network structure, a new composite material with unique properties can be created. This structure can provide a larger contact area, thereby having a dual regulatory effect on electrical and mechanical properties. By combining the double network structure of conductive polymers and biomass materials, this product can not only improve the electrical and mechanical properties of the material, but also broaden its application in multiple fields such as flexible electronics, smart packaging, and biomedicine. This innovative composite material is expected to become an important component of future smart materials and technologies. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a result diagram of mechanical property testing of the product prepared in the embodiment of the present invention;

[0038] Figure 2 This is a graph showing the results of conducting the electrical conductivity test of the product prepared in the embodiment of the present invention. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clear, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments.

[0040] The detailed description of the embodiments of the present invention provided in the following drawings is not intended to limit the scope of the invention claimed for protection, but merely represents a selected embodiment of the present invention. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0041] It should be noted that the terms "comprises", "includes" or any other variations are intended to cover non-exclusive inclusion, so that a process, element, method, article or equipment that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to the process, element, method, article or equipment.

[0042] The present invention discloses a method for preparing a biomass-modified hydrophobic electronic conductive polymer gel material, comprising the following steps:

[0043] 1) mixing a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor in a molar ratio of 1:(2-4) and freeze-drying to obtain a hydrophobic deep eutectic liquid;

[0044] 2) dissolving 2-4 parts of biomass material in 20-30 parts of buffer solution, adjusting the pH to 6-8, and then dropping 3-5 parts of anhydride modifier, reacting at 0-5°C to obtain a modified biomass material;

[0045] 3) mixing the modified biomass material with 2-4 parts of a conjugated monomer and 0.08-0.1 parts of a dopant, adding 3-5 parts of an oxidant dropwise at a temperature of 0-3° C., centrifuging, washing, purifying, and freeze-drying after the reaction to obtain a conductive polymer modified by the biomass material;

[0046] 4) Add 8-10 parts of deep eutectic liquid to 20-30 parts of surfactant and disperse by ultrasonic dispersion, then add 1-3 parts of hydrophobic monomer, 0.08-0.1 parts of cross-linking agent and 2-4 parts of biomass material modified conductive polymer prepared in step 3), pass protective gas, add dropwise 0.1-0.3 parts of initiator, react at 65-80° C. for 30 minutes, and obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0047] The features and performances of the present invention are further described in detail below in conjunction with the embodiments.

[0048] Example 1

[0049] 1) Preparation of deep eutectic liquid: n-octyltrimethylammonium bromide and diethyl maleate in a molar ratio of 1:2 were reacted at 80° C. for 2 h under reflux, and freeze-dried to obtain a deep eutectic liquid for use;

[0050] 2) Dissolve 2 parts of hydrophilic heparin in Tris buffer solution, adjust the pH to 8, then dropwise add 3 parts of NA-anhydride, and react at 0-5°C for 3 hours to obtain methallylated heparin;

[0051] 3) Add 2 parts of angelic anhydride and 0.08 parts of tannic acid to the methallylated heparin, add 3 parts of peracetic acid dropwise at a temperature of 0-3°C, react at low temperature for 24 hours, centrifuge, wash with ethanol, purify, and freeze-dry to obtain a biomass material-modified conductive polymer;

[0052] 4) 8-10 parts of the deep eutectic liquid prepared in step 1) were added to 20 parts of 1% carboxylic acid imidazoline solution and ultrasonically dispersed for 30 minutes, and then 3 parts of isooctyl acrylate, 0.08 parts of MBA and 2 parts of the product of step 3) were added thereto at 60°C and heated by N 2 1h, 0.1 parts of APS were added dropwise, and the mixture was reacted at 70°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0053] N 2 The main function of is to remove oxygen and eliminate the interference of oxygen, so that it can further undergo cross-linking reaction.

[0054] Example 2

[0055] 1) Preparation of deep eutectic liquid: n-octyltrimethylammonium bromide and diethyl maleate in a molar ratio of 1:4 were reacted at 80° C. under reflux for 2 h, and freeze-dried to obtain a deep eutectic liquid for use;

[0056] 2) dissolving 2-4 parts of maltodextrin and gum arabic in a mass ratio of 1:1 in a phosphate buffer solution, adjusting the pH to 8, and then adding 4 parts of itaconic anhydride dropwise, reacting at 0-5° C. for three hours to obtain a methacrylated biomass material;

[0057] 3) adding 4 parts of 3-(2-nitrovinyl)pyridine and 0.08 parts of citric acid to the methacrylated biomass material in step 2), adding 5 parts of potassium dichromate dropwise at a temperature of 0-3° C. and reacting for 24 hours, centrifuging, washing with ethanol, purifying, and freeze-drying to obtain a biomass material-modified conductive polymer;

[0058] 4) 9 parts of deep eutectic liquid prepared in step 1) were added to 20 parts of 1% cocamidopropyl betaine and ultrasonically dispersed for 30 minutes, and then 1 part of ethyl acrylate, 0.09 parts of MBA and 2 parts of the product of step 3) were added thereto and heated at 60°C with N 2 1h, 0.2 parts of BPO were added dropwise, and the mixture was reacted at 90°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0059] Example 3

[0060] 1) Preparation of deep eutectic liquid: tetra-n-octylammonium bromide and triloxanide furoate in a molar ratio of 1:2 were reacted at 80° C. for 2 h under reflux, and freeze-dried to obtain a deep eutectic liquid for use;

[0061] 2) dissolving 2 parts of konjac and carboxymethyl chitosan in a mass ratio of 2:1 in a disodium hydrogen phosphate-sodium dihydrogen phosphate buffer solution, adjusting the pH to 8, and then dropping 3 parts of maleic acid glycosides, reacting at 0-5° C. for 3 hours to obtain a methacrylated biomass material;

[0062] 3) adding 3 parts of 1-vinyl-3-butylimidazolium bromide and 0.1 parts of aminosulfonic acid to the methacrylated biomass material obtained in step 2), adding 3 parts of hydrogen peroxide dropwise at a temperature of 0-3° C. to react at low temperature for 24 hours, centrifuging, washing with ethanol, purifying, and freeze-drying to obtain a biomass material-modified conductive polymer;

[0063] 4) 9 parts of the deep eutectic liquid obtained in step 1) were added to 20 parts of 1% dodecyl dimethyl betaine by mass and ultrasonically dispersed for 30 minutes, and then 1 part of octadecyl methacrylate, 0.09 parts of MBA and 2 parts of the product of step 3) were added thereto at 60°C and heated by N 2 1h, 0.3 parts of KPS was added dropwise, and the mixture was reacted at 70°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0064] Example 4

[0065] 1) Preparation of deep eutectic liquid: Octadecyltrimethylammonium bromide and diethyl maleate in a molar ratio of 1:2 were reacted at 80° C. under reflux for 2 h, and freeze-dried to obtain a deep eutectic liquid for use;

[0066] 2) dissolving 4 parts of gelatin in an imidazole-hydrochloride buffer solution, adjusting the pH to 6, and then adding 4 parts of 2,3-dimethylmaleic anhydride dropwise, reacting at 0-5° C. for three hours to obtain a methacrylated biomass material;

[0067] 3) adding 3 parts of 1-(3-sulfopropyl)-2-vinylpyridine hydroxide inner salt and 0.08 parts of p-toluenesulfonic acid to the methacrylated biomass material obtained in step 2), adding 3-5 parts of ferric permanganate dropwise at 0-3° C. to react at low temperature for 24 hours, centrifuging, washing with ethanol, purifying, and freeze-drying to obtain a biomass material-modified conductive polymer;

[0068] 4) Add 9 parts of the solution prepared in step 1) to 30 parts of sodium lauryl sulfate with a mass fraction of 1% and disperse for 30 minutes under deep ultrasonication, then add 2 parts of hydroxyethyl acrylate, 0.1 parts of MBA and 2 parts of the product of step 3) at 60°C and pass N 2 1h, 0.2 parts of BPO were added dropwise, and the mixture was reacted at 90°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0069] Example 5

[0070] 1) Preparation of deep eutectic liquid: octadecyltrimethylammonium bromide and gold paraben in a molar ratio of 1:3 were reacted at 80° C. for 2 h under reflux, and freeze-dried to obtain a deep eutectic liquid for use;

[0071] 2) dissolving 3 parts of heparin and konjac in a mass ratio of 1:2 in a phosphate buffer solution, adjusting the pH to 8, and then dropping 3 parts of crotonic anhydride, reacting at 0-5° C. for 3 hours to obtain a methacrylated biomass material;

[0072] 3) adding 3 parts of 1-vinyl-3-butylimidazolium bromide and 0.08-0.1 parts of lactic acid to the methacrylated biomass material obtained in step 2), adding 3 parts of hydrogen peroxide dropwise at 0-3° C. to react at low temperature for 24 hours, centrifuging, washing with ethanol, purifying, and freeze-drying to obtain a biomass material-modified conductive polymer;

[0073] 4) 10 parts of the deep eutectic liquid prepared in step 1) were added to 30 parts of 1% dodecyl dimethyl betaine by mass fraction and ultrasonically dispersed for 30 minutes, and then 2 parts of isooctyl acrylate, 0.008 parts of MBA and 2 parts of the product of step 3) were added thereto and heated at 60°C with N 2 1h, 0.2 parts of KPS were added dropwise, and the mixture was reacted at 70°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0074] Example 6

[0075] 1) Preparation of deep eutectic liquid: dioctyldimethylammonium chloride and diethyl maleate in a molar ratio of 1:2 were reacted at 80° C. for 2 h under reflux, and freeze-dried to obtain a deep eutectic liquid for use;

[0076] 2) dissolving 4 parts of konjac in a Tris buffer solution, adjusting the pH to 8, and then dropping 3 parts of NA-anhydride, reacting at 0-5° C. for 3 hours to obtain a methacrylated biomass material;

[0077] 3) adding 3 parts of 1-vinyl-3-ethylimidazolium bromide and 0.1 parts of citric acid to the methacrylated biomass material obtained in step 2), adding 3 parts of perchloric acid dropwise at a temperature of 0-3° C. to react at low temperature for 24 hours, centrifuging, washing with ethanol, purifying, and freeze-drying to obtain a biomass material-modified conductive polymer;

[0078] 4) 8-10 parts of the deep eutectic liquid prepared in step 1) were added to 20 parts of 1% sodium coconut sulfate by mass and ultrasonically dispersed for 30 minutes, and then 3 parts of octadecyl methacrylate, 0.008 parts of MBA and 2 parts of the product of step 3) were added thereto at 60°C and heated by N 2 1h, 0.3 parts of APS were added dropwise, and the mixture was reacted at 70°C for 30min to obtain a biomass-modified hydrophobic electronic conductive polymer gel material.

[0079] The mechanical properties of the above embodiments were tested, and the test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the six solutions in the embodiments all have excellent mechanical properties, among which embodiment 1 is the best embodiment.

[0080] The electrical performance of Examples 1-6 was tested, and the test results were as shown in the figure. Figure 2 As shown. It can be seen that the biomass modified hydrophobic electronic conductive polymer gel material has excellent electrical properties.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A biomass-modified hydrophobic electronic conductive polymer gel material, characterized in that: The raw materials include the following components by mass: 8-10 parts of hydrophobic deep eutectic liquid, 2-4 parts of biomass material, 1-4 parts of anhydride modifier, 2-4 parts of conjugated monomer, 1-3 parts of hydrophobic monomer, 0.08-0.1 parts of dopant, 3-5 parts of oxidant, 20-30 parts of buffer solution and 20-30 parts of surfactant; The hydrophobic deep eutectic liquid is composed of a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor in a molar ratio of 1:(2-4).

2. The biomass-modified hydrophobic electronic conductive polymer gel material according to claim 1, characterized in that: The hydrophobic hydrogen bond donor is trioctylmethylammonium bromide, n-octyltrimethylammonium bromide, tetra-n-octylammonium bromide, octadecyltrimethylammonium bromide or dioctyldimethylammonium chloride; The hydrophobic hydrogen bond acceptor is ethylparaben, methylparaben, diloxanide furoate or diethyl maleate.

3. The biomass-modified hydrophobic electronic conductive polymer gel material according to claim 1, characterized in that: The biomass material is one or more of heparin, maltodextrin, cassava starch, carboxymethyl chitosan, gelatin, gum arabic, konjac and hydroxypropyl deacetylated chitosan.

4. The biomass-modified hydrophobic electronic conductive polymer gel material according to claim 1, characterized in that: The acid anhydride modifier is angelic anhydride, NA-anhydride, crotonic anhydride, itaconic anhydride, maleic anhydride or 2,3-dimethylmaleic anhydride.

5. The biomass-modified hydrophobic electronic conductive polymer gel material according to claim 1, characterized in that: The conjugated monomer is 1-(3-sulfopropyl)-2-vinylpyridine hydroxide inner salt, 3-(2-nitrovinyl)pyridine, 1-vinyl-3-butylimidazolium bromide or 1-vinyl-3-ethylimidazolium bromide; The hydrophobic monomer is isooctyl acrylate, ethyl acrylate, octadecyl methacrylate or hydroxyethyl acrylate.

6. The biomass-modified hydrophobic electronically conductive polymer gel material according to claim 1, characterized in that: The cross-linking agent is MBA; The initiator is ammonium persulfate, potassium persulfate or BPO.

7. The biomass-modified hydrophobic electronically conductive polymer gel material according to claim 1, characterized in that: The doping agent is tannic acid, p-toluenesulfonic acid, aminosulfonic acid, citric acid, lactic acid or formic acid; The oxidant is peracetic acid, perchloric acid, hypochlorous acid, ammonium persulfate, potassium dichromate, hydrogen peroxide, potassium permanganate or ferric permanganate.

8. The biomass-modified hydrophobic electronically conductive polymer gel material according to claim 1, characterized in that: The buffer solution is a Tris buffer solution, a phosphate buffer, a disodium hydrogen phosphate-sodium dihydrogen phosphate buffer or an imidazole-hydrochloride buffer; The surfactant is dodecyl dimethyl betaine, carboxylate type imidazoline, sodium coconut sulfate, sodium lauryl sulfate or cocamidopropyl betaine.

9. A method for preparing a biomass-modified hydrophobic electronically conductive polymer gel material, characterized in that: include: 1) mixing a hydrophobic hydrogen bond donor and a hydrophobic hydrogen bond acceptor in a molar ratio of 1:(2-4) and freeze-drying to obtain a hydrophobic deep eutectic liquid; 2) dissolving 2-4 parts of biomass material in 20-30 parts of buffer solution, adjusting the pH to 6-8, and then dropping 3-5 parts of anhydride modifier, reacting at 0-5°C to obtain a modified biomass material; 3) mixing the modified biomass material with 2-4 parts of a conjugated monomer and 0.08-0.1 parts of a dopant, adding 3-5 parts of an oxidant dropwise at a temperature of 0-3° C., centrifuging, washing, purifying, and freeze-drying after the reaction to obtain a conductive polymer modified by the biomass material; 4) Add 8-10 parts of deep eutectic liquid to 20-30 parts of surfactant and disperse by ultrasonic dispersion, then add 1-3 parts of hydrophobic monomer, 0.08-0.1 parts of cross-linking agent and 2-4 parts of biomass material modified conductive polymer prepared in step 3), pass protective gas, add 0.1-0.3 parts of initiator dropwise, react at 65-80° C. for 30 minutes, and obtain the biomass-modified hydrophobic electronic conductive polymer gel material.

10. Use of the biomass-modified hydrophobic electronically conductive polymer gel material according to any one of claims 1 to 8 in the preparation of a flexible sensor.

Citation Information

Patent Citations

  • Dynamic polymer with hybrid cross-linking network

    CN109666160A

  • Preparation method of eutectic gel with adjustable mechanical properties

    CN117487059A

  • Self-repairing ionic conductive information storage gel as well as preparation method and application thereof

    CN117534793A