Packaging adhesive film and heterojunction battery assembly

By using a packaging film containing irradiation bridge agent and metal bonding agent in heterojunction solar cell modules, the problems of high silver paste cost and low adhesion are solved, and the adhesion and reliability of the components are improved. The amount of silver paste is reduced and bubble removal ability is enhanced.

CN119019945APending Publication Date: 2024-11-26HANGZHOU FIRST APPLIED MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411169307.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In mass production, heterojunction solar cell modules are limited by the high cost brought by high silver paste usage, and the adhesive force between the packaging film and the battery is low, resulting in easy delamination at high temperatures, affecting reliability.

Method used

Using a packaging film including an adhesive layer, a barrier layer and a support layer, the support layer contains an irradiation bridge agent and a metal bonding agent, which induces copolymerization through high-energy electron beam or ultraviolet radiation to form hydrogen bonds with metal oxides on the surface of the battery. Or coordination bonds to improve adhesion; the barrier layer consists of vinyl polyolefin resin, and the bridge agent and metal bonding agent in the barrier support layer migrate to the bond layer, preventing the bonding layer from being pre-crosslinked and ensuring good flow and bonding.

Benefits of technology

It improves the adhesion and reliability of heterojunction battery modules, reduces the risk of delamination between the packaging film and the battery, enhances the bubble removal ability and adhesion of the modules, reduces the amount of silver paste, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019945A_ABST
    Figure CN119019945A_ABST
Patent Text Reader

Abstract

The invention provides a packaging adhesive film and a heterojunction battery assembly. The packaging adhesive film comprises a bonding layer, a blocking layer and a supporting layer which are sequentially stacked, the blocking layer comprises vinyl polyolefin resin, the bonding layer and the supporting layer respectively and independently comprise ethylene-vinyl acetate copolymer, the supporting layer further comprises an irradiation bridging agent and a metal bonding agent, the irradiation bridging agent is a micromolecular monomer or polymer containing at least three acrylate groups, and the metal binding agent is a micromolecular monomer or polymer containing at least one olefinic double bond and at least one functional group; the functional group is selected from any one or more of an epoxy group, an isocyanate group, a siloxane group, a hydroxyl group, a carboxyl group, an anhydride group, a sulfydryl group and an amino group; the olefinic double bonds are selected from any one or more of vinyl, allyl, acrylate groups and methacrylate groups; and the pre-crosslinking degree of the supporting layer is 10-60%. The packaging adhesive film can solve the problem of poor reliability of a heterojunction battery assembly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging adhesive films, and in particular to a packaging adhesive film and a heterojunction battery assembly. Background Art

[0002] Heterojunction cells are the crystalline silicon solar cell route with the lowest carbon footprint due to their high photoelectric conversion efficiency, low temperature coefficient, good weak light response, thin film, and few process steps. However, the mass production of heterojunction solar cell modules is still limited by the high cost caused by the high amount of silver paste used. A main grid-free (0BB) technology has emerged in the industry, which uses copper wires with tin-lead plated on the surface to directly contact the secondary grid for conductivity. This can save a considerable amount of silver, but this physical contact is very easy to be damaged by the packaging material during the lamination process, causing poor contact. On the other hand, the surface of the heterojunction battery is metal oxide, and the packaging film has low adhesion to it. When the module is operated at high temperature, the packaging film is easy to delaminate from the battery, causing reliability risks. Summary of the invention

[0003] The main purpose of the present invention is to provide a packaging film and a heterojunction battery assembly to solve the problem of poor reliability of heterojunction battery assemblies in the prior art.

[0004] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a packaging film, which comprises an adhesive layer, a barrier layer and a support layer stacked in sequence, the barrier layer comprises a vinyl polyolefin resin, and the support layer comprises an irradiation bridging agent and a metal binder, wherein the irradiation bridging agent refers to a small molecule monomer or polymer containing at least three acrylate groups, and the metal binder refers to a small molecule monomer or polymer containing at least one olefinic double bond and at least one functional group, and the functional group is selected from any one or more of epoxy, isocyanate, siloxane, hydroxyl, carboxyl, anhydride, mercapto, and amino groups; the olefinic double bond is selected from any one or more of vinyl, allyl, acrylate, and methacrylate groups; and the pre-crosslinking degree of the support layer is 10 to 60%.

[0005] Further, the pre-crosslinking degree of the above-mentioned support layer is 30-50%; and / or, the thickness of the support layer is 30-200 μm; and / or, the above-mentioned support layer includes ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer in the support layer is 15-33wt%, and under the test conditions of 190°C and 2.16kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30g / 10min, preferably 1-15g / 10min; and / or, in parts by weight, the above-mentioned support layer includes: 100 parts of ethylene-vinyl acetate copolymer, 0.1-3 parts of irradiation bridging agent and 0.05-3 parts of metal binder.

[0006] Further, the above-mentioned radiation bridging agent is a multi-acrylate monomer and a polymer thereof, and the multi-acrylate monomer is preferably selected from any one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, ethoxylated pentaerythritol triacrylate, propoxylated pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated trimethylolpropane trimethacrylate, propoxylated trimethylolpropane trimethacrylate, and dipentaerythritol hexaacrylate.

[0007] Furthermore, the metal binder is selected from glycidyl methacrylate, maleic anhydride, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, butoxymethyl acrylamide, vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triisopropoxysilane, vinyl tri(β-methoxyethoxy)silane, acrylic acid, 3,4-epoxycyclohexylmethyl methacrylate, 3,4-epoxycyclohexyl methacrylate, 1,2-epoxy-4-vinylcyclohexane, glycidyl acrylate , tetrahydrofurfuryl methacrylate, tetrahydrofurfuryl acrylate, methacrylic acid, acrylamide, N-isopropylacrylamide, N-tert-butylacrylamide, N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacryloyl, N-(2-hydroxypropyl)methacrylamide, methacrylamide, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate, epoxy acrylate, allyl glycidyl ether, polyurethane acrylate and any one or more of epoxy resins with any double bonds.

[0008] Furthermore, the vinyl polyolefin resin in the barrier layer is an ethylene homopolymer or a copolymer of ethylene, propylene and α-olefin; the mole fraction of ethylene in the vinyl polyolefin resin is greater than 70%; the carbon number of the α-olefin is preferably 4 to 10, and under the test conditions of 190°C and 2.16kg, the melt index of the vinyl polyolefin resin is preferably 2 to 20g / 10min, and the melting point of the vinyl polyolefin resin is preferably 40 to 125°C; preferably, the thickness of the barrier layer is 50 to 250μm, and the molecular weight distribution index of the vinyl polyolefin resin is preferably less than 2.3.

[0009] Furthermore, the above-mentioned bonding layer includes ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer in the bonding layer is 15-33wt%, and under the test conditions of 190°C and 2.16kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30g / 10min; the bonding layer preferably also contains a silane coupling agent; the thickness of the bonding layer is preferably 30-250μm.

[0010] Furthermore, in parts by weight, the barrier layer and the bonding layer each independently include 0.1 to 2 parts of a first organic peroxide, the support layer also includes 0 to 2 parts of a second organic peroxide, and / or the support layer also includes 0 to 2 parts of a photoinitiator; wherein, preferably, the first organic peroxide and the second organic peroxide each independently include tert-butyl peroxide-2-ethylhexyl carbonate, tert-amyl peroxide-2-ethylhexyl carbonate, tert-hexyl peroxide-2-ethylhexyl carbonate, tert-butyl peroxide isopropyl carbonate, tert-butyl peroxide isobutyl carbonate, tert-amyl peroxide isopropyl carbonate, tert-amyl peroxide isobutyl carbonate, tert-butyl peroxide 2-ethylhexanoate, tert-butyl peroxide 3,5,5-trimethylhexanoate, tert-butyl peroxide 3,5 ,5-trimethylhexanoic acid tert-amyl ester, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)cyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, 1,1-bis(tert-butyl peroxy)cyclohexane, any one or more thereof; preferably, the photoinitiator is selected from any one or more of benzophenone and its derivatives, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl trimethylbenzoyl phenylphosphonate, 2-hydroxy-2-methyl-1-phenylacetone, 1-hydroxycyclohexyl phenyl ketone, and benzoin dimethyl ether.

[0011] Furthermore, at least one of the above-mentioned bonding layer, support layer or barrier layer contains an ultraviolet light conversion agent, and the ultraviolet light conversion agent is preferably selected from any one or more of organic fluorescent pigments, rare earth organic complexes, rare earth inorganic compounds, CdSe quantum dots, and perovskite quantum dots; preferably, the ultraviolet light conversion agent converts light with a wavelength of 300 to 400 nm into visible light with a wavelength greater than 400 nm.

[0012] Further, at least one of the above-mentioned adhesive layer, support layer or barrier layer contains an ultraviolet light absorber, and the ultraviolet light absorber is preferably selected from 2-hydroxy-4-octyloxybenzophenone, 2-cyano-3,3-diphenylacrylate, ethylhexyl p-methoxycinnamate, isooctyl p-methoxycinnamate, dimethyl 4-methoxybenzylidenemalonate, N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)-oxalamide, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3-[a,a-dimethylbenzyl]benzotriazole, Any one or more of 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-octyloxyphenol, 2-(2'-hydroxy-3',5'-bis(a,a-dimethylbenzyl)phenyl)benzotriazole, and polysiloxane-15.

[0013] According to another aspect of the present invention, a heterojunction battery assembly is provided, comprising a packaging film, wherein the packaging film is the aforementioned packaging film.

[0014] The technical scheme of the present invention is applied, and the irradiation bridging agent and metal binder containing the above specific functional groups are copolymerized by the free radicals generated during high-energy electron beam irradiation or ultraviolet irradiation, and cross-linked with the EVA copolymer, which helps to form hydrogen bonds or coordination bonds between the metal oxides on the surface of the heterojunction battery, thereby improving the adhesion between the support layer and the heterojunction battery, and then under high temperature operation, reducing the reliability risk caused by the easy delamination of the encapsulation film in the heterojunction battery assembly from the heterojunction battery. At the same time, the pre-crosslinked support layer has low fluidity, which can effectively support and fix the fitting of the circular welding wire and the fine grid line of the battery. In addition, the barrier layer of the present invention is composed of vinyl polyolefin resin, which has the effect of blocking the migration of the bridging agent and the metal binder in the support layer to the bonding layer, so that the bonding layer can be effectively prevented from being pre-crosslinked during the irradiation process, thereby ensuring that the bonding layer has good fluidity, ensuring good adhesion and exhaust between it and the front glass or back glass (back plate), helping to reduce the bubbles of the assembly, and improving the reliability of the heterojunction battery assembly. Controlling the pre-crosslinking degree of the support layer within the above range can make the support layer have both low fluidity and high adhesion. If the pre-crosslinking degree of the support layer is lower than 10%, when the encapsulation film is used at the subsequent component end, due to its high fluidity, the encapsulation film will flow between the welding wire and the battery, causing poor contact, thereby affecting the power of the photovoltaic component; if the pre-crosslinking degree of the support layer is higher than 60%, the adhesion between the encapsulation film and the heterojunction battery is relatively low. Therefore, controlling the pre-crosslinking degree of the support layer to be 10-60% can take into account both the fluidity and adhesion of the support layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0016] Figure 1 A schematic structural diagram of a heterojunction battery assembly provided according to Example 1 of the present invention is shown.

[0017] The above drawings include the following reference numerals:

[0018] 1. Front glass; 2. First bonding layer; 3. First barrier layer; 4. First support layer; 5. Silicon heterojunction cell; 6. Second support layer; 7. Second barrier layer; 8. Second bonding layer; 9. Polymer back panel or back glass. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0020] As analyzed in the background art, the heterojunction battery assembly in the prior art has the problem of poor reliability. To solve this problem, the present invention provides a packaging film and a heterojunction battery assembly.

[0021] In a typical embodiment of the present application, a packaging film is provided, which includes a bonding layer, a barrier layer and a support layer stacked in sequence, the barrier layer includes a vinyl polyolefin resin, and the support layer includes a radiation bridging agent and a metal binder, wherein the radiation bridging agent refers to a small molecule monomer or polymer containing at least three acrylate groups, and the metal binder refers to a small molecule monomer or polymer containing at least one olefinic double bond and at least one functional group, and the functional group is selected from any one or more of an epoxy group, an isocyanate group, a siloxane group, a hydroxyl group, a carboxyl group, an anhydride group, a thiol group, and an amino group; the olefinic double bond is selected from any one or more of a vinyl group, an allyl group, an acrylate group, and a methacrylate group; and the pre-crosslinking degree of the support layer is 10 to 60%.

[0022] The irradiation bridging agent and metal binder containing the above specific functional groups, the two are copolymerized by the free radicals generated during high-energy electron beam irradiation or ultraviolet irradiation, and cross-linked with the EVA copolymer, which helps to form hydrogen bonds or coordination bonds between the metal oxides on the surface of the heterojunction battery, thereby improving the adhesion between the support layer and the heterojunction battery, and then under high temperature operation, reducing the reliability risk caused by the easy delamination of the encapsulation film in the heterojunction battery assembly from the heterojunction battery. At the same time, the pre-crosslinked support layer has low fluidity, which can effectively support and fix the fitting of the circular welding wire and the fine grid line of the battery. In addition, the barrier layer of the present invention is composed of vinyl polyolefin resin, which has the effect of blocking the migration of the bridging agent and the metal binder in the support layer to the bonding layer, so that the bonding layer can be effectively prevented from being pre-crosslinked during the irradiation process, thereby ensuring that the bonding layer has good fluidity, ensuring good adhesion and exhaust between it and the front glass or back glass (back plate), helping to reduce the bubbles of the assembly, and improving the reliability of the heterojunction battery assembly. Controlling the pre-crosslinking degree of the support layer within the above range can make the support layer have both low fluidity and high adhesion. If the pre-crosslinking degree of the support layer is lower than 10%, when the encapsulation film is used at the subsequent component end, due to its high fluidity, the encapsulation film will flow between the welding wire and the battery, causing poor contact, thereby affecting the power of the photovoltaic component; if the pre-crosslinking degree of the support layer is higher than 60%, the adhesion between the encapsulation film and the heterojunction battery is relatively low. Therefore, controlling the pre-crosslinking degree of the support layer to be 10-60% can take into account both the fluidity and adhesion of the support layer.

[0023] In one embodiment of the present application, the pre-crosslinking degree of the support layer is 30-50%; and / or the thickness of the support layer is 30-200 μm; and / or the support layer comprises ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer in the support layer is 15-33 wt %, and under the test conditions of 190° C. and 2.16 kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30 g / 10 min, preferably 1-15 g / 10 min. And / or, in parts by weight, the support layer comprises 100 parts of ethylene-vinyl acetate copolymer, 0.1-3 parts of irradiation bridging agent, and 0.05-3 parts of metal binder.

[0024] The support layer with the above pre-crosslinking degree has lower fluidity, which can effectively prevent the adhesive from flowing between the welding wire and the battery during the component lamination process, thereby causing poor contact problems. Its low fluidity is achieved by pre-crosslinking. Specifically, the encapsulation film of the present invention forms a primary film by multi-layer co-extrusion, and then the support layer is pre-crosslinked by ultraviolet radiation or electron beam radiation, so that the support layer of the present application has low fluidity and high adhesion. The synergistic effect between the components with the above content is better, so that the bonding force between the support layer and the heterojunction battery is stronger. It is preferred to control the VA content and melt index of the ethylene-vinyl acetate copolymer within the above range, which is conducive to improving its polymerization reaction activity, thereby providing a certain strength for the encapsulation film after curing.

[0025] In one embodiment of the present application, the above-mentioned radiation bridging agent is a multi-acrylate monomer and a polymer thereof, and the multi-acrylate monomer is preferably selected from any one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, ethoxylated pentaerythritol triacrylate, propoxylated pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated trimethylolpropane trimethacrylate, propoxylated trimethylolpropane trimethacrylate, and dipentaerythritol hexaacrylate.

[0026] The above preferred irradiation bridging agent has more abundant functional groups, which is more conducive to exerting the synergistic effect between it and the functional groups in the metal binder, thereby making the two show better adhesion to the heterojunction battery.

[0027] In one embodiment of the present application, the metal binder is selected from glycidyl methacrylate, maleic anhydride, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, butoxymethyl acrylamide, vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triisopropoxysilane, vinyl tri(β-methoxyethoxy)silane, acrylic acid, 3,4-epoxycyclohexyl methyl methacrylate, 3,4-epoxycyclohexyl methacrylate, 1,2-epoxy-4-vinylcyclohexane, acrylic acid ... Any one or more of glycerol ester, tetrahydrofurfuryl methacrylate, tetrahydrofurfuryl acrylate, methacrylic acid, acrylamide, N-isopropylacrylamide, N-tert-butylacrylamide, N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacryloyl, N-(2-hydroxypropyl)methacrylamide, methacrylamide, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate, epoxy acrylate, allyl glycidyl ether, polyurethane acrylate and epoxy resin with any double bond.

[0028] The preferred above metal binder has a richer functional group, which is more conducive to the synergistic effect between it and the functional group in the irradiation bridging agent, so that the two show better adhesion to the heterojunction battery. In addition, the double bond group of the metal binder is bonded to the EVA macromolecular matrix during the irradiation process, and the functional group can increase the surface adhesion to the heterojunction battery. Further, the preferred metal binder of the present application is glycidyl methacrylate, and the preferred irradiation bridging agent is trimethylolpropane triacrylate. Under electron beam radiation or UV light radiation, the generated free radicals trigger the double bonds of trimethylolpropane triacrylate and the double bonds of glycidyl methacrylate to copolymerize, and the redundant double bonds of trihydroxypropane triacrylate are bonded to the EVA macromolecular matrix, playing the role of bridging crosslinking, so that the EVA matrix has a certain degree of pre-crosslinking. In the encapsulation lamination process, the epoxy group of glycidyl methacrylate is combined with the metal oxide on the surface of the heterojunction battery.

[0029] In one embodiment of the present application, the vinyl polyolefin resin in the barrier layer is an ethylene homopolymer or a copolymer of ethylene, propylene and α-olefin; the mole fraction of ethylene in the vinyl polyolefin resin is greater than 70%; the carbon number of the α-olefin is preferably 4 to 10, and under the test conditions of 190°C and 2.16kg, the melt index of the vinyl polyolefin resin is preferably 2 to 20 g / 10 min, and the melting point of the vinyl polyolefin resin is preferably 40 to 125°C; preferably, the thickness of the barrier layer is 50 to 250 μm, and the molecular weight distribution index of the vinyl polyolefin resin is preferably less than 2.3.

[0030] The above barrier layer preferably helps to reduce the water vapor entering the heterojunction battery assembly to corrode the heterojunction battery as much as possible, and can effectively prevent the mutual migration of the additives of the support layer and the adhesive layer. The thickness and molecular weight distribution index of the above barrier layer are preferably within the above range, which helps to further improve the water vapor barrier performance of the encapsulation film.

[0031] In one embodiment of the present application, the above-mentioned bonding layer includes ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer in the bonding layer is 15-33wt%, and under the test conditions of 190°C and 2.16kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30g / 10min; the bonding layer preferably also includes a silane coupling agent; the thickness of the bonding layer is preferably 30-250μm.

[0032] Preferably, the VA content and melt index of the above ethylene-vinyl acetate copolymer are within the above ranges, which is beneficial to improving its polymerization reaction activity, thereby providing more sufficient adhesion to the packaging film after curing. Preferably, the adhesive layer also contains a silane coupling agent and the thickness of the adhesive layer is controlled within the above range, which helps to further improve the adhesion of the packaging film after curing.

[0033] In one embodiment of the present application, the barrier layer and the bonding layer further independently include 0.1 to 2 parts of the first organic peroxide, the support layer further includes 0 to 2 parts of the second organic peroxide, and / or the support layer further includes 0 to 2 parts of a photoinitiator; wherein, preferably, the first organic peroxide and the second organic peroxide are each independently selected from tert-butyl peroxide-2-ethylhexyl carbonate, tert-amyl peroxide-2-ethylhexyl carbonate, tert-hexyl peroxide-2-ethylhexyl carbonate, tert-butyl peroxide isopropyl carbonate, tert-butyl peroxide isobutyl carbonate, tert-amyl peroxide isopropyl carbonate, tert-amyl peroxide isobutyl carbonate, tert-butyl peroxide 2-ethylhexanoate, tert-butyl peroxide 3,5,5-trimethylhexanoate, tert-butyl peroxide Any one or more of tert-amyl peroxy-3,5,5-trimethylhexanoate, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)cyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, and 1,1-bis(tert-butyl peroxy)cyclohexane; the photoinitiator is preferably selected from any one or more of benzophenone and its derivatives, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl trimethylbenzoylphenylphosphonate, 2-hydroxy-2-methyl-1-phenylacetone, 1-hydroxycyclohexyl phenyl ketone, and benzoin dimethyl ether.

[0034] The preferred organic peroxides above help to fully crosslink the encapsulation film during the lamination process and are not prone to yellowing. The preferred photoinitiators above help to quickly and efficiently initiate the pre-crosslinking of EVA and the copolymerization of the irradiation bridging agent and the metal binder during UV light irradiation.

[0035] In one embodiment of the present application, at least one of the above-mentioned bonding layer, support layer or barrier layer contains an ultraviolet light conversion agent, and the ultraviolet light conversion agent is preferably selected from any one or more of organic fluorescent pigments, rare earth organic complexes, rare earth inorganic compounds, CdSe quantum dots, and perovskite quantum dots; preferably, the ultraviolet light conversion agent converts light with a wavelength of 300 to 400 nm into visible light with a wavelength greater than 400 nm.

[0036] The above preferred ultraviolet light conversion agent helps to better convert ultraviolet light and convert light with a wavelength of 300 to 400 nm into visible light with a wavelength greater than 400 nm, thereby improving the photoelectric conversion efficiency of the heterojunction battery.

[0037] In order to delay the aging of the packaging film, in one embodiment of the present application, it is preferred that at least one of the above-mentioned adhesive layer, support layer or barrier layer contains a UV absorber, and the UV absorber is preferably selected from 2-hydroxy-4-octyloxybenzophenone, 2-cyano-3,3-diphenylacrylate, ethylhexyl p-methoxycinnamate, isooctyl p-methoxycinnamate, dimethyl 4-methoxybenzylidenemalonate, N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)-oxalamide, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3 -[a,a-dimethylbenzyl]-5-tert-octyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 3,5-di-tert-butyl-4-hydroxybenzoic acid hexadecyl, 2-(4,6-diphenyl-1,3,5-triazine-2)-5-n-hexaneoxyphenol, 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-octyloxyphenol, 2-(2'-hydroxy-3',5'bis(a,a-dimethylbenzyl)phenyl)benzotriazole, polysiloxane-15, or any one or more thereof.

[0038] In another typical embodiment of the present application, a heterojunction battery assembly is provided, comprising encapsulation films stacked in sequence, the encapsulation films being the encapsulation films described above.

[0039] The heterojunction battery in the above heterojunction battery assembly of the present application has no main grid, only fine grid. During the production process of the assembly, the battery cells are first connected in series with tinned copper wires. Unlike the conventional welding process, the copper wires are physically contacted and fixed with the fine grid lines on the front and back of the battery by liquid glue or other similar methods, and then a layer of the encapsulation film provided by the present invention is laid on both the front and back sides, with the upper surface being the front glass and the lower surface being the back glass or polymer backplane. At the lamination temperature (130-160°C) of the stacked assembly, the low-temperature alloy on the surface of the copper wire melts and chemically fuses with the fine grid of the battery to form a conductive path, thereby greatly reducing the silver paste consumption of the heterojunction battery and reducing the preparation cost of the heterojunction battery assembly. In addition, the encapsulation film has excellent adhesion to the heterojunction battery, which improves the reliability of the heterojunction battery assembly.

[0040] The beneficial effects of the present application will be described below in conjunction with specific embodiments and comparative examples.

[0041] Example 1

[0042] As attached Figure 1 As shown, this example provides a heterojunction battery assembly, which includes a front glass 1, a first adhesive layer 2, a first barrier layer 3, a first support layer 4, a silicon heterojunction battery 5, a second support layer 6, a second barrier layer 7, a second adhesive layer 8, a polymer back panel or a back glass 9 stacked on one side, wherein the first adhesive layer 2 and the second adhesive layer 8 have the same formula and performance, the first barrier layer 3 and the second barrier layer 7 have the same formula and performance, and the first support layer 4 and the second support layer 6 have the same formula and performance.

[0043] Formula of the first adhesive layer 1: 100 parts of EVA (VA content is 28wt%, melt index is 20g / 10min), 0.4 parts of γ-methacryloxypropyltrimethoxysilane, 0.7 parts of triallyl isocyanurate, 0.5 parts of tert-butyl peroxy-2-ethylhexyl carbonate, and 0.3 parts of ultraviolet light absorber 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole (Double Bond Chemical, CHISORB328);

[0044] The formula of the first barrier layer 2 is: 100 parts of ethylene-butene copolymer, wherein the molar fraction of ethylene is 95%, the melt index is 5 g / 10 min, the molecular weight distribution index is 2.0, and the melting point is 108° C.;

[0045] The formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28 wt%, melt index is 6 g / 10 min), 0.6 parts of trimethylolpropane triacrylate, 0.3 parts of glycidyl methacrylate, and 0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate.

[0046] After the three-layer formula is mixed evenly independently, it is plasticized by three independent screw extruders and then enters the T-die through a combiner to form a three-layer co-extruded packaging film. The first barrier layer 2 is in the middle, the thickness of the first barrier layer 2 is 150 microns, the thickness of the first support layer 3 is 100 microns, and the thickness of the first bonding layer 1 is 200 microns. The total thickness of the packaging film is 450 microns. The first support layer 3 of the prepared packaging film faces the radiation source and is irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV and the irradiation dosage is 100KGy. The first support layer 3 of the irradiated packaging film has a pre-crosslinking degree of 40%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%.

[0047] During the lamination process, the interconnecting wires of the heterojunction battery do not need to be welded in advance, but can be pre-fixed with glue. The supporting layer of the encapsulation film is closely attached to the battery surface and in direct contact with the welding wires, while the adhesive layer faces the glass or backplane to obtain a heterojunction battery assembly.

[0048] Example 2

[0049] The difference from Example 1 is that the electron beam irradiation dosage is 70 KGy, so that the first support layer 3 has a pre-crosslinking degree of 20%, and finally a heterojunction battery assembly is obtained.

[0050] Example 3

[0051] The difference from Example 1 is that the electron beam irradiation dosage is 115 KGy, so that the first support layer 3 has a pre-crosslinking degree of 50%, and finally a heterojunction battery assembly is obtained.

[0052] Example 4

[0053] The difference from Example 1 is that the electron beam irradiation dosage is 130 KGy, so that the first support layer 3 has a pre-crosslinking degree of 60%, and finally a heterojunction battery assembly is obtained.

[0054] Example 5

[0055] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 15wt%, melt index is 15g / 10min), 0.6 parts of trimethylolpropane triacrylate, 0.3 parts of glycidyl methacrylate, and 0.5 parts of peroxy-2-ethylhexyl tert-butyl carbonate. The first supporting layer 3 of the prepared packaging film faces the radiation source and is irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV, and the irradiation dosage is 100KGy. The first supporting layer 3 of the packaging film after irradiation has a pre-crosslinking degree of 38%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%, and finally a heterojunction battery assembly is obtained.

[0056] Example 6

[0057] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.3 parts of trimethylolpropane triacrylate, 3 parts of glycidyl methacrylate, and 0.5 parts of peroxy-2-ethylhexyl tert-butyl carbonate. The first supporting layer 3 of the prepared packaging film is facing the radiation source and irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV, and the irradiation dosage is 100KGy. The first supporting layer 3 of the packaging film after irradiation has a pre-crosslinking degree of 30%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%, and finally a heterojunction battery assembly is obtained.

[0058] Example 7

[0059] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.1 parts of trimethylolpropane triacrylate, 0.05 parts of glycidyl methacrylate, and 0.5 parts of peroxy-2-ethylhexyl tert-butyl carbonate. The first supporting layer 3 of the prepared packaging film faces the radiation source and is irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV, and the irradiation dosage is 100KGy. The first supporting layer 3 of the packaging film after irradiation has a pre-crosslinking degree of 10%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%, and finally a heterojunction battery assembly is obtained.

[0060] Example 8

[0061] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.6 parts of dipentaerythritol hexaacrylate, 0.3 parts of glycidyl methacrylate, and 0.5 parts of peroxy-2-ethylhexyl carbonate tert-butyl ester. The first supporting layer 3 of the prepared packaging film faces the radiation source and is irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV, and the irradiation dosage is 100KGy. The first supporting layer 3 of the packaging film after irradiation has a pre-crosslinking degree of 42%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%, and finally a heterojunction battery assembly is obtained.

[0062] Example 9

[0063] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.6 parts of trimethylolpropane triacrylate, 0.3 parts of methacrylic acid, and 0.5 parts of peroxy-2-ethylhexyl tert-butyl carbonate. The first supporting layer 3 of the prepared packaging film faces the radiation source and is irradiated with a high-energy electron beam. The energy of the electron beam is 150KeV, and the irradiation dosage is 100KGy. The first supporting layer 3 of the packaging film after irradiation has a pre-crosslinking degree of 41%, and the pre-crosslinking degrees of the first barrier layer 2 and the first bonding layer 1 are both less than 3%, and finally a heterojunction battery assembly is obtained.

[0064] Example 10

[0065] The difference from Example 1 is that the formula of the first barrier layer 2 is: 100 parts of ethylene and hexene copolymer, wherein the molar fraction of ethylene is 95%, the melt index is 20 g / 10 min, the molecular weight distribution index is 2.0, and the melting point is 98° C., and finally a heterojunction battery assembly is obtained.

[0066] Embodiment 11

[0067] The difference from Example 1 is that the formula of the first barrier layer 2 is: 100 parts of ethylene and octene copolymer, wherein the molar fraction of ethylene is 95%, the melt index is 1 g / 10 min, the molecular weight distribution index is 2.0, and the melting point is 98° C., and finally a heterojunction battery assembly is obtained.

[0068] Example 12

[0069] The difference from Example 1 is that the formula of the first bonding layer 1 is: 100 parts of EVA (VA content is 15wt%, melt index is 1g / 10min), 0.4 parts of γ-methacryloxypropyltrimethoxysilane, 0.7 parts of triallyl isocyanurate, 0.5 parts of tert-amyl peroxide-2-ethylhexyl carbonate, and 0.3 parts of ultraviolet light absorber 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole (Double Bond Chemical, CHISORB 328), and finally a heterojunction battery component is obtained.

[0070] Comparative Example 1

[0071] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.3 parts of glycidyl methacrylate, and 0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, and finally a heterojunction battery component is obtained.

[0072] Comparative Example 2

[0073] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min) and 0.6 parts of trimethylolpropane triacrylate, and 0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, and finally a heterojunction battery component is obtained.

[0074] Comparative Example 3

[0075] The difference from Example 1 is that the formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.6 parts of triallyl isocyanurate, 0.3 parts of glycidyl methacrylate, and 0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, and finally a heterojunction battery assembly is obtained.

[0076] Comparative Example 4

[0077] The difference from Example 1 is that the formula of the first bonding layer 1 is: 100 parts of EVA (VA content is 15wt%, melt index is 1g / 10min), 0.4 parts of γ-methacryloxypropyltrimethoxysilane, 0.7 parts of triallyl isocyanurate, 0.5 parts of trimethylolpropane triacrylate, 0.5 parts of tert-amyl peroxide-2-ethylhexyl carbonate, and 0.3 parts of ultraviolet light absorber 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole (Double Bond Chemical, CHISORB 328).

[0078] The formula of the first supporting layer 3 is: 100 parts of EVA (VA content is 28wt%, melt index is 6g / 10min), 0.3 parts of glycidyl methacrylate, and 0.5 parts of tert-butyl peroxide-2-ethylhexyl carbonate, and finally a heterojunction battery component is obtained.

[0079] Comparative Example 5

[0080] The difference from Example 1 is that the first supporting layer 3 is not pre-crosslinked, and a heterojunction battery assembly is finally obtained.

[0081] The adhesion force A (unit N / 10mm) between the supporting layer and the heterojunction battery of the heterojunction battery module, the adhesion force B (unit N / 10mm) between the adhesive layer and the front glass, the bubble rate C (unit: %) of the heterojunction battery module, and the module EL shadow D (unit: place) in the above embodiments and comparative examples were tested, and the test results are listed in Table 1.

[0082] Test method for the adhesion force A between the support layer and the heterojunction battery: Take 3mm thick glass, single-chip crystalline silicon battery, encapsulation film, and backplane, and put them into the vacuum laminator in the order of glass / encapsulation film / battery / isolation strip / encapsulation film / backplane (the support layer of the encapsulation film is set toward the battery cell side), and laminate and cure at 145℃ for 18 minutes. Test on a tensile machine with a peeling speed of 100mm / min, and record the peeling strength value to characterize the adhesion force A (unit N / 10mm) between the support layer of the encapsulation film and the battery cell.

[0083] Test method for the adhesive force B between the adhesive layer and the front glass: Take 3mm thick glass, encapsulation film, and TPT backplane, and put them into a vacuum laminator in the order of glass / film / backplane (the adhesive layer of the encapsulation film is set toward the glass side), and laminate at 145℃ for 16 minutes. The test is carried out in accordance with GB / T2790-1995, using a tensile machine for testing, with a test speed of 100mm / min, and recording the peel strength value to characterize the adhesive force B (unit N / 10mm) between the adhesive layer of the encapsulation film and the front glass.

[0084] The test method of the bubble rate C of the heterojunction battery module is as follows: put the glass / encapsulation film / cell / encapsulation film / glass into the vacuum laminator in the order (the support layer of the encapsulation film is set toward the cell side), and laminate at 145°C (vacuuming for 6 minutes, laminating for 12 minutes) to make a double-glass module. A total of 100 modules are made for each combination. After the module cools down, the appearance of the module is visually observed. If there are more than one bubble with a diameter greater than 1mm, it is counted as a bubble module. The bubble rate C is: the number of bubble modules / 100 (unit: %).

[0085] Component EL shadow D test method: When the encapsulation film is used at the component end, if the fluidity is large, it will flow between the welding wire and the battery to cause poor contact. Through the component EL test, the location of the poor contact is shown as a shadow in the EL. Put it into the vacuum laminator in the order of glass / encapsulation film / cell / encapsulation film / glass (the support layer of the encapsulation film is set toward the cell side), and laminate at 145℃ (vacuuming for 6 minutes, laminating for 12 minutes) to make a double-glass component. The shadow of the component cell is observed through EL tracking, and the total number of shadows is D (unit: place).

[0086] Table 1

[0087] Implementation / Comparative Example A(N / 10mm) B(N / 10mm) C(%) D(place) Example 1 45 165 0 0 Example 2 49 168 0 5 Example 3 43 163 0 0 Example 4 40 164 0 0 Example 5 48 170 0 0 Example 6 44 163 0 0 Example 7 35 162 0 8 Example 8 46 168 0 0 Example 9 44 166 0 0 Example 10 46 167 0 0 Embodiment 11 44 163 0 0 Example 12 43 151 0 0 Comparative Example 1 44 163 0 15 Comparative Example 2 20 160 0 0 Comparative Example 3 43 162 0 12 Comparative Example 4 42 122 10 0 Comparative Example 5 48 171 0 18

[0088] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0089] The irradiation bridging agent and metal binder containing the above specific functional groups, the two are copolymerized by the free radicals generated during high-energy electron beam irradiation or ultraviolet irradiation, and cross-linked with the EVA copolymer, which helps to form hydrogen bonds or coordination bonds between the metal oxides on the surface of the heterojunction battery, thereby improving the adhesion between the support layer and the heterojunction battery, and then under high temperature operation, reducing the reliability risk caused by the easy delamination of the encapsulation film in the heterojunction battery assembly from the heterojunction battery. At the same time, the pre-crosslinked support layer has low fluidity, which can effectively support and fix the fitting of the circular welding wire and the fine grid line of the battery. In addition, the barrier layer of the present invention is composed of vinyl polyolefin resin, which has the effect of blocking the migration of the bridging agent and the metal binder in the support layer to the bonding layer, so that the bonding layer can be effectively prevented from being pre-crosslinked during the irradiation process, thereby ensuring that the bonding layer has good fluidity, ensuring good adhesion and exhaust between it and the front glass or back glass (back plate), helping to reduce the bubbles of the assembly, and improving the reliability of the heterojunction battery assembly. Controlling the pre-crosslinking degree of the support layer within the above range can make the support layer have both low fluidity and high adhesion. If the pre-crosslinking degree of the support layer is lower than 10%, when the encapsulation film is used at the subsequent component end, due to its high fluidity, the encapsulation film will flow between the welding wire and the battery, causing poor contact, thereby affecting the power of the photovoltaic component; if the pre-crosslinking degree of the support layer is higher than 60%, the adhesion between the encapsulation film and the heterojunction battery is relatively low. Therefore, controlling the pre-crosslinking degree of the support layer to be 10-60% can take into account both the fluidity and adhesion of the support layer.

[0090] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A packaging film, characterized in that: The packaging film includes an adhesive layer, a barrier layer and a support layer stacked in sequence, the barrier layer includes a vinyl polyolefin resin, and the support layer includes an irradiation bridging agent and a metal binder, wherein the irradiation bridging agent refers to a small molecule monomer or polymer containing at least three acrylate groups, and the metal binder refers to a small molecule monomer or polymer containing at least one olefinic double bond and at least one functional group, and the functional group is selected from any one or more of epoxy, isocyanate, siloxane, hydroxyl, carboxyl, anhydride, mercapto, and amino groups; the olefinic double bond is selected from any one or more of vinyl, allyl, acrylate, and methacrylate groups; and the pre-crosslinking degree of the support layer is 10 to 60%.

2. The packaging film according to claim 1, characterized in that: The pre-crosslinking degree of the support layer is 30-50%; and / or the thickness of the support layer is 30-200 μm; And / or, the support layer comprises ethylene-vinyl acetate copolymer, the VA content of the ethylene-vinyl acetate copolymer in the support layer is 15-33wt%, and under the test conditions of 190°C and 2.16kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30g / 10min, preferably 1-15g / 10min; And / or, in parts by weight, the support layer comprises: 100 parts of the ethylene-vinyl acetate copolymer; 0.1 to 3 parts of the irradiated bridging agent; and 0.05 to 3 parts of the metal binder.

3. The packaging film according to claim 1 or 2, characterized in that: The radiation bridging agent is a multi-acrylate monomer and a polymer thereof, and the multi-acrylate monomer is preferably selected from any one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, ethoxylated pentaerythritol tetraacrylate, propoxylated pentaerythritol tetraacrylate, ethoxylated pentaerythritol triacrylate, propoxylated pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated trimethylolpropane trimethacrylate, propoxylated trimethylolpropane trimethacrylate, and dipentaerythritol hexaacrylate.

4. The encapsulation film according to any one of claims 1 to 3, characterized in that: The metal binder is selected from any one or more of glycidyl methacrylate, maleic anhydride, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, butoxymethyl acrylamide, vinyl triethoxysilane, vinyl trimethoxysilane, vinyl triisopropoxysilane, vinyl tri(β-methoxyethoxy)silane, acrylic acid, 3,4-epoxycyclohexyl methyl methacrylate, 3,4-epoxycyclohexyl methacrylate, 1,2-epoxy-4-vinylcyclohexane, glycidyl acrylate, tetrahydrofurfuryl methacrylate, tetrahydrofurfuryl acrylate, methacrylic acid, acrylamide, N-isopropyl acrylamide, N-tert-butyl acrylamide, N-(2-hydroxyethyl) acrylamide, N-(2-hydroxyethyl) methacryloyl, N-(2-hydroxypropyl) methacrylamide, methacrylamide, 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate, epoxy acrylate, allyl glycidyl ether, polyurethane acrylate and epoxy resin with any double bond.

5. The encapsulation film according to any one of claims 1 to 4, characterized in that: The vinyl polyolefin resin in the barrier layer is an ethylene homopolymer or a copolymer of ethylene, propylene and α-olefin; the molar fraction of ethylene in the vinyl polyolefin resin is greater than 70%; preferably, the carbon number of the α-olefin is 4 to 10, and under the test conditions of 190°C and 2.16kg, the melt index of the vinyl polyolefin resin is preferably 2 to 20g / 10min, and the melting point of the vinyl polyolefin resin is preferably 40 to 125°C; preferably, the thickness of the barrier layer is 50 to 250μm, and the molecular weight distribution index of the vinyl polyolefin resin is preferably less than 2.

3.

6. The packaging adhesive film according to any one of claims 1 to 5, characterized in that: The bonding layer comprises ethylene-vinyl acetate copolymer, wherein the VA content of the ethylene-vinyl acetate copolymer in the bonding layer is 15-33 wt %, and under the test conditions of 190° C. and 2.16 kg, the melt index of the ethylene-vinyl acetate copolymer is preferably 1-30 g / 10 min; Preferably, the bonding layer further comprises a silane coupling agent; and preferably, the bonding layer has a thickness of 30 to 250 μm.

7. The encapsulation film according to any one of claims 1 to 6, characterized in that: In parts by weight, the barrier layer and the bonding layer further independently include 0.1 to 2 parts of a first organic peroxide, the support layer further includes 0 to 2 parts of a second organic peroxide, and / or the support layer further includes 0 to 2 parts of a photoinitiator; wherein, preferably, the first organic peroxide and the second organic peroxide are each independently selected from tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxy-2-ethylhexyl carbonate, tert-hexyl peroxy-2-ethylhexyl carbonate, tert-butyl peroxy-isopropyl carbonate, tert-butyl peroxy-isobutyl carbonate, tert-amyl peroxy-isopropyl carbonate, tert-amyl peroxy-isobutyl carbonate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy-3 , tert-amyl peroxy of 5,5-trimethylhexanoate, 1,1-bis(tert-butyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexyl peroxy)cyclohexane, 1,1-bis(tert-amyl peroxy)cyclohexane, 1,1-bis(tert-butyl peroxy)cyclohexane; preferably, the photoinitiator is selected from any one or more of benzophenone and its derivatives, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl trimethylbenzoyl phenylphosphonate, 2-hydroxy-2-methyl-1-phenylacetone, 1-hydroxycyclohexyl phenyl ketone, and benzoin dimethyl ether.

8. The packaging film according to any one of claims 1 to 7, characterized in that: At least one of the bonding layer, the support layer or the barrier layer contains an ultraviolet light conversion agent, and the ultraviolet light conversion agent is preferably selected from any one or more of organic fluorescent pigments, rare earth organic complexes, rare earth inorganic compounds, CdSe quantum dots, and perovskite quantum dots; preferably, the ultraviolet light conversion agent converts light with a wavelength of 300 to 400 nm into visible light with a wavelength greater than 400 nm.

9. The packaging adhesive film according to any one of claims 1 to 8, characterized in that: At least one of the adhesive layer, the support layer or the barrier layer contains an ultraviolet light absorber, and the ultraviolet light absorber is preferably selected from 2-hydroxy-4-octyloxybenzophenone, 2-cyano-3,3-diphenylacrylate, ethylhexyl p-methoxycinnamate, isooctyl p-methoxycinnamate, dimethyl 4-methoxybenzylidenemalonate, N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)-oxalamide, 2-(2'-hydroxy-5'-tert-butylphenyl)- 2-(2-hydroxy-3-[a,a-dimethylbenzyl]-5-tert-octyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 3,5-di-tert-butyl-4-hydroxybenzoic acid hexadecyl ester, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-n-hexaneoxyphenol, 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)- Any one or more of 5-octyloxyphenol, 2-(2'-hydroxy-3',5'bis(a,a-dimethylbenzyl)phenyl)benzotriazole, and polysilicone-15.

10. A heterojunction battery assembly, comprising a packaging film, characterized in that: The packaging film is the packaging film according to any one of claims 1 to 9.

Citation Information

Cited By

  • Special composite adhesive film for main-grid-free photovoltaic module as well as preparation method and application of special composite adhesive film

    CN119391312A