Organosilicon epoxy curing agent as well as preparation method and application thereof

Catalyst-free dropping reaction was performed by using a mixture of 1,3-cyclohexadimethylamine, polyetheramine D230, KH550 and disiloxane epoxy double-capsule and alkyl glycidyl ether AGE in epoxy resin coating. The problem of insufficient weather resistance and bonding performance of traditional epoxy resin coatings is solved, and efficient and low-cost silicone epoxy curing agent preparation is achieved, which improves the coating's weather resistance, acid resistance and salt spray resistance.

CN119019648APending Publication Date: 2024-11-26ANHUI ADVANCED BUILDING MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115681.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional epoxy resin coatings have shortcomings in their weathering resistance and adhesive properties. In addition, the existing silicone hydrosilicon preparation of silicone epoxy curing agents requires precious metal catalysts, which is complex and costly.

Method used

The reaction was carried out using a mixture of 1,3-cyclohexylamine, polyetheramine D230, KH550 and disiloxane epoxy double-capsule and alkyl glycidyl ether AGE. Without catalyst, silicone epoxy was prepared by dropping addition. Curing agent improves the coating's weather resistance, acid resistance and salt spray resistance.

Benefits of technology

The preparation of silicone epoxy curing agent with simple operation and low cost is realized, which improves the adhesion, toughness and weather resistance of the coating and improves the adhesiveness with the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993554360000021
    Figure BDA0004993554360000021
  • Figure BDA0004993554360000022
    Figure BDA0004993554360000022
  • Figure BDA0004993554360000041
    Figure BDA0004993554360000041
Patent Text Reader

Abstract

The invention relates to an organic silicon epoxy curing agent as well as a preparation method and application thereof, and belongs to the technical field of heavy anti-corrosion coatings. The organic silicon epoxy curing agent is prepared from the following components in parts by weight: 42 to 77 parts of 1, 3-cyclohexanedimethylamine; 10 to 15 parts of polyether amine D230; 1 to 3 parts of KH550; 55 to 83 parts of amino-terminated siloxane; 22 to 30 parts of an amino-terminated long-chain epoxy-amine adduct; the preparation method comprises the following steps: mixing and stirring 1, 3-cyclohexanedimethylamine, polyether amine D230 and KH550 at room temperature for 20 to 30 minutes, so as to obtain a base material; the preparation method comprises the following steps: mixing and stirring disiloxane epoxy double end sockets and alkyl glycidyl ether AGE for 20-30 minutes to obtain a dripping material; and heating the obtained base material to a temperature, stirring under the protection of nitrogen, dropwise adding the dropwise adding material into the base material, preserving heat after dropwise adding is finished, and then cooling to room temperature to obtain the organic silicon epoxy curing agent. The organic silicon epoxy curing agent is combined with epoxy resin color paste, a coating has a good anti-corrosion effect, and the method is simple in operation process, low in cost and high in production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heavy-duty anticorrosive coatings, and in particular to an organosilicon epoxy curing agent and a preparation method and application thereof. Background Art

[0002] Corrosion is mainly the deterioration of metal or non-metal and its contact with the environment after chemical dielectric reaction. In Asia alone, anti-corrosion is an industry with an annual value of trillions of dollars. Anti-corrosion coatings are generally divided into primer and topcoat coatings, with primer applied first and topcoat applied later.

[0003] Traditional primer coatings are mostly epoxy resins, which have strong adhesion to the substrate. However, epoxy resin coatings are prone to breakage due to unsaturated benzene ring bonds, resulting in poor weathering resistance and yellowing. Coatings with good weathering resistance are mostly polysiloxanes and fluorocarbons with weak molecular polarity, but their adhesion to the substrate is also poor.

[0004] How to improve the weather resistance of epoxy resin coatings is a common problem encountered by technical personnel in the industry. At present, the industry generally introduces siloxane into the curing agent, and the siloxane curing agent is combined with the resin to form a silicone epoxy modified coating with strong weather resistance and adhesion performance, but most of them use cartel catalysts for hydrosilylation to prepare silicone epoxy curing agents. The prior art discloses a preparation method of a polyamino silicone epoxy curing agent, an epoxy anticorrosive protective paint using the curing agent, and a preparation method thereof. The silicone epoxy curing agent is prepared by hydrosilylation reaction, which requires the participation of a precious metal catalyst, and the preparation process is complicated and the cost is high. Summary of the invention

[0005] In view of this, the main purpose of the present invention is to provide an organosilicon epoxy curing agent and a preparation method and application thereof. The technical problem to be solved is to use a mixture of 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550 as a base material, and drop a mixture of disiloxane epoxy double heads and alkyl glycidyl ether AGE into the base material, and complete the reaction between the main component molecules without the participation of a catalyst, so that the prepared organosilicon epoxy curing agent has excellent weather resistance, acid resistance and salt spray resistance.

[0006] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical scheme. The present invention proposes an organosilicon epoxy curing agent, which comprises the following components by weight:

[0007] 42-77 parts of 1,3-cyclohexanedimethylamine; 10-15 parts of polyetheramine D230; 1-3 parts of KH550; 55-83 parts of amino-terminated siloxane; 22-30 parts of amino-terminated long-chain epoxy-amine adduct.

[0008] The purpose of the present invention and the technical problems to be solved can be further achieved by adopting the following technical measures.

[0009] Preferably, in the aforementioned organosilicon epoxy curing agent, the general formula of the amino-terminated siloxane is as follows:

[0010]

[0011] Preferably, in the aforementioned organosilicon epoxy curing agent, the general formula of the amino-terminated long-chain epoxy-amine adduct is as follows:

[0012]

[0013] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. A method for preparing an organosilicon epoxy curing agent proposed by the present invention comprises the following steps:

[0014] 1) Mix 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550 and stir at room temperature for 20-30 minutes to obtain a base material;

[0015] 2) mixing disiloxane epoxy double end cap and alkyl glycidyl ether AGE for 20-30 minutes to obtain a dropwise addition material;

[0016] 3) The base material obtained in step 1) is heated to a certain temperature, stirred under nitrogen protection, and the dropwise material is added dropwise to the base material. After the dropwise addition is completed, the temperature is kept, and then cooled to room temperature to obtain an organosilicon epoxy curing agent.

[0017] The purpose of the present invention and the technical problems to be solved can be further achieved by adopting the following technical measures.

[0018] Preferably, in the preparation method of the aforementioned organosilicon epoxy curing agent, in step 1), the mass ratio of the polyetheramine D230 to 1,3-cyclohexanedimethylamine is 10% to 15%, and the mass ratio of the polyetheramine KH550 to 1,3-cyclohexanedimethylamine is 1% to 3%.

[0019] Preferably, in the above-mentioned method for preparing the organosilicon epoxy curing agent, in step 2), the mass percentage of the alkyl glycidyl ether AGE to the 1,3-cyclohexanedimethylamine in step 1) is 15% to 20%.

[0020] Preferably, in the aforementioned method for preparing the organosilicon epoxy curing agent, in step 2), the mass percentage of the disiloxane epoxy double head to the 1,3-cyclohexanedimethylamine in step 1) is 40% to 60%.

[0021] Preferably, in the aforementioned method for preparing an organosilicon epoxy curing agent, in step 2), the alkyl glycidyl ether AGE is selected from at least one of C12 to C14 alkyl glycidyl ethers.

[0022] Preferably, in the aforementioned method for preparing an organosilicon epoxy curing agent, in step 2), the disiloxane epoxy double-capped functional group R is selected from one of a methyl group and a cycloalkane group.

[0023] Preferably, in the aforementioned method for preparing the organosilicon epoxy curing agent, in step 3), the heating temperature is 70-80°C; the rotation speed is 1000-1200 r / min; the dropping time is 2-3 h, and the dropping acceleration rate is 0.4-0.7 g / min.

[0024] The purpose of the present invention and the technical problem solved are achieved by adopting the following technical scheme. The present invention proposes an organosilicon epoxy coating, which comprises an epoxy resin color paste and an organosilicon epoxy curing agent in a mass ratio of (60-75):345; the organosilicon epoxy curing agent comprises the following components by weight: 42-77 parts of 1,3-cyclohexanedimethylamine; 10-15 parts of polyetheramine D230; 1-3 parts of KH550; 55-83 parts of amino-terminated siloxane; and 22-30 parts of amino-terminated long-chain epoxy-amine adduct.

[0025] Compared with the prior art, the organosilicon epoxy curing agent and its preparation method and application described in the present invention have the following beneficial effects:

[0026] The present invention uses a mixture of 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550 as a base material, and drips a mixture of disiloxane epoxy double head and alkyl glycidyl ether AGE into the base material to obtain an organosilicon epoxy curing agent. The reaction between the main component molecules can be completed without the participation of a catalyst, and the operation is simple and the preparation cost is low. The addition of KH550 can improve the adhesion between the coating and the substrate, the long chain of the alkyl glycidyl ether AGE improves the toughness of the coating, and the introduction of disiloxane improves the weather resistance, acid resistance and salt spray resistance of the coating.

[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION

[0028] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description of an organosilicon epoxy curing agent and its preparation method and application according to the present invention, its specific implementation, structure, characteristics and effects in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0029] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the usual meanings understood by ordinary technicians in the field to which the present invention belongs. If no specific experimental steps or conditions are specified below, the operations or conditions of the conventional experimental steps described in the literature in the field can be followed.

[0030] Some embodiments of the present invention provide a silicone epoxy curing agent, comprising the following components in parts by weight:

[0031] 42-77 parts of 1,3-cyclohexanedimethylamine; 10-15 parts of polyetheramine D230; 1-3 parts of KH550; 55-83 parts of amino-terminated siloxane; 22-30 parts of amino-terminated long-chain epoxy-amine adduct.

[0032] In some embodiments, optionally, the general formula of the amino-terminated siloxane is as follows:

[0033]

[0034] In some embodiments, optionally, the general formula of the amino-terminated long-chain epoxy-amine adduct is as follows:

[0035]

[0036] Specifically, the main component of the organosilicon epoxy curing agent is the reaction product of 1,3-cyclohexanedimethylamine, disiloxane epoxy double head and alkyl glycidyl ether AGE, and the general reaction formula is as follows:

[0037]

[0038] The organosilicon epoxy curing agent of the present invention is a mixture of the above main component reaction compound and 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550.

[0039] Some embodiments of the present invention also provide a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0040] 1) Mix 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550 and stir at room temperature for 20-30 minutes to obtain a base material;

[0041] 2) mixing disiloxane epoxy double end cap and alkyl glycidyl ether AGE for 20-30 minutes to obtain a dropwise addition material;

[0042] 3) heating the base material obtained in step 1), stirring under nitrogen protection, and slowly dropping the drop material into the base material, the dropping time is not less than 2h, and the dropping rate is preferably 0.5-0.6g / min. If the time is less than 2h or the rate is greater than 0.6g / min, the drop is added too fast and agglomeration is easy. If the rate is less than 0.5g / min, the time cost is increased. After the drop is completed, in order to ensure that the residue reacts fully, keep warm for not less than 1 hour, and then cool to room temperature to obtain the silicone epoxy curing agent.

[0043] In some embodiments, optionally, in step 1), the polyetheramine D230 is used to adjust the curing time of the coating, and KH550 is used to improve the adhesion between the coating and the substrate. The mass ratio of polyetheramine D230 to 1,3-cyclohexanedimethylamine is 10% to 15%. When it is greater than 15%, the content of polyetheramine D230 is too high, which affects the surface drying time of the coating; the mass ratio of KH550 to 1,3-cyclohexanedimethylamine is 1% to 3%. When it is less than 1%, the amount of KH550 added is too low and the adhesion performance is not high; when the content is higher than 3%, the coating foams more and also affects the surface drying time.

[0044] In some embodiments, optionally, in step 2), the alkyl glycidyl ether AGE is an active diluent of the silicone epoxy curing agent, which plays a role of long-chain filling; the mass percentage of the alkyl glycidyl ether AGE to the 1,3-cyclohexanedimethylamine in step (1) is 15% to 20%. If it is less than 15%, the amount of AGE added is too low to affect the flexibility of the coating; if it is more than 20%, the amount of AGE added is too high to affect the strength.

[0045] In some embodiments, optionally, in step 2), the mass percentage of the disiloxane epoxy double head to the 1,3-cyclohexanedimethylamine in step (1) is 40% to 60%. When the mass percentage is lower than 40%, the amount of disiloxane epoxy double head added is too low and the anti-aging effect cannot be exerted; when the mass percentage is higher than 60%, the added amount is too high and the viscosity of the synthesized curing agent is too high, which affects the construction.

[0046] In some embodiments, optionally, in step 2), considering the convenience of purchase, the alkyl glycidyl ether AGE is selected from at least one of C12 to C14 alkyl glycidyl ethers purchased from the market.

[0047] In some embodiments, optionally, in step 2), the disiloxane epoxy double-headed functional group R is selected from one of a methyl group and a cycloalkane group, and the methyl group and the cycloalkane group are saturated bonds, which are stable and not easy to break, thereby improving the weather resistance of the coating.

[0048] In some embodiments, optionally, in step 3), the heating temperature is 70-80°C; if it is lower than 70°C, the temperature is too low, affecting the reaction rate and the reaction time is longer; if it is higher than 80°C, the temperature is too high, the reaction rate is high, and it is easy to agglomerate; the rotation speed is 1000-1200r / min, when it is lower than 1000r / min, the rotation speed is too low and it is easy to agglomerate, and when it is higher than 1200r / min, it is easy to splash; the dripping time is 2-3h; if the dripping time is less than 2h, the dripping is too fast and it is easy to agglomerate; if the dripping time is greater than 3h, the production efficiency is too low.

[0049] Some embodiments of the present invention also provide an organosilicon epoxy coating, which includes an epoxy resin color paste with a mass ratio of (60-75):345 and the above-mentioned organosilicon epoxy curing agent. The epoxy resin color paste can be composed of an epoxy resin, a filler and an auxiliary agent with a mass ratio of 300:210:18.4, wherein the resin can be E51, the filler can include TiO2, calcined kaolin and gas-phase SiO2 with a mass ratio of 10:2:9, and the auxiliary agent can include a leveling agent, a dispersant, a defoamer, an anti-settling agent and a light-oxidation stabilizer with a mass ratio of 2:3.6:2:4.8:6. The dispersant can be a dispersant BYK-P 104S, the defoamer can be a defoamer BYK-A530, the anti-settling agent can be an anti-settling agent BYK-410, the leveling agent can be a leveling agent BYK-333, and the light-oxidation stabilizer can be a light-oxidation stabilizer VX56.

[0050] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.

[0051] Example 1

[0052] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0053] (1) Mix 100g 1,3-cyclohexanedimethylamine, 10g polyetheramine D230 and 1g KH550 at room temperature and stir for 30min to prepare the base material;

[0054] (2) 40 g of disiloxane epoxy double end cap and 15 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0055] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of nitrogen with a purity of 99%. The drop material is slowly added dropwise to the base material at a drop rate of 0.45 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0056] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 1 below.

[0057] Table 1

[0058]

[0059] Example 2

[0060] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0061] (1) Mix 100g 1,3-cyclohexanedimethylamine, 10g polyetheramine D230 and 2g KH550 at room temperature and stir for 30min to prepare the base material;

[0062] (2) 45 g of disiloxane epoxy double end cap and 18 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0063] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of nitrogen with a purity of 99%. The drop material is slowly added dropwise to the base material at a drop rate of 0.5 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0064] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 2 below.

[0065] Table 2

[0066]

[0067] Example 3

[0068] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0069] (1) Mix 100g 1,3-cyclohexanedimethylamine, 12g polyetheramine D230 and 3g KH550 at room temperature and stir for 30min to prepare the base material;

[0070] (2) 50 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0071] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of nitrogen with a purity of 99%. The drop material is slowly added dropwise to the base material at a drop rate of 0.58 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0072] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 3 below.

[0073] Table 3

[0074]

[0075] Example 4

[0076] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0077] (1) Mix 100 g 1,3-cyclohexanedimethylamine, 12 g polyetheramine D230 and 2 g KH550 at room temperature and stir for 30 min to prepare the base material;

[0078] (2) 55 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0079] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added to the base material at a drop rate of 0.6 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0080] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 4 below.

[0081] Table 4

[0082]

[0083] Example 5

[0084] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0085] (1) 100 g 1,3-cyclohexanedimethylamine, 13 g polyetheramine D230, and 3 g KH550 were mixed and stirred at room temperature for 30 min to prepare the base material;

[0086] (2) 60 g of disiloxane epoxy double end cap and 18 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0087] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added dropwise to the base material at a drop rate of 0.65 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0088] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 5 below.

[0089] Table 5

[0090]

[0091]

[0092] Example 6

[0093] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0094] (1) 100 g 1,3-cyclohexanedimethylamine, 13 g polyetheramine D230, and 3 g KH550 were mixed and stirred at room temperature for 30 min to prepare the base material;

[0095] (2) 60 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0096] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added dropwise to the base material at a drop rate of 0.65 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0097] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 6 below.

[0098] Table 6

[0099]

[0100] Example 7

[0101] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0102] (1) 100 g 1,3-cyclohexanedimethylamine, 14 g polyetheramine D230, and 2 g KH550 were mixed and stirred at room temperature for 30 min to prepare the base material;

[0103] (2) 55 g of disiloxane epoxy double end cap and 18 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0104] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added to the base material at a drop rate of 0.6 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0105] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 7 below.

[0106] Table 7

[0107]

[0108] Example 8

[0109] This embodiment provides a method for preparing an organosilicon epoxy curing agent, comprising the following steps:

[0110] (1) Mix 100g 1,3-cyclohexanedimethylamine, 15g polyetheramine D230 and 3g KH550 at room temperature and stir for 30min to prepare the base material;

[0111] (2) 60 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0112] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of nitrogen with a purity of 99%. The drop material is slowly added dropwise to the base material at a drop rate of 0.66 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain a silicone epoxy curing agent.

[0113] The composition and total active hydrogen equivalent weight (AHEW) of the silicone epoxy curing agent are shown in Table 8 below.

[0114] Table 8

[0115]

[0116] Comparative Example 1

[0117] The curing agent of this comparative example is pure 1,3-cyclohexanedimethylamine, and its active hydrogen equivalent weight (AHEW) is 35.6.

[0118] Comparative Example 2

[0119] The curing agent of this comparative example is a non-terminal aminosiloxane and an amino-terminated long-chain epoxy-amine adduct component, and its preparation method comprises the following steps:

[0120] 100 g of 1,3-cyclohexanedimethylamine, 13 g of polyetheramine D230, and 3 g of KH550 were mixed and stirred at room temperature for 30 min to obtain the composite curing agent, and its active hydrogen equivalent (AHEW) was 37.8.

[0121] Comparative Example 3

[0122] The curing agent of this comparative example is a terminal amino long-chain epoxy-amine adduct component, and its preparation method comprises the following steps:

[0123] (1) Mix 100g 1,3-cyclohexanedimethylamine, 10g polyetheramine D230 and 2g KH550 at room temperature and stir for 30min to prepare the base material;

[0124] (2) 45 g of disiloxane epoxy double end cap is added as a drop feed;

[0125] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of nitrogen with a purity of 99%. The drop material is slowly added dropwise to the base material at a drop rate of 0.37 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain the curing agent.

[0126] The composition and total active hydrogen equivalent (AHEW) of the epoxy curing agent are shown in Table 9 below.

[0127] Table 9

[0128]

[0129] Comparative Example 4

[0130] The curing agent of this comparative example is a terminal aminosiloxane component, and its preparation method comprises the following steps:

[0131] (1) Mix 100g 1,3-cyclohexanedimethylamine, 12g polyetheramine D230 and 3g KH550 at room temperature and stir for 30min to prepare the base material;

[0132] (2) 20 g of alkyl glycidyl ether AGE is added dropwise;

[0133] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added dropwise to the base material at a drop rate of 0.15 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain the epoxy curing agent.

[0134] The composition and total active hydrogen equivalent (AHEW) of the epoxy curing agent are shown in Table 10 below.

[0135] Table 10

[0136]

[0137] Comparative Example 5

[0138] The curing agent of this comparative example does not contain KH550 component, and its preparation method comprises the following steps:

[0139] (1) Mix 100 g of 1,3-cyclohexanedimethylamine and 12 g of polyetheramine D230 at room temperature and stir for 30 min to prepare the base material;

[0140] (2) 55 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0141] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added dropwise to the base material at a drop rate of 0.6 g / min. After the addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain the epoxy curing agent.

[0142] The composition and total active hydrogen equivalent (AHEW) of the epoxy curing agent are shown in Table 11 below.

[0143] Table 11

[0144]

[0145] Comparative Example 6

[0146] The curing agent of this comparative example does not contain D230 component, and its preparation method comprises the following steps:

[0147] (1) Mix 100g 1,3-cyclohexanedimethylamine and 3g KH550 at room temperature and stir for 30min to prepare the base material;

[0148] (2) 60 g of disiloxane epoxy double end cap and 20 g of alkyl glycidyl ether AGE were mixed and stirred for 30 min as a dropwise addition material;

[0149] (3) The base material is heated to 70° C. and stirred at a speed of 1000 r / min under the protection of 99% pure nitrogen. The drop material is slowly added dropwise to the base material at a drop rate of 0.65 g / min. After the dropwise addition is completed, the mixture is kept warm for 1 hour and then cooled to room temperature to obtain the epoxy curing agent.

[0150] The composition and total active hydrogen equivalent (AHEW) of the epoxy curing agent are shown in Table 12 below.

[0151] Table 12

[0152]

[0153] The curing agents of Examples 1-8 and Comparative Examples 1-6 of the present invention were fully mixed with the epoxy resin color paste shown in Table 13 in a certain proportion, and the coating was applied according to the relevant provisions of GB / T 6745 "Hull Paint". The weather resistance, acid resistance, salt spray resistance and other properties of the coating were measured, and the performance data are shown in Table 14 below.

[0154] Table 13 Composition of epoxy resin color paste

[0155]

[0156]

[0157] The preparation method of epoxy resin color paste is as follows: first add epoxy resin to a stirring tank, add filler and functional additives in sequence at a stirring speed of 100r / min, then adjust the stirring speed to 1300r / min, disperse for 30min, and perform sand milling after the stirring and dispersion is completed, grind to a fineness of less than 30μm, and obtain epoxy resin color paste. The epoxy equivalent weight (EEW) of the epoxy resin color paste is calculated to be 345. The dispersant is dispersant BYK-P 104S (purchased from BYK, Germany), the defoamer is defoamer BYK-A530 (purchased from BYK, Germany), the anti-settling agent is anti-settling agent BYK-410 (purchased from BYK, Germany), the leveling agent is leveling agent BYK-333 (purchased from BYK, Germany), and the light oxidation stabilizer is light oxidation stabilizer VX56 (purchased from Xinxiu Chemical).

[0158] The mixing ratio of the curing agent and the epoxy resin paste is active hydrogen equivalent (AHEW): epoxy equivalent (EEW) of the paste. For example, the active hydrogen equivalent (AHEW) of the curing agent in Example 1 is 60.9, and the mass ratio of the curing agent and the epoxy resin paste in Example 1 is 60.9:345.

[0159] The coating aging resistance test method shall be carried out in accordance with GB / T 1865-2009 "Artificial weathering and artificial radiation exposure of paints and varnishes to filtered xenon arc radiation", the pulling performance test method shall be carried out in accordance with GB / T5210-2006 "Paints and varnishes adhesion test by pull-off method", the wear resistance test method shall be carried out in accordance with GB / T 1768-2006 "Determination of abrasion resistance of paints and varnishes - Rotating rubber grinding wheel method", the acid and salt water resistance test method shall be carried out in accordance with GB / T 9274-1988 "Determination of resistance of paints and varnishes to liquid media", and the salt spray resistance test method shall be carried out in accordance with GB / T 1771-2007 "Determination of neutral salt spray resistance of paints and varnishes".

[0160] Table 14 Curing agent detection test results of Examples 1-8 and Comparative Examples 1-6

[0161]

[0162]

[0163] It can be seen from the data in Table 14 that the coatings prepared by the silicone epoxy curing agent of Examples 1-8 of the present invention have better anti-corrosion effects than those of Comparative Examples 1-6. The xenon lamp aging resistance refers to GB / T 1766-2008 "Rating Method for Aging of Paint and Varnish Coatings", and the larger the color difference value, the worse the aging resistance. Acid resistance, salt spray resistance, and salt water resistance, the coating is qualified if it does not bubble, rust, crack, or fall off. It can be seen from Table 14 that the introduction of siloxane can effectively enhance the aging resistance and wear resistance of the coating, mainly because the siloxane free group has weaker hydrogen abstraction ability than other groups and is more stable. The addition of KH550 can effectively improve the drawing performance of the coating, mainly because the KH550 coupling agent contains two different functional groups, one end of which is connected to the inorganic material and the other end forms a covalent bond with the resin, thereby coupling the two different materials together to improve their drawing performance. The introduction of alkyl glycidyl ether AGE can improve its flexibility, which is mainly due to its unique long chain effect, which can increase the flexibility of the resin.

[0164] In the specification of the present invention, a lot of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some embodiments, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this specification.

[0165] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0166] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

[0167] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A silicone epoxy curing agent, characterized in that: The following components are included by weight: 42-77 parts of 1,3-cyclohexanedimethylamine; 10-15 parts of polyetheramine D230; 1-3 parts of KH550; 55-83 parts of amino-terminated siloxane; 22-30 parts of amino-terminated long-chain epoxy-amine adduct.

2. The organosilicon epoxy curing agent according to claim 1, characterized in that: The general formula of the amino-terminated siloxane is as follows:

3. The organosilicon epoxy curing agent according to claim 1, characterized in that: The general formula of the amino-terminated long-chain epoxy-amine adduct is as follows:

4. A method for preparing an organosilicon epoxy curing agent, characterized in that: The following steps are involved: 1) Mix 1,3-cyclohexanedimethylamine, polyetheramine D230 and KH550 and stir at room temperature for 20-30 minutes to obtain a base material; 2) mixing disiloxane epoxy double end cap and alkyl glycidyl ether AGE for 20-30 minutes to obtain a dropwise addition material; 3) The base material obtained in step 1) is heated to a certain temperature, stirred under nitrogen protection, and the dropwise material is added dropwise to the base material. After the dropwise addition is completed, the temperature is kept, and then cooled to room temperature to obtain an organosilicon epoxy curing agent.

5. The method for preparing the organosilicon epoxy curing agent according to claim 4, characterized in that: In step 1), the mass percentage of the polyetheramine D230 to 1,3-cyclohexanedimethylamine is 10% to 15%, and the mass percentage of the polyetheramine KH550 to 1,3-cyclohexanedimethylamine is 1% to 3%.

6. The method for preparing the organosilicon epoxy curing agent according to claim 4, characterized in that: In step 2), the mass percentage of the alkyl glycidyl ether AGE to the 1,3-cyclohexanedimethylamine in step 1) is 15% to 20%.

7. The method for preparing the organosilicon epoxy curing agent according to claim 4, characterized in that: In step 2), the mass percentage of the disiloxane epoxy double head to the 1,3-cyclohexanedimethylamine in step 1) is 40% to 60%.

8. The method for preparing the organosilicon epoxy curing agent according to claim 4, characterized in that: In step 2), the alkyl glycidyl ether AGE is selected from at least one of C12 to C14 alkyl glycidyl ethers; and the disiloxane epoxy double-capped functional group R is selected from one of a methyl group and a cycloalkane group.

9. The method for preparing the organosilicon epoxy curing agent according to claim 4, characterized in that: In step 3), the heating temperature is 70-80° C.; the rotation speed is 1000-1200 r / min; the dropping time is 2-3 h, and the dropping rate is 0.4-0.7 g / min.

10. An organosilicon epoxy coating, characterized in that: The organosilicon epoxy coating comprises an epoxy resin color paste and an organosilicon epoxy curing agent in a mass ratio of (60-75):345; the organosilicon epoxy curing agent comprises the following components in parts by weight: 42-77 parts of 1,3-cyclohexanedimethylamine; 10-15 parts of polyetheramine D230; 1-3 parts of KH550; 55-83 parts of amino-terminated siloxane; and 22-30 parts of amino-terminated long-chain epoxy-amine adduct.