Special steel bar anticorrosive paint for aerated concrete plate and production method of special steel bar anticorrosive paint

By using nanosheet-like carbon-containing silicon powder and ferrous oxide in aerated concrete slabs, the problems of easy cracking and low adhesion of existing steel bar anticorrosion paints are solved, and high adhesion and Anti-corrosion, improving the durability and crack resistance of the board.

CN119019892APending Publication Date: 2024-11-26JIANGXI MINERAL RESOURCES GUARANTEE SERVICE CENT +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411340067.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing reinforced anticorrosion paint is prone to cracking, has low adhesion and rust in aerated concrete slabs, which affects the durability of the slabs.

Method used

The nanosheet-like carbon-containing silicon powder, ferrous oxide and blending agent are prepared in a specific proportion. The steel bar anticorrosion paint with high viscosity and crack resistance is prepared by stirring, and the ferrous oxide is ensured during the production process. Completely dispersed.

Benefits of technology

It improves the adhesion between steel bars and concrete, eliminates surface bubbles, enhances crack resistance and corrosion resistance, and improves the durability and temperature and heat corrosion resistance of the board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019892A_ABST
    Figure CN119019892A_ABST
Patent Text Reader

Abstract

The invention relates to a special steel bar anticorrosive paint for aerated concrete slabs and a production method thereof. The special steel bar anticorrosive paint is prepared by mixing and stirring the following components by mass: 600-800Kg of styrene-butadiene latex series; the weight of the nano flaky carbon-containing plant silicon powder is 130Kg to 350Kg; 30 Kg to 60 Kg of ferrous oxide; 20 Kg to 40 Kg of a defoaming agent; and 0.015 Kg-0. 025 Kg of a blending agent. The invention relates to the technical field of steel bar anticorrosive paint. According to the present invention, the use is safe and convenient, the dip-coating and the brush-coating can be performed, the nano sheet-shaped carbon-containing silicon-planting body SiO2 powder has the sheet-shaped diameter-thickness ratio of 5-20 and the particle size of 300 nm-5 [mu] m, such that the steel bar has no crack after the dip-coating and drying, the 1-2 mm bubble attached to the upper surface of the longitudinal steel bar is eliminated, the adhesion force of the cylinder mould steel bar after the paint dipping is enhanced, and the cylinder mould steel bar can be firmly combined with the concrete so as to achieve the good water resistance. The steel bar adhesive force detection value reaches about 1.8 Mpa, the crack resistance is enhanced, good corrosion resistance is achieved, and the durability of the plate structure is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel bar anticorrosion paint, in particular to a special steel bar anticorrosion paint for aerated concrete plates and a production method thereof. Background Art

[0002] Steel bar anticorrosive paint is a necessary material for mesh cage dipping in the production of autoclaved aerated concrete panels. It uses carboxylated styrene butadiene latex as the main raw material, nano-flaky carbon-containing phytolith SiO2 powder as the auxiliary raw material, and ferrous oxide as an antioxidant. They are mixed in a certain proportion in a special mixing tank, and poured into the dipping tank for use after stirring. The shortcomings of the anticorrosive paint prepared with these four raw materials are: the surface of the mesh cage dipped paint after anticorrosion is prone to cracking, especially the large surface of the connecting piece shows multiple fine cracks, small bubbles are attached to the upper surface of the longitudinal steel bar, it is easy to rust, the temperature and heat resistant rust area rate exceeds 5%, and the adhesion between the paint and the steel bar is low. The steel bar adhesion test value is only about 1.0Mpa, which affects the durability of the plate structure. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a special steel bar anti-corrosion paint for aerated concrete panels and a production method thereof, which has high hiding power, high adhesion, high crack resistance and good durability and is suitable for use with autoclaved aerated concrete panels.

[0004] The above technical objectives of the present invention are achieved through the following technical solutions: The special steel anti-corrosion paint for aerated concrete plates includes the following ingredients mixed and stirred in a mass ratio: styrene-butadiene latex series: 600Kg-800Kg; nano-flaky carbon-containing phytolith powder: 130Kg-350Kg; ferrous oxide: 30Kg-60Kg; defoaming agent: 20Kg-40Kg; blending agent: 0.015Kg-0.025Kg.

[0005] In a preferred example, the present invention can be further configured as follows: the styrene butadiene latex series includes one of styrene butadiene latex, carboxylated styrene butadiene latex, and carboxylated styrene butadiene latex.

[0006] In a preferred example, the present invention can be further configured as follows: the nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province, which is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flake diameter-to-thickness ratio of 5-20, and a particle size of 300 nanometers-5μm.

[0007] In a preferred example, the present invention can be further configured as follows: the ferrous oxide is CAS No.: 1345-25-1.

[0008] In a preferred example, the present invention can be further configured as follows: the defoaming agent is octanol or 2-ethylhexanol.

[0009] In a preferred example, the present invention can be further configured as follows: the conditioning agent is sodium tetraborate decahydrate.

[0010] The production method of special steel bar anticorrosive paint for aerated concrete plate comprises the following steps: S1, weigh the following raw materials according to the mass ratio: styrene-butadiene latex series: 600Kg-800Kg; nano-flaky carbonaceous phytolith powder: 130Kg-350Kg; ferrous oxide: 30Kg-60Kg; defoaming agent: 20Kg-40Kg; blending agent: 0.015Kg-0.025Kg.

[0011] S2, pour the styrene-butadiene latex series into a special stirring tank, stir for 5-30 minutes, gradually pour the phytolith SiO2 powder into the stirring tank, and stir for 5-30 minutes; S3, add defoamer and continue stirring; S4, after the generated ammonia smell is exhausted, slowly add ferrous oxide and continue stirring for 5-30 minutes to completely disperse the ferrous oxide; S5, finally add the blending agent and stir until evenly mixed to obtain the special steel anti-corrosion paint for aerated concrete panels.

[0012] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The present invention is safe and convenient to use, can be dipped or brushed, and because the nano-flaky carbon-containing phytolith SiO2 powder has a flake diameter-to-thickness ratio of 5-20 and a particle size of 300 nanometers to 5 μm, there is no crack after the steel bar is dipped and dried, and the bubbles of ¢1-2 mm attached to the upper surface of the longitudinal steel bar are eliminated, and the bonding force of the mesh steel bar after the dip painting is enhanced, and the steel bar is firmly bonded to the concrete. The steel bar adhesion test value reaches about 1.8 Mpa, which enhances the crack resistance, has good corrosion resistance, and improves the durability of the plate structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a SEM image of nano-flaky carbon-containing phytolith SiO2 powder. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below in conjunction with the accompanying drawings. Embodiment 1:

[0015] Reference Figure 1The special steel anticorrosive paint for aerated concrete plates disclosed by the present invention comprises the following components which are mixed and stirred in a mass ratio: styrene-butadiene latex series: 600 kg; nano-flaky carbonaceous phytolith powder: 200 kg; ferrous oxide: 60 kg; defoamer: 40 kg; and blending agent: 0.025 kg.

[0016] The styrene butadiene latex series is carboxylated styrene butadiene latex.

[0017] The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flaky appearance with a thickness of less than 100nm, and a particle size of 300nm-5μm.

[0018] The ferrous oxide is CAS No.: 1345-25-1.

[0019] The defoaming agent is octanol.

[0020] The blending agent is sodium tetraborate decahydrate. Embodiment 2:

[0021] Based on the raw materials provided in Example 1, the present invention also provides a method for producing a special steel anti-corrosion paint for air concrete plates, comprising the following steps: S1, weigh the following raw materials according to the mass ratio: the following ingredients are mixed and stirred according to the mass ratio: styrene-butadiene latex series: 600Kg; nano-flaky carbonaceous phytolith powder: 200Kg; ferrous oxide: 60Kg; defoaming agent: 40Kg; and blending agent: 0.025Kg.

[0022] S2, pour the carboxylated styrene butadiene latex into a special stirring tank, stir for 5-30 minutes, gradually pour the phytolith SiO2 powder into the stirring tank, and stir for 5-30 minutes; S3, add defoamer and continue stirring; S4, after the generated ammonia smell is exhausted, slowly add ferrous oxide and continue stirring for 10-60 minutes to completely disperse the ferrous oxide; S5, finally add the blending agent and stir until evenly mixed to obtain the special steel anti-corrosion paint for aerated concrete panels.

[0023] In summary, in combination with Example 1 and Example 2, the special steel bar anti-corrosion paint for aerated concrete plates is obtained by using the above-mentioned raw materials and the above-mentioned method. After testing, the following results are obtained: there are no cracks on the steel bars after dipping and drying, and the bubbles of 1-2 mm attached to the upper surface of the longitudinal steel bars are eliminated. The bonding force of the mesh steel bars after dipping is enhanced, and the paint is firmly bonded to the concrete. The steel bar adhesion test value reaches 1.8Mpa, the heat and heat corrosion area rate reaches 3.7%, the crack resistance is enhanced, it has good corrosion resistance, and the durability of the plate structure is improved. Embodiment 3:

[0024] Reference Figure 1 The special steel anticorrosive paint for aerated concrete plates disclosed by the present invention comprises the following components which are mixed and stirred in a mass ratio: 800 kg of carboxyl styrene butadiene latex; 130 kg of nano-flaky carbonaceous phytolith SiO2 powder; 30 kg of ferrous oxide; 40 kg of defoaming agent; and 0.025 kg of blending agent.

[0025] The styrene butadiene latex series is PC-2 type carboxyl styrene butadiene latex.

[0026] The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flaky appearance with a thickness of less than 100nm, and a particle size of 300nm-5μm.

[0027] The ferrous oxide is CAS No.: 1345-25-1.

[0028] The defoaming agent is octanol.

[0029] The blending agent is sodium tetraborate decahydrate.

[0030] In this embodiment, the materials provided in this embodiment are used and the production method provided in Example 2 is utilized to obtain a special steel anti-corrosion paint for aerated concrete plates. After testing, the steel bars are free of cracks after dipping and drying, and the bubbles of 1-2 mm attached to the upper surface of the longitudinal steel bars are eliminated. The bonding strength of the mesh steel bars after dipping is enhanced, and the paint is firmly bonded to the concrete. The steel bar adhesion test value reaches 1.85Mpa, and the heat corrosion resistance area rate reaches 3.5%, which enhances the crack resistance, has good corrosion resistance, and improves the durability of the plate structure. Embodiment 4:

[0031] The special steel anticorrosive paint for aerated concrete plate disclosed by the invention comprises the following components which are mixed and stirred according to mass ratio: 700 kg of carboxyl styrene butadiene latex; 220 kg of nano-flaky carbonaceous phytolith SiO2 powder; 60 kg of ferrous oxide; 20 kg of defoaming agent; and 0.015 kg of blending agent.

[0032] The carboxylated styrene butadiene latex is PC-2 type carboxylated styrene butadiene latex.

[0033] The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flaky appearance with a thickness of less than 100nm, and a particle size of 300nm-5μm.

[0034] The ferrous oxide has a CAS No. of 1345-25-1.

[0035] The defoaming agent is 2-ethylhexanol.

[0036] The blending agent is sodium tetraborate decahydrate.

[0037] In this embodiment, the materials provided in this embodiment are used and the production method provided in Example 2 is utilized to obtain a special steel anti-corrosion paint for aerated concrete plates. After testing, the steel bars are free of cracks after dipping and drying, and the bubbles of 1-2 mm attached to the upper surface of the longitudinal steel bars are eliminated. The bonding force of the mesh steel bars after dipping is enhanced, and the paint is firmly bonded to the concrete. The steel bar adhesion test value reaches 1.7 Mpa, and the heat corrosion resistance area rate reaches 3.5%, which enhances the crack resistance, has good corrosion resistance, and improves the durability of the plate structure. Embodiment 5:

[0038] The special steel anticorrosive paint for aerated concrete plate disclosed by the invention comprises the following components which are mixed and stirred according to mass ratio: 620 kg of carboxyl styrene butadiene latex; 300 kg of nano-flaky carbonaceous phytolith SiO2 powder; 50 kg of ferrous oxide; 30 kg of defoaming agent; and 0.020 kg of blending agent.

[0039] The carboxylated styrene butadiene latex is PC-2 type carboxylated styrene butadiene latex.

[0040] The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flaky appearance with a thickness of less than 100nm, and a particle size of 300nm-5μm.

[0041] The ferrous oxide has a CAS No. of 1345-25-1.

[0042] The defoaming agent is 2-ethylhexanol.

[0043] The blending agent is sodium tetraborate decahydrate.

[0044] In this embodiment, the materials provided in this embodiment are used and the production method provided in Example 2 is utilized to obtain a special steel anti-corrosion paint for aerated concrete plates. After testing, the steel bars are free of cracks after dipping and drying, and the bubbles of 1-2 mm attached to the upper surface of the longitudinal steel bars are eliminated. The bonding force of the mesh steel bars after dipping is enhanced, and the paint is firmly bonded to the concrete. The steel bar adhesion test value reaches 1.6Mpa, and the heat corrosion resistance area rate reaches 3.83%, which enhances the crack resistance, has good corrosion resistance, and improves the durability of the plate structure. Embodiment 6:

[0045] The special steel anticorrosive paint for aerated concrete plate disclosed by the invention comprises the following components which are mixed and stirred according to mass ratio: carboxylated styrene butadiene latex: carboxylated styrene butadiene latex: 750 kg; nano-flaky carbonaceous phytolith SiO2 powder: 200 kg; ferrous oxide: 30 kg; defoamer: 20 kg; and blending agent: 0.015 kg.

[0046] The carboxylated styrene butadiene latex is PC-2 type carboxylated styrene butadiene latex.

[0047] The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flaky appearance with a thickness of less than 100nm, and a particle size of 300nm-5μm.

[0048] The ferrous oxide has a CAS No. of 1345-25-1.

[0049] The defoaming agent is octanol.

[0050] The blending agent is sodium tetraborate decahydrate.

[0051] In this embodiment, the materials provided in this embodiment are used and the production method provided in Example 2 is utilized to obtain a special steel anti-corrosion paint for aerated concrete plates. After testing, the steel bars are free of cracks after dipping and drying, and the bubbles of 1-2 mm attached to the upper surface of the longitudinal steel bars are eliminated. The bonding force of the mesh steel bars after dipping is enhanced, and the paint is firmly bonded to the concrete. The steel bar adhesion test value reaches 1.52Mpa, and the heat corrosion resistance area rate reaches 3.51%, which enhances the crack resistance, has good corrosion resistance, and improves the durability of the plate structure.

[0052] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Special steel anti-corrosion paint for aerated concrete plate, characterized by: The following ingredients are mixed and stirred according to mass ratio: styrene-butadiene latex series: 600Kg-800Kg; nano-flaky carbon-containing phytolith powder: 130Kg-350Kg; ferrous oxide: 30Kg-60Kg; defoaming agent: 20Kg-40Kg; and blending agent: 0.015Kg-0.025Kg.

2. The special steel bar anticorrosive paint for aerated concrete plate according to claim 1, characterized in that: The styrene butadiene latex series includes one of styrene butadiene latex, carboxylated styrene butadiene rubber and carboxylated styrene butadiene latex.

3. The special steel bar anticorrosive paint for aerated concrete plate according to claim 1, characterized in that: The nano-flaky carbonaceous phytolith powder is made from the newly discovered phytolith SiO2 ore in Fengcheng, Jiangxi Province. It is sieved with 200 mesh, calcined at 400-650 degrees without oxygen, and then ball-milled to obtain a SiO2 content of 85-90%, a carbon content of 5-10%, a FeO content of 1-3%, a flake diameter-to-thickness ratio of 5-20, and a particle size of 300 nanometers-5μm.

4. The special steel anticorrosion paint for aerated concrete plate according to claim 1, characterized in that: The ferrous oxide is CAS No.: 1345-25-1.

5. The special steel bar anticorrosive paint for aerated concrete plate according to claim 1, characterized in that: The defoaming agent is octanol or 2-ethylhexanol.

6. The special steel bar anticorrosive paint for aerated concrete plate according to claim 1, characterized in that: The conditioning agent is sodium tetraborate decahydrate.

7. A method for producing a special steel anticorrosion paint for aerated concrete plates, according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, weigh the following raw materials according to mass ratio: styrene-butadiene latex series: 600Kg-800Kg; nano-flaky carbonaceous phytolith powder: 130Kg-350Kg; ferrous oxide: 30Kg-60Kg; defoaming agent: 20Kg-40Kg; blending agent: 0.015Kg-0.025Kg; S2, pour the styrene-butadiene latex series into a special stirring tank, stir for 5-30 minutes, gradually pour the phytolith SiO2 powder into the stirring tank, and stir for 5-30 minutes; S3, add defoamer and continue stirring; S4, after the generated ammonia smell is exhausted, slowly add ferrous oxide and continue stirring for 5-30 minutes to completely disperse the ferrous oxide; S5, finally add the blending agent and stir until evenly mixed to obtain the special steel anti-corrosion paint for aerated concrete panels.