Method for recovering P507 from P507-hydrochloric acid system raffinate
By adding rare earth chloride and dispersant to the P507-hydrochloric acid system, the pH value is controlled to form precipitates, and separation is performed using alkaline solution and flocculant, the poor recovery effect of organic extractant in the raffinate in the prior art is solved. The problem of this has achieved efficient P507 recycling and rare earth recycling, avoiding the generation of solid waste and wastewater.
Patent Information
- Application Number
- CN202411144729.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
Smart Images

Figure CN119020589A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of extractant recovery, and in particular to a method for recovering P507 in a raffinate of a P507-hydrochloric acid system. Background Art
[0002] Due to their unique physical and chemical properties, rare earth elements have wide application value in many fields such as metallurgy, glass, ceramics, chemical industry, nuclear industry, electronics industry, agriculture and medicine.
[0003] However, rare earth elements have similar electronic structures and chemical properties, and they always exist in the form of paragenetic minerals, making separation very difficult. In order to overcome this problem, researchers have been exploring different extraction systems. Among them, P204 (2-ethylhexyl phosphate) and P507 (2-ethylhexyl phosphate mono-ethylhexyl ester) are widely used due to their excellent extraction ability. In particular, P507 overcomes the shortcomings of P204, such as difficulty in stripping and easy emulsification, and has become a very promising extractant in extraction separation technology and rare earth analysis.
[0004] At present, researchers usually use the P507-hydrochloric acid system to extract and separate two different rare earths. This method uses P507 as an extractant to separate rare earth elements in a hydrochloric acid system. However, as the extraction process proceeds, a certain amount of organic extractant will remain in the raffinate, and how to effectively recover this organic extractant has become a problem.
[0005] Currently, there are mainly gravity separation, dissolved air flotation, adsorption and other methods for recovering organic extractants in the raffinate. Gravity separation and dissolved air flotation mainly rely on the density difference between the organic extractant and the aqueous phase, and treat the dispersed and emulsified organic extractants under the action of gravity or micro-nano bubbles. However, these methods have limited effects on the recovery of dissolved organic extractants.
[0006] The adsorption method uses the porosity of solid adsorbents such as activated carbon, fly ash, zeolite, and resin to achieve efficient adsorption and removal of organic extractants. However, after using adsorbents such as activated carbon to adsorb organic extractants, these adsorbents are often difficult to regenerate and recycle, and can usually only be used as disposable consumables, which not only increases processing costs, but also generates a large amount of solid waste.
[0007] Therefore, how to develop an organic extractant recovery method that can be both efficiently recovered and recycled has become an important issue to be solved in the current field of rare earth element separation. Summary of the invention
[0008] The present invention aims to solve the problems in the prior art that gravity separation and dissolved air flotation methods have poor recovery effects on organic extractants and that the adsorbent in the adsorption method cannot be recycled, and proposes a method for recovering P507 in the raffinate of a P507-hydrochloric acid system.
[0009] The technical method of the present invention is as follows:
[0010] The present invention provides a method for recovering P507 from a raffinate of a P507-hydrochloric acid system, the method comprising:
[0011] S1, adding rare earth chloride and dispersant to the raffinate to control the reaction pH value to 1-1.5;
[0012] S2, adding the reacted mixture to an alkaline solution, and controlling the pH value of the reaction end point to be 6-7;
[0013] S3. Acid hydrolyze and separate the precipitate obtained after the above reaction to obtain an organic solution containing P507 and a rare earth solution.
[0014] Specifically, step S1 includes: first adding a dispersant to the raffinate, stirring for a period of time, and then adding a rare earth chloride and mixing for a period of time; wherein the stirring time is 10 to 15 minutes, and the mixing time is 3 to 5 minutes.
[0015] In step S1, the volume ratio of the raffinate to the dispersant is 50±5L:2±0.25mL; the ratio of the amount of P507 in the raffinate to the amount of REO in the rare earth chloride solution is 0.16-0.29mol:10.2-11.85g.
[0016] The dispersant is water glass.
[0017] Specifically, step S2 includes: first adding an alkaline solution to the raffinate to control the pH value to 4-5, then adding a dispersant to react for a period of time, and finally adding an alkaline solution to control the pH value of the reaction end point to 6-7; wherein the reaction time is 5-10 minutes, and the rate of adding the alkaline solution is 0.1-0.3 L / h.
[0018] The dispersant is water glass.
[0019] The alkaline solution is an ammonium alkaline solution, including ammonia water or ammonium bicarbonate; the concentration of the alkaline solution is 8-15%.
[0020] In step S1, the ratio of raffinate to dispersant is 50±5L:2±0.25mL.
[0021] Specifically, the acid solution is hydrochloric acid, and the concentration of the hydrochloric acid is 8-15%.
[0022] In the present invention, after step S2, the method further includes: adding a flocculant to the precipitate obtained after the above reaction, and filtering.
[0023] The flocculant is polyacrylamide.
[0024] The present invention has the following beneficial effects:
[0025] (1) The present invention adds a dispersant to the raffinate to fully diffuse the residual P507, then adds rare earth chloride as a polymerization precursor, slowly adds an alkaline solution to precipitate the rare earth, utilizes the rare earth to polymerize with P507 during the precipitation process to form a precipitate, filters out the precipitate, and since the precipitate contains rare earth precipitate and P507, the precipitate is acid-hydrolyzed, the rare earth precipitate is converted into a rare earth chloride solution and back-extracted to an aqueous phase, the rare earth chloride is soluble in water, and the P507 organic solution is insoluble in water, thereby achieving separation of rare earth and P507, the separated rare earth solution can be used as a precursor, and the P507 organic solution can be used as an extractant.
[0026] (2) The recovery rate of P507 separated by the present invention reaches 95%.
[0027] (3) No solid waste or wastewater is generated during the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The present invention is a flow chart of the method for recovering P507 from the raffinate of the P507-hydrochloric acid system. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below through specific implementation cases and accompanying drawings. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0030] The present invention provides a method for recovering P507 from the raffinate of a P507-hydrochloric acid system, such as Figure 1 As shown, the method includes:
[0031] S1. Add rare earth chloride and dispersant to the raffinate to control the reaction pH value to 1-1.5.
[0032] In one embodiment, the raffinate contains P507.
[0033] In one embodiment, the dispersant is water glass. The dispersant can ensure that the P507 in the raffinate is uniformly dispersed in the water phase.
[0034] In one embodiment, the rare earth chloride includes one or more of lanthanum chloride solution, cerium chloride solution, praseodymium chloride solution, and neodymium chloride solution.
[0035] In one embodiment, rare earth chloride is used as a polymerization precursor to change the pH value, and then the organic extractant (ie, P507) in the raffinate is polymerized and precipitated in the subsequent process to achieve the effect of separating the organic.
[0036] In one embodiment, the volume ratio of the raffinate to the dispersant is 50±5 L:2±0.25 mL. For example, the volume ratio of the raffinate to the dispersant is 48 L:1.75 mL, 50 L:2 mL, 53 L:2.2 mL.
[0037] In one embodiment, the ratio of P507 in the raffinate to REO in the rare earth chloride solution is 0.16-0.29 mol: 10.2-11.85 g. For example, the ratio is 0.17 mol: 10.2 g, 0.21 mol: 10.8 g, 0.23 mol: 11.85 g. Here, the amount of dispersant added is determined based on the volume of the raffinate. Rare earth chloride is obtained based on the ratio of REO (rare earth oxide) to P507 in the raffinate.
[0038] Specifically, step S1 includes: first adding a dispersant to the raffinate, stirring for a period of time, then adding a rare earth chloride, and mixing for a period of time to control the reaction pH value to 1 to 1.5 to ensure that the subsequent alkaline solution neutralizes the acid.
[0039] The stirring time is 10 to 15 minutes, and the mixing time is 3 to 5 minutes. For example, the stirring time is 11 minutes, 13 minutes, and 15 minutes, and the mixing time is 3 minutes, 4 minutes, and 5 minutes.
[0040] S2. Add the mixture after the reaction into an alkaline solution and control the pH value at the reaction end point to be 6-7.
[0041] Here, the purpose of the alkaline substance is to adjust the pH value to form a precipitate of the rare earth elements in an ionic state, and during the formation process, P507 will follow into the precipitate. In other words, the present invention enriches both the rare earth and P507 to form a precipitate.
[0042] In one embodiment, the alkaline solution is an ammonium alkaline solution. The ammonium alkaline solution includes ammonia water or ammonium bicarbonate. The concentration of the alkaline solution is 8-15%. For example, the concentration of the alkaline solution is 10%, 12%, or 14%.
[0043] In one embodiment, in step S2, the volume ratio of the raffinate to the dispersant is 50±5L:2±0.25mL.
[0044] Specifically, step S2 includes: first adding an alkaline solution to the raffinate to control the pH value to 4-5, then adding a dispersant to react for a period of time, and finally adding an alkaline solution to control the pH value of the reaction end point to 6-7.
[0045] Here, the reason for suspending the addition of alkaline solution and adding dispersant when the pH value is in the range of 4 to 5 is that the closer the precipitation polymerization reaction is to the endpoint pH value, the easier it is to form large-particle precipitate solids, and the dispersant can prevent this phenomenon from happening, increase the specific surface area of the precipitate, and promote the polymerization of P507.
[0046] In one embodiment, the reaction time is 5 to 10 minutes. The rate of adding the alkaline solution is 0.1 to 0.3 L / h. For example, the reaction time is 6 minutes, 8 minutes, or 10 minutes.
[0047] S3. Acid hydrolyze and separate the precipitate obtained after the above reaction to obtain an organic solution containing P507 and a rare earth solution.
[0048] Specifically, the above reaction is followed by filtration to obtain a precipitate.
[0049] In one embodiment, the above reaction is filtered to obtain a supernatant. The rare earth concentration and P507 in the supernatant are calculated to calculate the P507 recovery rate and the rare earth recovery rate. Here, the rare earth concentration is measured by inductively coupled plasma atomic emission spectrometry, and P507 is calculated by measuring its phosphorus content. The supernatant of the present invention contains 0.00014 to 0.00029 mol / L of P507 and less than 0.005 g / L of rare earth.
[0050] After step S2, the method further includes: adding a flocculant to the precipitate obtained after the above reaction and filtering. Here, the precipitate obtained by filtering is then subjected to step S3.
[0051] In one embodiment, the flocculant is polyacrylamide. Here, after the precipitate is obtained, the solution is in a turbid state, and the solid particles are fine and the sedimentation speed is slow. The flocculant is added to aggregate the solid fine particles, accelerate sedimentation, and save time.
[0052] S3. Acid hydrolyze and separate the precipitate obtained after the above reaction to obtain an organic solution containing P507 and a rare earth solution.
[0053] Specifically, the acid solution is used for acid hydrolysis. The acid solution is hydrochloric acid. The concentration of hydrochloric acid is 8 to 15%. For example, the concentration of hydrochloric acid is 10%, 12%, or 14%.
[0054] Here, the purpose of acid hydrolysis is to dissolve the rare earth elements in the precipitate into rare earth chloride solution and back-extract to the water phase. Since P507 does not react with acid and P507 is insoluble in water, rare earth chloride is soluble in water, thereby separating the rare earth and P507 by phase separation.
[0055] Here, separation is carried out in a stratified manner. A phase separation device is used for stratification, with the aqueous phase (rare earth chloride) at the bottom and the organic phase (P507) at the top. After standing for a period of time, the bottom valve is opened to discharge the aqueous phase containing rare earth elements to achieve separation. Here, rare earth is used as a circulating carrier, and the separated organic phase can be put into production after the P507 concentration is tested.
[0056] In one embodiment, when the alkaline solution is ammonium bicarbonate and hydrochloric acid is used for acid hydrolysis, after step S3, the ammonium chloride solution contained in the raffinate in P507 is removed, and the ammonium chloride solution can produce industrial-grade salts, meeting the green and environmentally friendly production concept.
[0057] In order to better understand the above exemplary embodiments of the present invention, they are further described below with reference to specific examples.
[0058] Example 1
[0059] Step 1: Take 50L of the raffinate material in a reaction container, and measure its P507 content to be 0.0049mol / L. Start stirring and add 2mL of water glass. After 10 minutes, take 50mL of cerium chloride with a concentration of 204g / L and add it to the reaction container, stir and mix, and measure the rare earth concentration of the material to be 0.2037g / L.
[0060] Step 2: Add 25% ammonia water and control the flow rate at 0.17 L / h.
[0061] Step 3: Observe the change in pH value of the material. When the pH value of the material reaches 5, stop adding ammonia water, add 2mL of water glass, react for 10 minutes, continue to add ammonia water, when the pH value is 7, take a small amount of material and filter out the supernatant to measure its P507 content of 0.00025mol / L, and the rare earth content is less than 0.005g / L.
[0062] Step 4: After adding polyacrylamide precipitation, separate the supernatant and add 150 mL of 10% dilute hydrochloric acid to the precipitate to dissolve it. The reaction time is 30 minutes.
[0063] Step 5: The material after the reaction in step 4 was transferred to a liquid separation device for static stratification. The volume of the organic phase was 175 mL, and the P507 concentration was measured to be 1.29 mol / L. The volume of the aqueous phase was 214 mL, and the rare earth concentration was 47.64 g / L. The recovery rate of P507 was 94.85%.
[0064] Example 2
[0065] Step 1: Take 50L of the raffinate material in a reaction container, and measure its P507 content to be 0.0058mol / L. Start stirring and add 2mL of water glass. After 10 minutes, take 50mL of lanthanum chloride with a concentration of 218g / L and add it to the reaction container, stir and mix, and measure the rare earth concentration of the material to be 0.2177g / L.
[0066] Step 2: Add 25% ammonia water and control the flow rate at 0.15 L / h.
[0067] Step 3: Observe the change in pH value of the material. When the pH value of the material reaches 4.5, stop adding ammonia water, add 2mL of water glass, react for 10 minutes, and continue to add ammonia water. When the pH value is 6.5, take a small amount of material and filter out the supernatant. The P507 content is 0.00029mol / L, and the rare earth content is less than 0.005g / L.
[0068] Step 4: After adding polyacrylamide precipitation, separate the supernatant and add 162 mL of 10% dilute hydrochloric acid to the precipitate for dissolution. The reaction time is 25 minutes.
[0069] Step 5: After the reaction in step 4 was completed, the material was transferred to a liquid separation device and allowed to stand for stratification. The volume of the organic phase was 181 mL, and the P507 concentration was measured to be 1.59 mol / L. The volume of the aqueous phase was 225 mL, and the rare earth concentration was 48.43 g / L. The P507 recovery rate was 94.87%.
[0070] Example 3
[0071] Step 1: Take 50L of the raffinate material in a reaction container, and measure its P507 content to be 0.0032mol / L. Start stirring and add 2mL of water glass. After 10 minutes, take 50mL of a 1:1 mixed solution of praseodymium chloride and cerium chloride with a concentration of 237g / L and add it to the reaction container, stir and mix, and measure the rare earth concentration of the material to be 0.2367g / L.
[0072] Step 2: Add 25% ammonia water and control the flow rate at 0.2 L / h.
[0073] Step 3: Observe the change in pH value of the material. When the pH value of the material reaches 4.5, stop adding ammonia water, add 2mL of water glass, react for 10 minutes, and continue to add ammonia water. When the pH value is 7, take a small amount of material and filter the clear liquid to measure its P507 content of 0.00014mol / L, and the rare earth content is less than 0.005g / L.
[0074] Step 4: After adding polyacrylamide precipitation, separate the supernatant, add 174 mL of 10% dilute hydrochloric acid to the precipitate for dissolution, and the reaction time is 20 minutes.
[0075] Step 5: The material after the reaction in step 4 was transferred to a liquid separation device for static stratification. The volume of the organic phase was 155 mL, and the P507 concentration was measured to be 1.0 mol / L. The volume of the aqueous phase was 200 mL, and the rare earth concentration was 57.95 g / L. The P507 recovery rate was 95.65%.
[0076] Example 4
[0077] Step 1: Take 50L of the raffinate material in a reaction container, and measure its P507 content to be 0.0049mol / L. Start stirring and add 2mL of water glass. After 10 minutes, take 50mL of 215g / L neodymium chloride solution and add it to the reaction container and stir to mix. The rare earth concentration of the material is measured to be 0.2385g / L.
[0078] Step 2: Add 25% ammonium bicarbonate and control the flow rate at 0.2 L / h.
[0079] Step 3: Observe the change in pH value of the material. When the pH value of the material reaches 4.5, stop adding ammonium bicarbonate, add 2 mL of water glass, react for 10 minutes, and continue to add ammonium bicarbonate. When the pH value is 7, take a small amount of material and filter the clear liquid to measure its P507 content of 0.00017 mol / L, and the rare earth content is less than 0.006 g / L.
[0080] Step 4: After adding polyacrylamide precipitation, separate the supernatant, add 178 mL of 10% dilute hydrochloric acid to the precipitate for dissolution, and the reaction time is 20 minutes.
[0081] Step 5: The material after the reaction in step 4 was transferred to a liquid separation device for static stratification. The volume of the organic phase was 155 mL, and the P507 concentration was measured to be 1.58 mol / L. The volume of the aqueous phase was 200 mL, and the rare earth concentration was 53.75 g / L. The P507 recovery rate was 97.48%.
[0082] This document uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solution and its core idea of the present application. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solution deviate from the scope of the technical solution of the embodiments of the present application.
Claims
1. A method for recovering P507 from the raffinate of a P507-hydrochloric acid system, characterized in that: The method comprises: S1, adding rare earth chloride and dispersant to the raffinate to control the reaction pH value to 1-1.5; S2, adding the reacted mixture to an alkaline solution, and controlling the pH value of the reaction end point to be 6-7; S3. Acid hydrolyze and separate the precipitate obtained after the above reaction to obtain an organic solution containing P507 and a rare earth solution.
2. The recycling method according to claim 1, characterized in that: The S1 step includes: Firstly add dispersant to the raffinate, stir for a while, then add rare earth chloride, and mix for a while; The stirring time is 10 to 15 minutes, and the mixing time is 3 to 5 minutes.
3. The recycling method according to claim 1, characterized in that: In step S1, the volume ratio of raffinate to dispersant is 50±5L:2±0.25mL; The ratio of P507 in the raffinate to REO in the rare earth chloride solution is 0.16-0.29 mol: 10.2-11.85 g.
4. The recycling method according to claim 1, characterized in that: The S2 step includes: Firstly add alkaline solution to the raffinate to control the pH value to 4-5, then add dispersant to react for a period of time, and finally add alkaline solution to control the pH value of the reaction end point to 6-7; The reaction time is 5 to 10 minutes, and the rate of adding the alkaline solution is 0.1 to 0.3 L / h.
5. The recycling method according to claim 4, characterized in that: The dispersant is water glass.
6. The recycling method according to claim 1, characterized in that: In step S1, the ratio of raffinate to dispersant is 50±5L:2±0.25mL.
7. The recycling method according to claim 1, characterized in that: The alkaline solution is an ammonium alkaline solution, including ammonia water or ammonium bicarbonate; the concentration of the alkaline solution is 8-15%.
8. The recycling method according to claim 1, characterized in that: The acid solution used for acid hydrolysis is hydrochloric acid, and the concentration of the hydrochloric acid is 8-15%.
9. The recycling method according to claim 1, characterized in that: After step S2, it also includes: A flocculant is added to the precipitate obtained after the above reaction and filtered.
10. The recycling method according to claim 9, characterized in that: The flocculant is polyacrylamide.