Preparation method of polyurea material

By combining modified mesoporous silica and modified polyacrylate, the hydrophobicity and adhesion of polyurea materials are enhanced, solving the problems of insufficient water resistance and adhesion of polyurea materials, and achieving better mechanical properties and protective effects.

CN119019921AInactive Publication Date: 2024-11-26QINGDAO AODAWEI ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411285651.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyurea materials generally have poor water resistance and low adhesion to substrates, and existing modification methods are insufficient to simultaneously improve mechanical properties and water resistance.

Method used

Polyurea materials were prepared by treating mesoporous silica with ethanolamine and silane coupling agents, and then combining them with enoneimine and triphenylsilyl alcohol to modify polyacrylate, thereby enhancing their hydrophobicity and adhesion.

Benefits of technology

It improves the hydrophobicity and adhesion of polyurea materials, enhances their waterproof, oil-proof, and stain-proof properties, improves their mechanical strength and compressive strength, and reduces the possibility of the material peeling off from the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043044960000111
    Figure BDA0005043044960000111
  • Figure FDA0005043044950000021
    Figure FDA0005043044950000021
Patent Text Reader

Abstract

The present invention relates to the technical field of polyurea materials, particularly to a polyurea material preparation method, which comprises: 1, heating polyether polyol and modified mesoporous silica to a temperature of 110-120 DEG C, carrying out dehydration under a vacuum condition, cooling to a temperature of 65-80 DEG C, adding polyisocyanate, and carrying out a heat preservation reaction for 1-2 h to obtain a component A; step 2, mixing modified polyacrylate, a solvent, a leveling aid and a defoaming aid, and uniformly stirring to obtain a component B; and step 3, uniformly mixing the component A and the component B according to a weight ratio, and reacting for 4-6 hours under the condition of 70-90 DEG C to obtain a reaction product. According to the preparation method of the polyurea material, the modified mesoporous silica is added, so that the hydrophobic property of the polyurea material is improved, and when organic components permeate into mesopores of the modified mesoporous silica and are cured, the hydrophobic property of the polyurea material is improved; the overall strength of the polyurea material can be effectively improved, and the adhesive force of the polyurea material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurea materials, and in particular to a method for preparing a polyurea material. Background Art

[0002] One-component polyurea is a type of polyurea-containing compound that is generated by mixing an isocyanate component with a blocked amino compound, unblocking the blocked amino compound, and reacting the unblocked amine group with isocyanate. Polyurea is a dense elastomeric substance containing a large number of highly polar polyurea groups and hydrogen bonds. It has the characteristics of corrosion resistance, waterproofness, and wear resistance. Therefore, it has a wide range of applications in the fields of waterproofing, corrosion resistance, anti-wear, and surface decoration. One-component polyurea does not require additional mixing and mixing during use, and can be directly applied. It has the advantages of simple and convenient construction and excellent physical and chemical properties.

[0003] However, polyurea also has some disadvantages. Problems such as general water resistance and low adhesion to substrates have always restricted the application of polyurea. In order to improve the water resistance and surface hydrophobicity of polyurea materials, researchers often use hydroxy silicone oil (PDMS) with excellent water resistance, heat resistance and chemical resistance to modify them. However, the modified polyurea either has good water resistance but poor mechanical properties, or good mechanical properties but poor water resistance. Therefore, we proposed a preparation method of polyurea material to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a polyurea material.

[0005] A method for preparing a polyurea material comprises the following steps:

[0006] Step 1, heating the polyether polyol and modified mesoporous silica to 110-120° C., dehydrating under vacuum conditions, then cooling to 65-80° C., adding polyisocyanate, and keeping the temperature for reaction for 1-2 hours to obtain component A;

[0007] Step 2, mixing the modified polyacrylate, the solvent, the leveling agent and the defoaming agent and stirring them evenly to obtain component B;

[0008] Step 3, mixing component A and component B uniformly according to the weight ratio, reacting at 70-90° C. for 4-6 hours to obtain a reaction product;

[0009] The weight ratio of the polyether polyol, modified mesoporous silica and polyisocyanate is 50:8-12:30-60;

[0010] The weight ratio of the modified polyacrylate, the solvent, the leveling agent and the defoaming agent is 50:10-14:0.3-2:0.1-2;

[0011] The weight ratio of the component A to the component B is 1:0.3-0.5.

[0012] Preferably, the preparation method of the modified mesoporous silica comprises the following steps: mixing mesoporous silica and ethanolamine in a mass ratio of 1:0.8 to 1.2, then mixing with an ethanol solution and ultrasonically dispersing for 1 hour, adding an appropriate amount of silane coupling agent, ultrasonically dispersing for 5 minutes, transferring the mixed solution to a flask, heating in a water bath at 65 to 75°C, condensing and refluxing for 2 to 4 hours, filtering and washing the mesoporous silica powder, and drying to obtain the modified mesoporous silica powder.

[0013] Preferably, the particle size of the mesoporous silica is 200-400 nm, and the particle size of the mesoporous silica is 10-20 nm.

[0014] Preferably, the modified polyacrylate is obtained by reacting polyacrylate, keteneimine, triphenylsilanol and acrylate monomers, wherein the weight ratio of polyacrylate, keteneimine, triphenylsilanol and acrylate is 50:8-12:6-9:12-15.

[0015] Preferably, the general formula of the ketene imine is: Wherein R1 is an alkane, R2 and R3 are aromatic hydrocarbons, and at least one of R2 and R3 is a fluorine-containing aromatic hydrocarbon.

[0016] Preferably, the acrylic acid ester monomer is one or more of methyl methacrylate, butyl methacrylate, butyl acrylate, methyl acrylate, isooctyl acrylate, isopentyl acrylate and glycidyl acrylate.

[0017] Preferably, the preparation method of the modified polyacrylate comprises the following steps: firstly mixing polyacrylate, ketene imine and acrylate monomer, stirring for 1 to 2 hours at a temperature of 20 to 30° C. to carry out a preliminary reaction, then adding triphenylsilanol, heating to 40 to 55° C., and continuing stirring for 40 to 60 minutes to obtain the modified polyacrylate.

[0018] Preferably, the polyisocyanate is one or more of hexamethylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and toluene diisocyanate; the polyether polyol is one or more of polyethylene glycol ether, polypropylene glycol ether, polyglycerol ether, polypentaerythritol ether, and polytetramethylene ether diol.

[0019] Preferably, the leveling aid is one of a polyacrylate leveling agent, a polyester leveling agent, a fluorine-modified polyacrylate leveling agent, and a silicone leveling agent, and the solvent is cyclohexanone, n-butanol, N,N-dimethylacetamide or toluene.

[0020] The beneficial effects of the present invention are:

[0021] 1. The preparation method of the polyurea material proposed in the present invention adds modified mesoporous silica, and the mesoporous silica has good hydrophobicity after being modified by ethanolamine and silane coupling agent, thereby improving the hydrophobicity of the polyurea material. The modified mesoporous silica has good binding property with the organic component. When the organic component penetrates into the mesopores of the modified mesoporous silica and solidifies, the overall strength of the polyurea material can be effectively improved, and the adhesion of the polyurea material is improved.

[0022] 2. The preparation method of the polyurea material proposed in the present invention adds modified polyacrylate, wherein the modified polyacrylate contains ketene imine and triphenylsilanol. The fluorocarbon part of ketene imine can effectively improve the waterproof, oil-proof and anti-fouling properties of the polyurea material. Triphenylsilanol can improve the waterproof performance of the polyurea material to a certain extent. The end of triphenylsilanol has three benzene rings, and the end of ketene imine has two benzene rings, and there is a large gap between the benzene rings, so that the polyurea material has a certain anti-compression performance. After the polyurea material is subjected to external force, it is not easy to peel off from the substrate, which further improves the adhesion of the polyurea material. DETAILED DESCRIPTION

[0023] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.

[0024] Some experimental reagents: cyclohexanone, n-butanol, N,N-dimethylacetamide, toluene, hexamethylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, toluene diisocyanate, polyethylene glycol ether, polypropylene glycol ether, polypropylene glycol ether, polypentaerythritol ether and polytetramethylene ether diol were purchased from Wanhua Chemical Group Co., Ltd.; methyl methacrylate, butyl methacrylate, butyl acrylate, methyl acrylate, isooctyl acrylate, isoamyl acrylate and glycidyl acrylate were purchased from Nanjing Gucai New Materials Technology Co., Ltd.; mesoporous silica was purchased from Hubei Huifu Nanomaterials Co., Ltd.; silane coupling agents (KH570, KH590) were purchased from Shandong Huachen New Materials Co., Ltd.; leveling agents and defoaming agents were purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0025] In Example 1, a method for preparing a polyurea material comprises the following steps:

[0026] Step 1, heating the polyether polyol and modified mesoporous silica to 110° C., dehydrating under vacuum conditions, then cooling to 65° C., adding polyisocyanate, and keeping the temperature for reaction for 1 hour to obtain component A;

[0027] Step 2, mixing the modified polyacrylate, the solvent, the leveling agent and the defoaming agent and stirring them evenly to obtain component B;

[0028] Step 3, mixing component A and component B uniformly according to the weight ratio, reacting at 70° C. for 4 hours to obtain a reaction product;

[0029] The weight ratio of polyether polyol, modified mesoporous silica and polyisocyanate is 50:8:30;

[0030] The weight ratio of modified polyacrylate, solvent, leveling agent and defoaming agent is 50:10:0.3:0.1;

[0031] The weight ratio of component A to component B is 1:0.3.

[0032] The preparation method of modified mesoporous silica comprises the following steps: mixing mesoporous silica and ethanolamine in a mass ratio of 1:0.8, then mixing with an ethanol solution and ultrasonically dispersing for 1 hour, adding an appropriate amount of silane coupling agent, ultrasonically dispersing for 5 minutes, transferring the mixed solution to a flask, heating in a water bath at 65° C., condensing and refluxing for 2 hours, filtering and washing the mesoporous silica powder, and drying to obtain the modified mesoporous silica powder.

[0033] The particle size of the mesoporous silica is 200 to 400 nm, and the particle size of the mesoporous silica is 10 to 20 nm.

[0034] The modified polyacrylate is obtained by reacting polyacrylate, ketene imine, triphenylsilanol and acrylate monomers, wherein the weight ratio of polyacrylate, ketene imine, triphenylsilanol and acrylate is 50:8:6:12.

[0035] The general formula of ketene imine is: Wherein R1 is an alkane, R2 and R3 are aromatic hydrocarbons, and at least one of R2 and R3 is a fluorine-containing aromatic hydrocarbon.

[0036] The acrylate monomer is methyl methacrylate.

[0037] The preparation method of modified polyacrylate comprises the following steps: firstly, polyacrylate, ketene imine and acrylate monomer are mixed, stirred for 1 hour at a temperature of 20°C to carry out a preliminary reaction, and then triphenylsilanol is added, the temperature is raised to 40°C, and stirring is continued for 40 minutes to obtain modified polyacrylate.

[0038] The polyisocyanate is hexamethylene diisocyanate; and the polyether polyol is polyethylene glycol ether.

[0039] The leveling agent is a polyacrylate leveling agent, and the solvent is cyclohexanone.

[0040] In Example 2, a method for preparing a polyurea material comprises the following steps:

[0041] Step 1, heating the polyether polyol and modified mesoporous silica to 120° C., dehydrating under vacuum conditions, then cooling to 80° C., adding polyisocyanate, and keeping the temperature for reaction for 2 hours to obtain component A;

[0042] Step 2, mixing the modified polyacrylate, the solvent, the leveling agent and the defoaming agent and stirring them evenly to obtain component B;

[0043] Step 3, mixing component A and component B uniformly according to the weight ratio, reacting at 90° C. for 6 hours to obtain a reaction product;

[0044] The weight ratio of polyether polyol, modified mesoporous silica and polyisocyanate is 50:12:60;

[0045] The weight ratio of modified polyacrylate, solvent, leveling agent and defoaming agent is 50:14:2:2;

[0046] The weight ratio of component A to component B is 1:0.5.

[0047] The preparation method of modified mesoporous silica comprises the following steps: mixing mesoporous silica and ethanolamine in a mass ratio of 1:1.2, then mixing with an ethanol solution and ultrasonically dispersing for 1 hour, adding an appropriate amount of silane coupling agent, ultrasonically dispersing for 5 minutes, transferring the mixed solution to a flask, heating in a water bath at 75°C, condensing and refluxing for 4 hours, filtering and washing the mesoporous silica powder, and drying to obtain the modified mesoporous silica powder.

[0048] The particle size of the mesoporous silica is 200 to 400 nm, and the particle size of the mesoporous silica is 10 to 20 nm.

[0049] The modified polyacrylate is obtained by reacting polyacrylate, keteneimine, triphenylsilanol and acrylate monomers, wherein the weight ratio of polyacrylate, keteneimine, triphenylsilanol and acrylate is 50:12:9:15.

[0050] The general formula of ketene imine is: Wherein R1 is an alkane, R2 and R3 are aromatic hydrocarbons, and at least one of R2 and R3 is a fluorine-containing aromatic hydrocarbon.

[0051] The acrylate monomer is butyl methacrylate.

[0052] The preparation method of modified polyacrylate comprises the following steps: firstly, polyacrylate, ketene imine and acrylate monomer are mixed, stirred for 2 hours at a temperature of 30°C to carry out a preliminary reaction, and then triphenylsilanol is added, the temperature is raised to 55°C, and stirring is continued for 60 minutes to obtain modified polyacrylate.

[0053] The polyisocyanate is diphenylmethane diisocyanate.

[0054] The leveling agent is an organic silicon leveling agent and the solvent is toluene.

[0055] In Example 3, a method for preparing a polyurea material comprises the following steps:

[0056] Step 1, heating the polyether polyol and modified mesoporous silica to 115° C., dehydrating under vacuum conditions, then cooling to 70° C., adding polyisocyanate, and keeping the temperature for reaction for 1.5 hours to obtain component A;

[0057] Step 2, mixing the modified polyacrylate, the solvent, the leveling agent and the defoaming agent and stirring them evenly to obtain component B;

[0058] Step 3, mixing component A and component B uniformly according to the weight ratio, reacting at 80° C. for 5 hours to obtain a reaction product;

[0059] The weight ratio of polyether polyol, modified mesoporous silica and polyisocyanate is 50:10:40;

[0060] The weight ratio of modified polyacrylate, solvent, leveling agent and defoaming agent is 50:12:1.5:1.2;

[0061] The weight ratio of component A to component B is 1:0.4.

[0062] The preparation method of modified mesoporous silica comprises the following steps: mixing mesoporous silica and ethanolamine in a mass ratio of 1:1, then mixing with an ethanol solution and ultrasonically dispersing for 1 hour, adding an appropriate amount of silane coupling agent, ultrasonically dispersing for 5 minutes, transferring the mixed solution to a flask, heating in a water bath at 70°C, condensing and refluxing for 3 hours, filtering and washing the mesoporous silica powder, and drying to obtain the modified mesoporous silica powder.

[0063] The particle size of the mesoporous silica is 200 to 400 nm, and the particle size of the mesoporous silica is 10 to 20 nm.

[0064] The modified polyacrylate is obtained by reacting polyacrylate, ketene imine, triphenylsilanol and acrylate monomers, wherein the weight ratio of polyacrylate, ketene imine, triphenylsilanol and acrylate is 50:10:7:14.

[0065] The general formula of ketene imine is: Wherein R1 is an alkane, R2 and R3 are aromatic hydrocarbons, and at least one of R2 and R3 is a fluorine-containing aromatic hydrocarbon.

[0066] The acrylic acid ester monomer is one or more of methyl methacrylate, butyl methacrylate, butyl acrylate, methyl acrylate, isooctyl acrylate, isopentyl acrylate and glycidyl acrylate.

[0067] The preparation method of modified polyacrylate comprises the following steps: firstly, polyacrylate, ketene imine and acrylate monomer are mixed, stirred for 1.2 hours at a temperature of 25°C to carry out a preliminary reaction, and then triphenylsilanol is added, the temperature is raised to 50°C, and stirring is continued for 50 minutes to obtain modified polyacrylate.

[0068] The polyisocyanate is one or more of toluene diisocyanate; polyether polyol polyglycerol ether.

[0069] The leveling agent is a fluorine-modified polyacrylate leveling agent, and the solvent is n-butanol.

[0070] In Examples 1-3, the acrylate monomer is one or more of methyl methacrylate, butyl methacrylate, butyl acrylate, methyl acrylate, isooctyl acrylate, isopentyl acrylate and glycidyl acrylate.

[0071] The polyisocyanate is one or more of hexamethylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and toluene diisocyanate; the polyether polyol is one or more of polyethylene glycol ether, polypropylene glycol ether, polyglycerol ether, polypentaerythritol ether, and polytetramethylene ether diol.

[0072] The leveling agent is one of polyacrylate leveling agent, polyester leveling agent, fluorine-modified polyacrylate leveling agent and silicone leveling agent, and the solvent is cyclohexanone, n-butanol, N,N-dimethylacetamide or toluene.

[0073] In Comparative Example 1, compared with Example 3, modified mesoporous silica was not added in Step 1, and the rest was the same as Example 3.

[0074] In Comparative Example 2, compared with Example 3, an equal mass of unmodified mesoporous silica is added in step 1 instead of modified mesoporous silica, and the rest is the same as Example 3.

[0075] In Comparative Example 3, compared with Example 3, modified polyacrylate was not added in Step 2, and the rest was the same as Example 3.

[0076] In Comparative Example 4, compared with Example 3, when preparing the modified polyacrylate, ketene imine was not added, and the rest was the same as Example 3.

[0077] In Comparative Example 5, compared with Example 3, triphenylsilanol was not added when preparing the modified polyacrylate, and the rest was the same as Example 3.

[0078] The following is a performance test of the polyurea materials prepared in Examples 1-3 and Comparative Examples 1-5, and the test contents include elongation, tensile strength, adhesion, water impermeability and water resistance. The test methods for elongation, tensile strength and water impermeability are: GB / T16777-2008 "Test methods for building waterproof coatings"; the test method for adhesion is: GB / T5210-2006 "Adhesion test of paint and varnish pull-off method"; the substrate is ceramic tile; the test method for water resistance is: GB / T1733-1993 "Determination of water resistance of paint film", and the test environment humidity is 80%. The test results are shown in Table 1.

[0079] Table 1

[0080]

[0081] In Examples 1-3, the tensile strength, adhesion and elongation are relatively high, and the water impermeability and water resistance are good; in Comparative Example 1, the water impermeability and water resistance are good, and the elongation, tensile strength and adhesion are significantly reduced; in Comparative Example 2, the water impermeability and water resistance are good, and the elongation, tensile strength and adhesion are reduced to a certain extent, which is better than Comparative Example 1; in Comparative Example 3, the water impermeability and water resistance are significantly reduced, the elongation is also significantly reduced, and the tensile strength and adhesion are reduced to a certain extent; in Comparative Example 4, the water impermeability and water resistance are reduced to a certain extent, the elongation is reduced to a certain extent, and the tensile strength and adhesion are better than Comparative Example 3; in Comparative Example 5, the water impermeability and water resistance are reduced to a certain extent, the elongation is reduced to a certain extent, and the tensile strength and adhesion are better than Comparative Example 3.

[0082] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a polyurea material, characterized in that: The following steps are involved: Step 1, heating the polyether polyol and modified mesoporous silica to 110-120° C., dehydrating under vacuum conditions, then cooling to 65-80° C., adding polyisocyanate, and keeping the temperature for reaction for 1-2 hours to obtain component A; Step 2, mixing the modified polyacrylate, the solvent, the leveling agent and the defoaming agent and stirring them evenly to obtain component B; Step 3, mixing component A and component B uniformly according to the weight ratio, reacting at 70-90° C. for 4-6 hours to obtain a reaction product; The weight ratio of the polyether polyol, modified mesoporous silica and polyisocyanate is 50:8-12:30-60; The weight ratio of the modified polyacrylate, the solvent, the leveling agent and the defoaming agent is 50:10-14:0.3-2:0.1-2; The weight ratio of the component A to the component B is 1:0.3-0.

5.

2. The method for preparing a polyurea material according to claim 1, characterized in that: The preparation method of the modified mesoporous silica comprises the following steps: mixing mesoporous silica and ethanolamine in a mass ratio of 1:0.8-1.2, then mixing with an ethanol solution and ultrasonically dispersing for 1 hour, adding an appropriate amount of silane coupling agent, ultrasonically dispersing for 5 minutes, transferring the mixed solution to a flask, heating in a water bath at 65-75° C., condensing and refluxing for 2-4 hours, filtering and washing the mesoporous silica powder, and drying to obtain the modified mesoporous silica powder.

3. The method for preparing a polyurea material according to claim 2, characterized in that: The particle size of the mesoporous silica is 200-400 nm, and the particle size of the mesoporous silica is 10-20 nm.

4. The method for preparing a polyurea material according to claim 3, characterized in that: The modified polyacrylate is obtained by reacting polyacrylate, ketene imine, triphenylsilanol and acrylate monomers, wherein the weight ratio of polyacrylate, ketene imine, triphenylsilanol and acrylate is 50:8-12:6-9:12-15.

5. The method for preparing a polyurea material according to claim 4, characterized in that: The general formula of the ketene imine is: Wherein R1 is an alkane, R2 and R3 are aromatic hydrocarbons, and at least one of R2 and R3 is a fluorine-containing aromatic hydrocarbon.

6. The method for preparing a polyurea material according to claim 5, characterized in that: The acrylic acid ester monomer is one or more of methyl methacrylate, butyl methacrylate, butyl acrylate, methyl acrylate, isooctyl acrylate, isopentyl acrylate and glycidyl acrylate.

7. The method for preparing a polyurea material according to claim 6, characterized in that: The preparation method of the modified polyacrylate comprises the following steps: firstly, polyacrylate, ketene imine and acrylate monomer are mixed, stirred for 1 to 2 hours at a temperature of 20 to 30° C. to carry out a preliminary reaction, then triphenylsilanol is added, the temperature is raised to 40 to 55° C., and stirring is continued for 40 to 60 minutes to obtain the modified polyacrylate.

8. The method for preparing a polyurea material according to claim 1 or 7, characterized in that: The polyisocyanate is one or more of hexamethylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and toluene diisocyanate; the polyether polyol is one or more of polyethylene glycol ether, polypropylene glycol ether, polyglycerol ether, polypentaerythritol ether, and polytetramethylene ether diol.

9. The method for preparing a polyurea material according to claim 8, characterized in that: The leveling agent is one of a polyacrylate leveling agent, a polyester leveling agent, a fluorine-modified polyacrylate leveling agent, and a silicone leveling agent, and the solvent is cyclohexanone, n-butanol, N,N-dimethylacetamide or toluene.

Citation Information

Cited By

  • Self-repairing type polyurea protective coating and preparation method thereof

    CN121108853A