Ultrathin semitransparent high-temperature-resistant antioxidant coating for metal surface, preparation method and construction process
By using ultra-thin translucent paint with ceramic resin and other components on the metal surface, combined with specific stirring and spraying processes, the existing coatings have been solved, and high temperature resistance, oxidation resistance, Strong adhesion and low cost effects.
Patent Information
- Application Number
- CN202411122084.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing high-temperature and antioxidant coatings for metal surfaces have problems such as high cost, thick coating, poor adhesion and easy shedding.
Using an ultra-thin translucent high-temperature antioxidant coating including ceramic resin, wetting agent, leveling agent and hexagonal boron nitride powder, it is prepared and sprayed on the metal surface through a specific stirring and spraying process, and the coating thickness is controlled. At 5-8 microns, spray with a spray gun and cure in an oven.
It has achieved high temperature resistance, anti-oxidation, strong adhesion, difficult to fall off, thin spray thickness and low cost, and simplified production process, improved production efficiency and the possibility of large-scale production.
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to an ultra-thin translucent high-temperature resistant and anti-oxidation coating for metal surfaces, a preparation method and a construction process. Background Art
[0002] The high temperature resistance and anti-oxidation treatment of metal surface is generally carried out by spray coating. Spraying high temperature resistant and anti-oxidation coating materials is costly, thick and has high stress; cold spraying or brushing coatings have thick coatings and are easy to fall off.
[0003] Therefore, it is necessary to develop a coating with thin spray thickness, strong adhesion, not easy to fall off, high temperature resistance and good oxidation resistance. Summary of the invention
[0004] The invention proposes an ultra-thin translucent high-temperature resistant and anti-oxidation coating for metal surface, a preparation method and a construction process, which solves the problems of high cost, thick coating, weak adhesion and easy falling off of existing high-temperature resistant and anti-oxidation coatings for metal surface.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention firstly proposes an ultra-thin translucent high temperature resistant and anti-oxidation coating for metal surface, which comprises the following components in parts by mass:
[0007] Ceramic resin: 50 parts;
[0008] Wetting agent: 0.2-0.5 parts;
[0009] Leveling agent: 0.2-0.5 parts;
[0010] Hexagonal boron nitride powder: 7-9 parts;
[0011] Anhydrous alcohol: 40-42 parts.
[0012] The present invention secondly proposes a method for preparing an ultra-thin translucent high-temperature resistant and anti-oxidation coating for a metal surface. The ultra-thin translucent high-temperature resistant and anti-oxidation coating for a metal surface described above is used. During preparation, ceramic resin, anhydrous alcohol accounting for 80% of the total mass, and hexagonal boron nitride powder are sequentially added to a mixer and stirred and mixed. The speed of the mixer is 2000-3000 rpm. After stirring for 15 minutes, a wetting agent and a leveling agent are added, and stirring and mixing are continued. After 5 minutes, the remaining 20% of the mass of anhydrous alcohol is added, and stirring and mixing is continued for 5 minutes.
[0013] The present invention further provides a construction process for an ultra-thin translucent high temperature resistant and anti-oxidation coating on a metal surface, comprising the following steps:
[0014] (1) First, the metal surface is sandblasted with a sand particle size of 120-150 mesh. After the sandblasting is completed, the metal surface is dusted with an air gun;
[0015] (2) Spraying is carried out in a clean workshop of 100,000 grade, with a temperature of 20-26 degrees and a humidity not exceeding 85%. The ultra-thin translucent high-temperature resistant and anti-oxidation coating on the metal surface prepared by the above construction process is sprayed on the metal surface using a tank-type spray gun or an automatic spray gun. The spray gun caliber is 0.8-1.4 mm, the air pressure is 0.4-0.6 MPa, and the coating thickness is between 5-8 microns;
[0016] (3) Put the sprayed metal parts into the oven for curing. The curing process is to heat up to 80 degrees in 10-15 minutes, then keep it warm for 15-20 minutes, then heat up to 200 degrees in 15-20 minutes, maintain it for 20-30 minutes, cool it down to below 100 degrees with the furnace, take it out and place it at room temperature, and conduct an appearance inspection. There should be no bubbles and impurities on the surface.
[0017] Beneficial effects of the present invention:
[0018] 1. The coating of the present invention has the advantages of high temperature resistance, oxidation resistance, strong adhesion, not easy to fall off, thin spray thickness and low cost.
[0019] 2. The coating preparation method of the present invention is simple, has high production efficiency, low cost, and is easy to mass produce.
[0020] 3. The construction process of the present invention is simple and efficient, the spraying quality is high, the spraying thickness is thin, and it is not easy to fall off. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] Example 1
[0023] An ultra-thin translucent high-temperature resistant and anti-oxidation coating for metal surface, comprising the following components in parts by mass:
[0024] Ceramic resin: 50 parts;
[0025] Wetting agent: 0.2-0.5 parts;
[0026] Leveling agent: 0.2-0.5 parts;
[0027] Hexagonal boron nitride powder: 7-9 parts;
[0028] Anhydrous alcohol: 40-42 parts.
[0029] The coating of the invention has the advantages of high temperature resistance, oxidation resistance, strong adhesion, not easy to fall off, thin spraying thickness and low cost.
[0030] Example 2
[0031] The present invention secondly proposes a method for preparing an ultra-thin translucent high-temperature resistant and anti-oxidation coating on a metal surface. The ultra-thin translucent high-temperature resistant and anti-oxidation coating on a metal surface described in Example 1 is used. During the preparation, ceramic resin, anhydrous alcohol accounting for 80% of the total mass, and hexagonal boron nitride powder are sequentially added into a blender for stirring and mixing. The speed of the blender is 2000-3000 rpm. After stirring for 15 minutes, a wetting agent and a leveling agent are added, and stirring and mixing are continued. After 5 minutes, the remaining 20% by mass of anhydrous alcohol is added, and stirring and mixing is performed again for 5 minutes.
[0032] The coating preparation method of the invention is simple, has high production efficiency, low cost and is easy for large-scale production.
[0033] Example 3
[0034] The present invention further provides a construction process for an ultra-thin translucent high temperature resistant and anti-oxidation coating on a metal surface, comprising the following steps:
[0035] (1) First, the metal surface is sandblasted with a sand particle size of 120-150 mesh. After the sandblasting is completed, the metal surface is dusted with an air gun;
[0036] (2) Spraying is performed in a clean workshop of 100,000 class, at a temperature of 20-26 degrees and a humidity of no more than 85%. The ultra-thin translucent high-temperature resistant and antioxidant coating for metal surface prepared in Example 2 is used. A tank-type spray gun or an automatic spray gun is used to spray the metal surface. The spray gun caliber is 0.8-1.4 mm, the air pressure is 0.4-0.6 MPa, and the coating thickness is between 5-8 μm.
[0037] (3) Put the sprayed metal parts into the oven for curing. The curing process is to heat up to 80 degrees in 10-15 minutes, then keep it warm for 15-20 minutes, then heat up to 200 degrees in 15-20 minutes, maintain it for 20-30 minutes, cool it down to below 100 degrees with the furnace, take it out and place it at room temperature, and conduct an appearance inspection. There should be no bubbles and impurities on the surface.
[0038] The construction process of the invention is simple and efficient, the spraying quality is high, the spraying thickness is thin, and it is not easy to fall off.
[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An ultra-thin translucent high temperature resistant and anti-oxidation coating for metal surfaces. Features: In parts by mass, it includes the following components: Ceramic resin: 50 parts; Wetting agent: 0.2-0.5 parts; Leveling agent: 0.2-0.5 parts; Hexagonal boron nitride powder: 7-9 parts; Anhydrous alcohol: 40-42 parts.
2. A method for preparing an ultra-thin translucent high temperature resistant and anti-oxidation coating for metal surface, Features: The ultra-thin translucent high-temperature resistant and antioxidant coating for metal surface as described in claim 1 is used. During preparation, ceramic resin, 80% of the total mass of anhydrous alcohol and hexagonal boron nitride powder are sequentially added to a blender and stirred and mixed. The speed of the blender is 2000-3000 rpm. After stirring for 15 minutes, a wetting agent and a leveling agent are added, and stirring and mixing are continued. After 5 minutes, the remaining 20% of the mass of anhydrous alcohol is added, and stirring and mixing is performed again for 5 minutes.
3. Construction technology of ultra-thin translucent high temperature resistant and anti-oxidation coating on metal surface: Features: The following steps are involved: (1) First, the metal surface is sandblasted with a sand particle size of 120-150 mesh. After the sandblasting is completed, the metal surface is dusted with an air gun; (2) Spraying is carried out in a clean workshop of 100,000 grade, with a temperature of 20-26 degrees and a humidity not exceeding 85%. The ultra-thin translucent high-temperature resistant and anti-oxidation coating on the metal surface prepared by the construction process of claim 2 is sprayed on the metal surface using a tank spray gun or an automatic spray gun, the spray gun caliber is 0.8-1.4 mm, the air pressure is 0.4-0.6 MPa, and the coating thickness is between 5-8 microns; (3) Put the sprayed metal parts into the oven for curing. The curing process is to heat up to 80 degrees in 10-15 minutes, then keep it warm for 15-20 minutes, then heat up to 200 degrees in 15-20 minutes, maintain it for 20-30 minutes, cool it down to below 100 degrees with the furnace, take it out and place it at room temperature, and conduct an appearance inspection. There should be no bubbles and impurities on the surface.
Citation Information
Patent Citations
Nanometer hybridized ceramic resin coating as well as preparation method and application of nanometer hybridized ceramic resin coating
CN109370397A
Heat dissipation coating, preparation method thereof and heating device
CN116676000A
Ceramic composition and method for manufacturing the same, and heat radiating member using the same
KR1020150004712A