Diatomite / chitosan composite material modified asphalt paint and preparation method thereof

Through the modified asphalt paint of diatomaceous earth/chitosan composite material, the problem of poor adhesion and flexibility of asphalt paint on the metal surface is solved, better metal adhesion, drying speed and leveling performance are achieved, and the asphalt paint is improved overall performance.

CN119019934AActive Publication Date: 2024-11-26PANJIN NORTHERN ASPHALT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411183824.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing asphalt paint has poor adhesion and flexibility on the metal surface, which is prone to peel off, resulting in corrosion of metal materials, limiting its promotion and application.

Method used

The diatomaceous earth/chitosan composite is prepared by ultrasonic wave to modify the asphalt paint to improve adhesion ability, film formation thickness and leveling performance, and speed up the drying speed.

Benefits of technology

It significantly improves the metal adhesion, flexibility and drying speed of asphalt paint, reduces pore shrinkage, and increases film formation thickness and viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012962940000041
    Figure BDA0005012962940000041
  • Figure BDA0005012962940000061
    Figure BDA0005012962940000061
Patent Text Reader

Abstract

The invention belongs to the technical field of metal anti-corrosion paint, and discloses diatomite / chitosan composite material modified asphalt paint and a preparation method thereof. The modified asphalt paint is prepared by taking petroleum asphalt as a main raw material, taking a mixture of xylene and 200 # solvent oil as a solvent, adding a diatomite / chitosan composite material for modification, adding boiled tung oil, a drier and a dispersing agent, and stirring and mixing at low temperature. The asphalt paint provided by the invention not only can obviously improve the adhesion ability, film-forming thickness and leveling performance of the asphalt paint on the metal surface, but also has good drying speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal anticorrosive paints, and in particular relates to a diatomaceous earth / chitosan composite material modified asphalt paint and a preparation method thereof. Background Art

[0002] With the widespread application of metal materials in various industries, the corrosion problem has become increasingly prominent, causing huge economic losses. Metal anti-corrosion paint is one of the most effective measures for corrosion protection of metal substrates by isolating metals from corrosive substances and effectively cutting off the corrosion circuit. Asphalt paint, as a metal anti-corrosion paint, has good water resistance, acid resistance, alkali resistance and chemical resistance. It is mainly used for metal materials corresponding to equipment indoors, underwater, underground and not exposed to sunlight. However, pure asphalt paint has poor metal adhesion and flexibility. It is easy to peel off after long-term use, loses its protective effect, causes local corrosion of metal materials, and limits its promotion and application. Adding drying vegetable oil or alkyd resin to asphalt paint can improve adhesion and flexibility, but the drying speed will be affected and reduced. At the same time, the paint film formed by asphalt paint has shrinkage holes, and additional leveling agent needs to be added to improve the leveling of asphalt paint. Summary of the invention

[0003] In view of this, in order to solve this problem, the present invention provides a diatomite / chitosan composite material modified asphalt paint and a preparation method thereof. The present invention uses ultrasound to prepare a diatomite / chitosan composite material (wherein ultrasound can quickly and efficiently disperse solid materials such as diatomite and chitosan in a solution to accelerate the reaction process of the composite material), and the prepared diatomite / chitosan composite material modified asphalt paint can not only significantly improve the adhesion ability, film thickness and leveling performance of the asphalt paint on the metal surface, but also has a good drying speed.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] The first technical purpose of the present invention is to provide a diatomaceous earth / chitosan composite material, which is made of the following raw materials in parts by weight:

[0006] Diatomaceous earth: 5-15 parts;

[0007] Silane coupling agent: 5-15 parts;

[0008] Ethanol aqueous solution: 150-200 parts;

[0009] Acetic acid: 0.5-2 parts;

[0010] Chitosan: 0.1-0.3 parts.

[0011] Furthermore, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or γ-glycidyloxypropyltrimethoxysilane, preferably γ-methacryloxypropyltrimethoxysilane, because compared with the other two silane coupling agents, its polarity is weaker, closer to the polarity of petroleum asphalt, and it is more soluble in organic solvents with weaker polarity such as xylene and solvent oil, so it can improve the dispersion stability of diatomaceous earth / chitosan composite materials in asphalt paint.

[0012] Furthermore, the mass fraction of the ethanol solution is 40-80%, preferably 45-55%.

[0013] Furthermore, the molecular weight of the chitosan is 30,000-100,000, preferably 30,000. Chitosan with a lower molecular weight is more easily dissolved in an acetic acid-containing solution, which helps the non-covalent complexing of chitosan and diatomaceous earth through the surface.

[0014] Furthermore, the preparation method of the diatomite / chitosan composite material is as follows:

[0015] Step 1, calcining diatomite in a muffle furnace at 450° C. for 3 h, cooling to room temperature, adding to an ethanol aqueous solution, then adding acetic acid, and stirring at 60° C. for 0.5-1 h to obtain an acidified diatomite dispersion.

[0016] Step 2: Add silane coupling agent and chitosan to the acidified diatomite dispersion, perform ultrasonic treatment at 80° C. for 2 h, and then filter and dry to obtain a diatomite / chitosan composite material.

[0017] It should be noted that the diatomaceous earth needs to be calcined at high temperature (450° C.) to remove organic impurities and increase micropore permeability, which is beneficial to surface modification and compounding with other materials.

[0018] The second technical purpose of the present invention is to provide a diatomaceous earth / chitosan composite material modified asphalt paint, which is made of the following raw materials in parts by weight:

[0019] Petroleum asphalt: 50-60 parts;

[0020] Organic solvent: 40-50 parts;

[0021] Vegetable oil: 5-10 parts;

[0022] Diatomaceous earth / chitosan composite material: 2-5 parts;

[0023] Drier: 0.3-1.5 parts;

[0024] Dispersant: 0.05-0.2 parts.

[0025] Furthermore, the petroleum asphalt is No. 10 construction petroleum asphalt, preferably No. 10 construction petroleum asphalt with a softening point of 110-130°C.

[0026] Furthermore, the organic solvent is selected from one or more combinations of No. 100 solvent oil, No. 200 solvent oil, toluene, and xylene, preferably a mixture of No. 200 solvent oil and xylene in a weight ratio of 1:(0.5-4), preferably a weight ratio of 1:(1-3).

[0027] Furthermore, the vegetable oil is selected from one or more combinations of soybean oil, castor oil, rapeseed oil, linseed oil, and tung oil, preferably tung oil.

[0028] Furthermore, the drying agent is composed of lead tarate, cobalt tarate and zinc tarate in the following mass percentages: 20-30%, 20-30%, and 40-60%.

[0029] Furthermore, the dispersant is a phosphate ester dispersant or a polyurethane dispersant, preferably a phosphate ester dispersant, which has better compatibility with asphalt paint than the latter and is more conducive to the dispersion stability of the diatomaceous earth / chitosan composite material.

[0030] The third technical purpose of the present invention is to provide a method for preparing the modified asphalt paint, which specifically comprises the following steps:

[0031] Step 1: Crush the petroleum asphalt into particles, and dissolve it in an organic solvent by stirring at room temperature for 2-3 hours to obtain an unmodified asphalt paint mother liquor.

[0032] Step 2: Grind the diatomaceous earth / chitosan composite material into fine powder, add it into the unmodified asphalt paint mother liquid together with tung oil, dispersant and drying agent, and stir at 80-100° C. for 2-3 hours to obtain the modified asphalt paint.

[0033] By adopting the above technical solution, petroleum asphalt with a higher softening point is selected and crushed into particles, which can improve the heat resistance of asphalt paint and improve the solubility of petroleum asphalt in organic solvents, so that petroleum asphalt can be dissolved in organic solvents at room temperature. Chitosan itself has multiple hydroxyl groups and amino groups, which have strong chelating and adsorption capabilities with metal surfaces, so that the diatomaceous earth composited with chitosan can further improve the metal adhesion of asphalt paint. The porosity of diatomaceous earth can accelerate the volatilization of the solvent of the paint film and the speed of the oxidation drying reaction of vegetable oil, thereby accelerating the drying speed of asphalt paint. Diatomaceous earth modified by silane coupling agent can improve the wetting state of diatomaceous earth, thereby improving the leveling performance of asphalt paint. Dispersing diatomaceous earth / chitosan composite materials in asphalt paint can change its rheological properties, increase viscosity, and increase film thickness.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] By adding diatomaceous earth / chitosan composite materials, not only can the metal adhesion and flexibility of asphalt paint be significantly improved, but also the drying speed of the asphalt paint film can be accelerated, and its leveling performance can be improved to inhibit the formation of shrinkage holes. In addition, the addition of composite materials can increase the viscosity of asphalt paint and increase the film thickness. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0038] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0039] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0040] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0041] The invention discloses a diatomite / chitosan composite material and a preparation method of modified asphalt paint thereof.

[0042] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0043] (I) Preparation example of diatomite / chitosan composite material

[0044] The raw material compositions and proportions of Preparation Examples 1-7 are shown in Table 1.

[0045] Preparation Example 1-7 A method for preparing a diatomaceous earth / chitosan composite material is as follows:

[0046] Step 1, calcining diatomite in a muffle furnace at 450° C. for 3 h, cooling to room temperature, adding to an ethanol aqueous solution, then adding acetic acid, and stirring at 60° C. for 0.5 h to obtain an acidified diatomite dispersion.

[0047] Step 2: Add silane coupling agent γ-methacryloxypropyltrimethoxysilane (KH 570) and chitosan (MW=30000) to the acidified diatomite dispersion, perform ultrasonic treatment at 80° C. for 2 h, and then filter and dry to obtain a diatomite / chitosan composite material.

[0048] Table 1 Raw material composition and ratio of Preparation Examples 1-7

[0049]

[0050] (II) Preparation Example of Diatomaceous Earth / Chitosan Composite Material Modified Asphalt Paint

[0051] Example 1

[0052] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0053] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0054] Step 2: Grind 3 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 1 into fine powder, add it into the unmodified asphalt paint mother liquor together with 10 g of cooked tung oil, 0.05 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.21 g of cobalt tarate, 0.21 g of zinc tarate, and 0.28 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0055] Example 2

[0056] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0057] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0058] Step 2: Grind 5 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 2 into fine powder, add it into the unmodified asphalt paint mother liquor together with 10 g of cooked tung oil, 0.10 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.09 g of cobalt tarate, 0.09 g of zinc tarate, and 0.12 g of lead tarate, and stir at 100° C. for 3 h to obtain modified asphalt paint.

[0059] Example 3

[0060] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0061] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0062] Step 2: Grind 3 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 3 into fine powder, add it into the unmodified asphalt paint mother liquor together with 5 g of cooked tung oil, 0.05 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.09 g of cobalt tarate, 0.09 g of zinc tarate, and 0.12 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0063] Example 4

[0064] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0065] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0066] Step 2: Grind 5 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 4 into fine powder, add it into the unmodified asphalt paint mother liquor together with 10 g of cooked tung oil, 0.15 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.3 g of cobalt tarate, 0.3 g of zinc tarate, and 0.4 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0067] Example 5

[0068] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0069] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0070] Step 2: Grind 5 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 5 into fine powder, add it into the unmodified asphalt paint mother liquor together with 5 g of cooked tung oil, 0.05 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.09 g of cobalt tarate, 0.09 g of zinc tarate, and 0.12 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0071] Example 6

[0072] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0073] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0074] Step 2: Grind 3 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 6 into fine powder, add it into the unmodified asphalt paint mother liquor together with 5 g of cooked tung oil, 0.10 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.18 g of cobalt tarate, 0.18 g of zinc tarate, and 0.24 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0075] Example 7

[0076] This embodiment provides a diatomaceous earth / chitosan composite material modified asphalt paint, and the preparation method is as follows:

[0077] Step 1: Crush 50g of No. 10 construction petroleum asphalt into granules, and dissolve it in a mixed solvent of 8g of No. 200 solvent oil and 25g of xylene by stirring at room temperature for 2h to obtain an unmodified asphalt paint mother liquor.

[0078] Step 2: Grind 5 g of the diatomaceous earth / chitosan composite material obtained in Preparation Example 7 into fine powder, add it into the unmodified asphalt paint mother liquor together with 10 g of cooked tung oil, 0.05 g of phosphate dispersant (Evonik TEGO DISPERS 655), 0.18 g of cobalt tarate, 0.18 g of zinc tarate, and 0.24 g of lead tarate, and stir at 100°C for 3 h to obtain modified asphalt paint.

[0079] Comparative Example

[0080] 50 g of No. 10 construction petroleum asphalt was crushed into granules, and dissolved in a mixed solvent of 8 g of No. 200 solvent oil and 25 g of xylene by stirring at room temperature for 2 h to obtain unmodified asphalt paint.

[0081] The viscosity (GB / T 1723) of the asphalt paint of the comparative example and Examples 1-7, as well as the appearance, metal adhesion (GB / T 1720), flexibility (GB / T 1730) and actual drying time (GB / T 1728) of the asphalt paint of the comparative example and Examples 1-7 were measured. Generally, the greater the viscosity, the greater the film thickness. The appearance of the paint film is observed to see whether there is shrinkage cavitation. The more shrinkage cavities there are, the worse the leveling property is. The metal adhesion is observed by drawing circles on the paint film on the metal surface to observe the peeling of the paint film, which is divided into 1-7 levels. The smaller the level, the stronger the adhesion. The flexibility is performed by bending and deforming the metal test piece to different degrees using shaft rods of different diameters. The smaller the shaft rod diameter, the greater the degree of bending deformation. The damaged state of the paint film on the metal surface is observed. The test results are the minimum shaft rod diameter corresponding to the paint film without mesh, cracks and peeling. The smaller the minimum shaft rod diameter, the better the flexibility. The shorter the actual drying time, the faster the drying speed of the paint film. The test results of Examples 1-7 are shown in Table 2.

[0082] Table 2 Metal adhesion, flexibility and actual drying time of asphalt paint in Examples 1-7

[0083]

[0084]

[0085] The results show that adding diatomite / chitosan composite materials to prepare modified asphalt paint can significantly improve the film thickness, leveling performance, metal adhesion and drying speed of asphalt paint. The optimal performance effect can be achieved by regulating the preparation of diatomite / chitosan composite materials and the content of diatomite / chitosan composite materials, tung oil and drying agent in asphalt paint.

[0086] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A diatomaceous earth / chitosan composite material modified asphalt paint, characterized in that: The diatomite / chitosan composite material modified asphalt paint is made of the following raw materials in parts by weight: Petroleum asphalt: 50-60 parts; Organic solvent: 40-50 parts; Vegetable oil: 5-10 parts; Diatomaceous earth / chitosan composite material: 2-5 parts; Drier: 0.3-1.5 parts; Dispersant: 0.05-0.2 parts.

2. The diatomite / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The petroleum asphalt is No. 10 construction petroleum asphalt.

3. The diatomaceous earth / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The organic solvent is selected from one or more combinations of No. 100 solvent oil, No. 200 solvent oil, toluene and xylene.

4. The diatomaceous earth / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The vegetable oil is selected from one or more combinations of soybean oil, castor oil, rapeseed oil, linseed oil and tung oil.

5. The diatomite / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The drying agent is composed of lead tarate, cobalt tarate and zinc tarate in the following mass percentages: 20-30%, 20-30% and 40-60%.

6. The diatomite / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The dispersant is a phosphate ester dispersant or a polyurethane dispersant, preferably a phosphate ester dispersant.

7. The diatomaceous earth / chitosan composite material modified asphalt paint according to claim 1, characterized in that: The diatomaceous earth / chitosan composite material is made of the following raw materials in parts by weight: Diatomaceous earth: 5-15 parts; Silane coupling agent: 5-15 parts; Ethanol aqueous solution: 150-200 parts; Acetic acid: 0.5-2 parts; Chitosan: 0.1-0.3 parts; Furthermore, the preparation process of the diatomite / chitosan composite material is as follows: 1) calcining diatomite in a muffle furnace at 430-460° C. for 2-4 h, cooling to room temperature, adding to an ethanol aqueous solution, then adding acetic acid, stirring at 60-80° C. for 0.5-1 h to obtain an acidified diatomite dispersion; 2) Adding silane coupling agent and chitosan to the acidified diatomite dispersion obtained in step 1), ultrasonically treating at 60-80° C. for 1.5-2.5 h, and then filtering and drying to obtain the diatomite / chitosan composite material.

8. The diatomaceous earth / chitosan composite material modified asphalt paint according to claim 7, characterized in that: The silane coupling agent is selected from one or more combinations of γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidyloxypropyltrimethoxysilane.

9. The diatomite / chitosan composite material modified asphalt paint according to claim 7, characterized in that: The mass fraction of the ethanol solution is 40-80%, and the molecular weight of the chitosan is 30000-100000.

10. A method for preparing the diatomite / chitosan composite material modified asphalt paint as claimed in claim 1, characterized in that: The method specifically comprises the following steps: Step 1: crush petroleum asphalt into particles, dissolve in an organic solvent by stirring at room temperature for 2-3 hours to obtain an unmodified asphalt paint mother liquor; Step 2: Grind the diatomaceous earth / chitosan composite material into fine powder, add it into the unmodified asphalt paint mother liquor obtained in step 1 in sequence together with vegetable oil, dispersant and drying agent, and stir at 80-100° C. for 2-3 hours to obtain the modified asphalt paint.

Citation Information

Patent Citations

  • Preparation method of flame-retardant modified asphalt

    CN108892958A

  • Compounding double-modified asphalt mixture additive

    CN111847973A

  • Pelleting lime fines with asphalt enhancing binders and methods of use in asphalt manufacturing

    US20060260508A1