Preparation method and application of low-power MXene-based photo-thermal driver with hydrophobic property

By introducing PTFE layers into MXene-based photothermal drivers and using layer-by-layer suction filtration, the problem of MXene materials being suction-free in humid environments is solved, and high-efficiency photothermal conversion and low-power drive are achieved, which improves the stability of the material and application potential.

CN119019755APending Publication Date: 2024-11-26UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146438.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

MXene-based photothermal drivers are susceptible to moisture and oxygen erosion in humid or steam-rich environments, resulting in degradation of structural and functional performance. The existing hydrophobic modification methods lead to high driving power, low photothermal conversion efficiency, and poor long-term stability. .

Method used

A low-power MXene-based photothermal driver composed of a passive layer and an active layer is used. The active layer is MXene and PTFE layers. The hydrophobic film is prepared by layer-by-layer suction filtration to improve the hydrophobicity and photothermal conversion efficiency of the material and reduce energy consumption. .

Benefits of technology

It significantly improves the stability of the material in humid environments and the photothermal conversion efficiency, extends the service life, realizes high-efficiency conversion at low power, is suitable for energy-sensitive application scenarios, and maintains long-term performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019755A_ABST
    Figure CN119019755A_ABST
Patent Text Reader

Abstract

The invention discloses a low-power MXene-based photo-thermal driver with hydrophobic characteristics and a preparation method, the low-power MXene-based photo-thermal driver is composed of a passive layer and an active layer, the active layer is a photo-thermal sensitive material layer MXene and a PTFE layer, and the active layer absorbs light energy and converts the light energy into heat energy; the passive layer is a material layer with a high coefficient of thermal expansion, heat generated by the active layer is transferred downwards to the passive layer, and the passive layer absorbs the heat to expand, so that the whole photo-thermal driver is bent towards the active layer. The preparation method has the advantages that the hydrophobicity and photothermal conversion efficiency of the material are enhanced, and high-efficiency conversion is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the fields of nanomaterial science, photothermal conversion technology and intelligent drive systems, and in particular to a preparation method and application of a low-power MXene-based photothermal actuator with hydrophobic properties. Background Art

[0002] In the field of smart materials and energy conversion, the development of photothermal actuators has important academic and practical value. Photothermal actuators are devices that use light energy to convert into heat energy to drive mechanical systems or change physical states. They are widely used in micro-robots, deformable materials, biomedical devices, and smart textiles. MXene, as an emerging two-dimensional nanomaterial, has become an ideal material for building efficient photothermal actuators due to its excellent light absorption performance and thermal conductivity. Although MXene-based photothermal actuators have demonstrated superior performance in experiments, they still face some challenges in practical applications, especially the environmental stability of materials. Due to its high hydrophilicity, MXene easily absorbs moisture from the air, which may lead to the degradation of its structural and functional properties, especially in humid or water vapor-rich environments. In addition, MXene materials are also easily oxidized in the air, further affecting their long-term stability and reliability.

[0003] In response to these problems, researchers have begun to explore the use of surface modification technology to improve the hydrophobicity of MXene, thereby enhancing its application potential in adverse environments. By introducing hydrophobic molecules or polymer coatings, MXene can be effectively isolated from moisture and oxygen in the environment, protecting MXene from hydrolysis and oxidation, thereby improving its environmental stability. This hydrophobic surface modification not only maintains the original photothermal performance of MXene, but also enhances the service life and reliability of the material in complex environments. However, the currently reported MXene-based hydrophobic photothermal drivers have high driving power, low photothermal conversion efficiency, and poor long-term stability, which is an area that needs to be improved in this application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a low-power MXene-based photothermal actuator with hydrophobic properties, which enhances the hydrophobicity and photothermal conversion efficiency of the material and achieves high-efficiency conversion.

[0005] In order to solve the above technical problems, the present invention provides a low-power MXene-based photothermal actuator with hydrophobic properties. The MXene-based photothermal actuator is composed of a passive layer and an active layer. The active layer is a photothermal sensitive material layer MXene and a PTFE layer, which absorbs light energy and converts it into thermal energy; the passive layer is a material layer with a high thermal expansion coefficient. The heat generated by the active layer is transferred downward to the passive layer. The passive layer absorbs heat and expands, so that the entire photothermal actuator bends toward the active layer. The preparation method thereof comprises the following steps: Step S1: Preparation of a few-layer MXene dispersion; comprising the following specific steps: Step S11: adding 1-2 g LiF into 20-40 mL 9 M HCl solution and stirring to obtain solution A; Further, stirring was performed at 35-45°C for 10-25 min. Step S12: 1-2 g Ti 3 AlC 2 The MAX precursor was slowly added to solution A and stirred continuously at 250-400 r / min; Further, stirring at 35-45° C. for 24-36 h; Step S13: After the reaction is complete, the solution is repeatedly rinsed with deionized water and centrifuged until the pH value of the supernatant reaches a weak acidity; Preferably, the pH range is 6-7; Step S14: the weakly acidic mixed solution is further stripped using high-power ultrasound in an ice bath, centrifuged and the supernatant is collected; Further, peeling for 30-60 min; Step S15: Take 1 mL of the prepared few-layer MXene dispersion and determine the concentration to be 17-25 mg / mL by weighing and vacuum filtration; seal the final MXene aqueous dispersion in a N2 environment and store it at 4°C.

[0006] Step S2: Preparation of MXene-based actuators; The MXene-based film was prepared by vacuum-assisted filtration: the MXene aqueous dispersion was vacuum-filtered using a polycarbonate filter membrane with a pore size of 0.2 µm and then dried to obtain the M / PC film; Step S3: Preparation of hydrophobic MXene-based actuators; On the surface of the M / PC film prepared in step S2, the hydrophobic material polytetrafluoroethylene PTFE is continuously filtered and then dried to obtain a P / M / PC film, which is a hydrophobic MXene-based actuator.

[0007] The filtration method is a layer-by-layer filtration method.

[0008] The volume ratio of the polytetrafluoroethylene PTFE to MXene is 1-2:1-3. Optimally, the volume ratio of the polytetrafluoroethylene PTFE to MXene is 1:2. MXene and PTFE are mixed in an optimized ratio to regulate the light absorption characteristics and thermal conductivity of the composite material to achieve high-efficiency energy conversion.

[0009] The P / M / PC film was illuminated with near-infrared light, and a thermal imager was used to record the real-time temperature changes and observe the driving conditions of the film. The optimal illumination power density was 0.16 W cm -2 The minimum driving light power density is 0.06 W cm -2 .

[0010] The superior effects of the present invention are: 1) Enhanced environmental stability: By introducing hydrophobic modification on the MXene surface, the stability of the material in humid or oxygen-containing environments is significantly improved, the hydrophobicity and photothermal conversion efficiency of the material are enhanced, the erosion of moisture and oxygen is prevented, and the oxidation and hydrolysis of the material are reduced, thereby extending the service life of the driver and maintaining its stable performance; 2) Low power and high efficiency: The preparation method of MXene-based actuators adopts a layer-by-layer filtration method, which achieves efficient light-to-heat conversion under low power input and reduces energy consumption. This is particularly important for energy conservation and sustainable operation, and is especially suitable for energy-sensitive application scenarios; 3) Long-term performance retention: By using high-stability materials and advanced design innovations, the photothermal drive can maintain efficient performance and good mechanical strength even under long-term operation and harsh conditions; 4) Broad application prospects: The above technical advantages make the MXene-based photothermal actuator of the present invention not only suitable for industrial automation, but also widely used in biomedicine, environmental monitoring, smart textiles and other fields. It is particularly suitable for application scenarios that require precise temperature control and high environmental stability, demonstrating broad market potential and application diversity. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings: Figure 1 This is a transmission electron microscope (TEM) photograph of MXene prepared in a specific embodiment of the present invention; Figure 2 The scanning electron microscope (SEM) image of the M / PC film prepared in the specific embodiment of the present invention; Figure 3Scanning electron microscope (SEM) spectrum of the P / M / PC film prepared in a specific embodiment of the present invention Figure 4 UV-Vis-NIR diffuse reflection test spectra of P / M / PC films with different volume ratios prepared in specific embodiments of the present invention; Figure 5 The natural light drive and bionic animal crawling application of P / M / PC in the specific embodiment of the present invention; Figure 6 The Marangoni actuator and plant thermal regulation application of P / M / PC in the specific embodiment of the present invention; Figure 7 This is a physical picture of the small intestine during the "welding" process in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0012] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0013] The present invention provides a low-power MXene-based photothermal actuator with hydrophobic properties. The MXene-based photothermal actuator is composed of a passive layer and an active layer. The active layer is a photothermal sensitive material layer of MXene and a PTFE layer, which absorbs light energy and converts it into heat energy; the passive layer is a material layer with a high thermal expansion coefficient, which is a PC film. The heat generated by the active layer is transferred downward to the passive layer, and the passive layer absorbs the heat and expands, causing the entire photothermal actuator to bend in the direction of the active layer; the preparation method thereof comprises the following steps: Step S1: Preparation of few-layer MXene dispersion; 1-2 g LiF was added to 20-40 mL 9 M HCl solution and stirred at 35-45°C for 10-25 min; then, 1-2 g Ti 3 AlC 2 The MAX precursor was slowly added to the above solution and stirred continuously at 250-400 r / min for 24-36 h at 35-45°C. After complete reaction, the solution was repeatedly rinsed with deionized water and centrifuged until the pH value of the supernatant reached about 6-7. Subsequently, the solution was mixed and further exfoliated with 400W ultrasound in an ice bath for 30-60 min, and then centrifuged and the supernatant was collected. 1 mL of the prepared few-layer MXene dispersion was taken from it, and the concentration was determined to be 17 mg / mL by weighing and vacuum filtration. Finally, the final MXene aqueous dispersion was sealed in a N2 environment and stored at 4°C. The transmission electron microscope photo of the obtained MXene is shown in FIG. Figure 1 shown.

[0014] Step S2: preparing MXene / PC film by vacuum-assisted filtration; The few-layer MXene aqueous dispersion prepared in step S1 was diluted to 5 mg / mL, and 2 mL of the above solution was accurately drawn with a pipette. The MXene aqueous dispersion was vacuum filtered through a polycarbonate PC membrane with a pore size of 0.2 µm, and then dried to obtain a MXene / PC film. The scanning electron microscope photo is shown in FIG. Figure 2 The best preparation method is layer-by-layer filtration.

[0015] Step S3: Preparation of hydrophobic MXene-based actuators; Use a pipette to accurately draw 1 mL of 0.1 g / mL PTFE solution, and continue to filter it onto the surface of the M / PC film prepared in step S2 by vacuum filtration. After drying, the P / M / PC film is obtained, which is a hydrophobic MXene-based actuator. The scanning electron microscope photo is shown in FIG. Figure 3 The best preparation method is layer-by-layer filtration.

[0016] The present invention also provides a method for optimizing the experimental parameters of driver performance, including optimization of infrared light power density, optimization of MXene and PTFE filtration volumes, and optimization of MXene and PTFE filtration methods; The near-infrared light power density is optimized by selecting near-infrared light power density of 0.06, 0.12, and 0.16 Wcm -2 , P / M / PC films of the same size were illuminated for the same time, and a thermal imager was used to record the real-time temperature changes and observe the driving conditions of the films. According to the experimental results, the optimal illumination power density is 0.16 W cm -2 The minimum driving light power density is 0.06 W cm -2 .

[0017] The optimization of the MXene and PTFE filtration volumes is as follows: first fix the volume of PTFE to 1 mL, change the volume of MXene to 0.5 mL, 1 mL, 2 mL, and 3 mL, prepare P / M / PC films in the above ratio, use the above-determined optimal power density for irradiation, and record the real-time temperature and driving angle changes. According to the experimental results, the optimal volume of MXene is 2 mL. Based on the aforementioned fixed MXene volume of 2 mL, change the volume of PTFE to 0, 1 mL, and 2 mL, prepare P / M / PC films in the above ratio, use the above-determined optimal power density for irradiation, and record the real-time temperature and driving angle changes. According to the experimental results, the optimal volume of PTFE is 1 mL.

[0018] The optimization of the filtration method of MXene and PTFE is: two methods are used to prepare the actuator respectively: MXene and PTFE were filtered layer by layer onto the PC membrane and dried to obtain the P / M / PC membrane; First, MXene and PTFE were mixed, then filtered onto a PC membrane, and dried to obtain a P+M / PC membrane; In both methods, the volume ratio of MXene to PTFE was 2:1, and 0.16 W cm -2 The light power density was used for illumination, and the real-time temperature and driving angle changes were recorded. According to the experimental results, the best preparation method for hydrophobic MXene-based actuators is the layer-by-layer filtration method.

[0019] In order to verify the effect of different volume ratios of MXene and PTFE on the photothermal conversion effect, the light absorption capacity of different films was studied by UV-Vis-NIR diffuse reflection. The results show that as the volume of MXene increases, the light absorption intensity also increases; after adding PTFE, the light absorption intensity of the film is enhanced, but if the volume of PTFE continues to increase, the light absorption intensity will tend to decrease. This is because the more PTFE there is, the more light intensity it absorbs, resulting in less light energy reaching the MXene layer, such as Figure 4 As shown. Figure 4 As shown in Figure a, as the volume of MXene increases, the absorption peak in the UV-Vis-NIR spectrum gradually increases, indicating that the increase in the amount of MXene effectively improves the photothermal efficiency of the P / M / PC film. This phenomenon is attributed to the light absorption and photothermal conversion properties of MXene, which converts light energy into thermal energy. However, the incident light energy is partially absorbed by the MXene layer, and the rest is reflected from the surface, resulting in energy dissipation, low photothermal conversion efficiency, and low photothermal heating effect. In contrast, the PTFE NP coating on the MXene surface effectively improves this situation. UV-Vis-NIR test results ( Figure 4 b) shows that the absorbance of the P / 2M / PC film is higher than that of the 2M / PC film, especially in the wavelength range of 750–1500 nm, where the absorbance increases significantly and reaches a peak value of about 1.6. This improvement indicates that the addition of PTFE improves the light absorption capacity of the 2M / PC film, especially in the NIR region, thus having a positive impact on the photothermal conversion efficiency.

[0020] Application of the hydrophobic MXene-based actuator in the hydrophobic bionic device of the present invention: The prepared MXene-based actuator is driven under extremely low light power, and sunlight is used to verify whether the film can be driven. The film is placed outdoors and covered with a culture dish to isolate the film from the influence of wind. The sunlight is blocked by hand to observe the driving condition of the film. Figure 5 As shown in a1–a3, the film reaches the maximum bending angle within 7 s. After the sun is blocked ( Figure 5 a4–a6), the film quickly returns to its initial state within 4 s.

[0021] Application of the hydrophobic MXene-based actuator in the hydrophobic bionic device of the embodiment of the present invention: using a paper cutter and Adobe Illustration software, actuators of different shapes are designed, and using a continuous switching laser, the actuator is made to perform bionic motion, such as Figure 5 As shown in b, during the near-infrared light irradiation, the "crab-shaped" robot arched upwards, and then returned to its initial state after the near-infrared light was turned off. Repeatedly turning the near-infrared laser on and off caused the "crab-shaped" robot to send obvious displacements ( Figure 5 c), and the lighting position controls the motion trajectory. A similar pattern cutting was also used to design an "octopus-shaped" robot that exhibited the same crawling characteristics ( Figure 5 d, e). Therefore, this untethered photothermal actuator encodes controllable biomimetic motion.

[0022] Application of hydrophobic MXene-based actuators in hydrophobic bionic devices according to embodiments of the present invention: The P / M / PC film is hydrophobic and suspended on the water surface. When the film is exposed to near-infrared light, it effectively runs on water, thereby crossing obstacles and weight transportation. The temperature increase caused by the photothermal effect forms a local temperature gradient on the water surface. According to the Marangoni effect, the surface tension of a liquid is inversely proportional to the temperature, where areas with higher surface tension exert greater pulling force on the surrounding liquid. Therefore, the temperature gradient field selectively generates a surface tension gradient field, which ultimately causes the film to move toward areas with higher surface tension (i.e., lower temperature). Figure 6 a shows a water transporter made of MXene actuators as a proof-of-concept demonstration. –2 Under near-infrared irradiation with laser power, the transport robot crosses preset obstacles on the water surface within tens of seconds by changing the illumination position. In addition, through the photothermal effect, the water transporter carries a load much heavier than its weight. Under near-infrared irradiation, the transporter carries a load 200 times its own weight, making it suitable for transporting biomaterials and drugs for directional delivery, such as Figure 6 As shown in b.

[0023] Application of the hydrophobic MXene-based actuator in a hydrophobic bionic device according to an embodiment of the present invention: The P / M / PC film is applied to heat-sensitive plant leaves, and the closing or opening of the plant leaves is controlled by light according to growth requirements, such as Figure 6c1-c2. By attaching the MXene film to the Mimosa pudica leaves, the surface temperature of the leaves increased rapidly from 28.2°C to 57.5°C under near-infrared irradiation, stimulating the leaf closure, as shown in the circled area in the figure. In contrast, the original leaves were without Xene film attached ( Figure 6 c3), using the same near-infrared light power and irradiation time, the temperature of the leaves remained basically unchanged and maintained the initial state. This hydrophobic bionic device has potential application prospects in artificial rhythm regulation of crops and plants.

[0024] Application of hydrophobic MXene-based actuators in biological tissue welding according to an embodiment of the present invention: "welding" of mouse small intestine wounds. The mice were given general anesthesia using the anesthetic urethane. After anesthesia, the hair in the surgical area was shaved, and the surgical area was thoroughly disinfected with 75% alcohol. A small longitudinal incision was made on the abdomen of the mouse, and the skin and abdominal wall were gently separated to expose the small intestine. A section of the small intestine was selected, and an incision was made at the designated location using surgical scissors without affecting the blood supply. The prepared P / M / PC was applied to the wound area, and then the treated area was irradiated with near-infrared light of a specific wavelength of 808 nm. Under the action of light, the P / M / PC film rapidly converts light energy into heat energy, triggering a local temperature rise, prompting tissue protein denaturation, and achieving rapid "welding" of the wound. The actual picture of the "welding" process is shown in the figure. Figure 7 shown.

[0025] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties, comprising the following steps: Step S1: Preparation of few-layer MXene dispersion; Step S2: Preparation of MXene-based actuators; The M / PC film was prepared by vacuum-assisted filtration; Step S3: Preparation of hydrophobic MXene-based actuators; On the surface of the M / PC film prepared in the above steps, the hydrophobic material polytetrafluoroethylene PTFE is continuously filtered and then dried to obtain a P / M / PC film.

2. The method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties according to claim 1, characterized in that: The step S1 comprises the following specific steps: Step S11: adding 1-2 g LiF into 20-40 mL 9 M HCl solution and stirring to obtain solution A; Step S12: slowly add 1-2 g of Ti3AlC2 MAX precursor into solution A and continue stirring at a speed of 250-400 r / min; Step S13: After the reaction is complete, the solution is repeatedly rinsed with deionized water and centrifuged until the pH value of the supernatant reaches a weak acidity; Step S14: the weakly acidic mixed solution is further stripped using high-power ultrasound in an ice bath, centrifuged and the supernatant is collected; Step S15: Take 1 mL of the prepared few-layer MXene dispersion, determine the concentration by weighing and vacuum filtration, and seal the final MXene aqueous dispersion in a N2 environment and store it at 4°C.

3. The method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties according to claim 1, characterized in that: The step S2 adopts a vacuum-assisted filtration method to prepare the M / PC film, which is to use a polycarbonate filter membrane with a pore size of 0.2 µm to vacuum filter the MXene aqueous dispersion, and then dry it to obtain the M / PC film.

4. The method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties according to claim 1, characterized in that: The filtration in step S3 is layer-by-layer filtration.

5. The method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties according to claim 1, characterized in that: The volume ratio of the polytetrafluoroethylene PTFE to MXene is 1-2:1-3.

6. The method for preparing a low-power MXene-based photothermal actuator with hydrophobic properties according to claim 5, characterized in that: The optimized volume ratio of polytetrafluoroethylene PTFE to MXene is 1:

2.

7. A low-power MXene-based photothermal actuator with hydrophobic properties prepared by the preparation method described in any one of claims 1-6.

8. A low-power MXene-based photothermal actuator with hydrophobic properties according to claim 7, characterized in that: The MXene-based photothermal actuator is composed of a passive layer and an active layer. The active layer is a photothermal sensitive material layer of MXene and PTFE, which absorbs light energy and converts it into heat energy. The passive layer is a material layer with a high thermal expansion coefficient. The heat generated by the active layer is transferred downward to the passive layer, which absorbs heat and expands, causing the entire photothermal actuator to bend toward the active layer. The optimal illumination power density is 0.16 W cm -2 The minimum driving light power density is 0.06 W cm -2 .

9. Application of a low-power MXene-based photothermal actuator with hydrophobic properties prepared by the preparation method described in any one of claims 1 to 6 in a hydrophobic bionic device.