Repeatable ultrahigh-temperature thermal protection coating
The ultra-high temperature thermal protection coating with multi-layer structures was prepared through atmospheric plasma spraying technology. The double powder feeding process and meltable powder were mixed, which solved the problems of insufficient thermal protection and complex preparation of existing coatings at high temperatures, and realized coating The layer is efficient, stable and reusable at high temperatures.
Patent Information
- Application Number
- CN202411144165.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
Existing thin thermal barrier coatings are difficult to meet thermal protection requirements at high temperatures, increasing thickness will lead to a decrease in the use temperature and thermal cycle times, and traditional gradient coatings are complex in preparation and are not conducive to engineering applications.
The ultra-high temperature thermal protection coating with multi-layer structures is prepared by atmospheric plasma spraying technology, including the bonding layer, the intermediate layer and the ceramic layer. The intermediate layer is mixed with powder through the double powder feeding process and the Y-shaped conveying pipeline, and uses a meltable spherical shape. Thin-walled hollow-shell nanot'-YSZ powder and NiCrAlY powder are mixed in different proportions to reduce the melting point difference of the initial powder and simplify the preparation process.
The coating thickness, temperature and number of repetitions are achieved. After 60 thermal shocks at 1750°C, the surface is intact, the interface bonding strength is high, the structure is stable, the number of repetitions is increased by 60 times, and the preparation process is simple and the cost is Low.
Smart Images

Figure CN119020718A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to thermal protection coatings, and more particularly to a repeatable ultra-high temperature thermal protection coating. Background Art
[0002] As the thermal protection requirements for engine hot end components become increasingly stringent, thin thermal barrier coatings (200 μm) can no longer meet the thermal protection and insulation requirements (Int. Mater. Rev. 58 (2013) 315-348). Increasing the thickness of the top coating is a promising technology that can improve the thermal insulation potential of the top coating by maintaining its mechanical properties (Surf. Coat. Technol. 205 (2010) 1250-1255.). However, the increase in thickness will lead to a decrease in the operating temperature and number of thermal cycles of the coating, because the residual stress and thermal stress in thick thermal barrier coatings (TTBCs) will increase with increasing thickness (Ceram. Int. 48 (2022) 5299-5311).
[0003] One way to overcome this problem is to introduce the concept of functional gradient materials (FGM) in TBCs (Surf. Coat. Technol. 154 (2002) 223-231). Gradient coatings can reduce stress concentration at discrete interfaces and solve the problem of short life of double-layer thick coatings under service conditions due to their continuous gradient of composition, elastic modulus, hardness, thermal conductivity, and thermal expansion coefficient (Mater. Lett. 38 (1999) 437-444). Atmospheric plasma spraying (APS) is one of the most commonly used technologies for manufacturing these coatings due to its low cost and high maturity (Surf. Eng. 34 (2018) 728-736.). However, since the melting point of ceramic powder (~2700°C) is much higher than that of metal powder (~1500°C), the APS melting power of metal powder (~30kw) is much lower than the full melting power of ceramic powder (~75kw) (Ceram.Int.48(2022)28800–28814, Sur.Coat.Technol.426(2021)127768). The power mismatch leads to excessive oxidation of metal particles or semi-melting of ceramic particles during the deposition of APS gradient coating (Surf.Coat.Technol.114(1999)181-186.). In order to solve the problem of mismatch in the melting power of the two initial powders in the gradient coating, relatively easier to melt hollow spherical YSZ powder can be used (Ceram.Int.48(2022)28800-28814.). In addition, the preparation process of traditional gradient coatings is relatively complicated due to the need for multiple material changes during spraying, which is not conducive to engineering applications (Ceram. Int. 47 (2021) 34361-34379). Summary of the invention
[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0005] In order to achieve these purposes and other advantages of the present invention, a repeatable ultra-high temperature thermal protective coating is provided, comprising: a bonding layer prepared on a substrate, an intermediate layer prepared on the bonding layer, and a ceramic layer prepared on the intermediate layer; wherein the number of the intermediate layers is ≥ 2 layers.
[0006] Preferably, the bonding layer is prepared by spraying bonding layer powder on the substrate using an atmospheric plasma spraying process, and the thickness thereof is 70 to 120 μm.
[0007] Preferably, the bonding layer powder is Oerlikon Metco Amdry 962 grade NiCrAlY, whose composition is Ni22Cr10Al1.0Y; and the matrix is GH5188 alloy.
[0008] Preferably, the preparation method of the intermediate layer is: using an atmospheric plasma spraying process, spraying the intermediate layer powder on the bonding layer to prepare a first intermediate layer, then spraying on the first intermediate layer to prepare a second intermediate layer, and continuing to spray to prepare an intermediate layer with a number of layers ≥ 2, each layer having a thickness of 80 to 150 μm.
[0009] Preferably, the ceramic layer is prepared by spraying ceramic layer powder on the intermediate layer using an atmospheric plasma spraying process, and the thickness thereof is 800-1000 μm.
[0010] Preferably, the ceramic layer powder is spherical thin-walled hollow shell nano t′-YSZ powder.
[0011] Preferably, the intermediate layer powder is obtained by mixing the bonding layer powder and the ceramic layer powder in a mass ratio of 1:0.5 to 5, and the bonding layer powder content in the intermediate layer powder gradually decreases with the increase of the number of intermediate layers, and the ceramic layer powder content gradually increases with the increase of the number of intermediate layers; wherein, the atmospheric plasma spraying process adopts a Y-type conveying pipe to deliver powder, and the bonding layer powder and the ceramic layer powder are independently and simultaneously delivered through the Y-type conveying pipe, and the powder delivery rate is adjusted so that the two powders are mixed according to the set mass ratio before entering the plasma flame zone.
[0012] Preferably, the process parameters of the atmospheric plasma spraying are: current 400-600A, voltage 60-80V, nitrogen flow rate 40-60 liters / minute, hydrogen flow rate 3-5 liters / minute, spraying distance 100-150mm, bonding layer powder feeding rate 0-40g / min, ceramic layer powder feeding rate 0-35g / min, and gun speed 500-700mm / s.
[0013] Preferably, the ceramic layer powder is pretreated before use, and the specific method is: HfO2, Zr 0.83 Y 0.01 Ce 0.16 O2 and ceramic layer powder are mixed, deionized water and polyethylene glycol 4000 are added, the mixture is ground for 1 to 2 hours, spray-dried at 250 to 350° C., and then heat-treated to obtain pretreated ceramic layer powder.
[0014] Preferably, the HfO2, Zr 0.83 Y 0.01 Ce 0.16 The mass ratio of O2 and ceramic layer powder is 1-10:1-10:80-98; the mass of polyethylene glycol 4000 and HfO2, Zr 0.83 Y 0.01 Ce 0.16 The ratio of the total mass of O2 and the ceramic layer powder is 1 to 3:100; the mass of the deionized water and the mass of HfO2, Zr 0.83 Y 0.01 Ce 0.16 The ratio of the total mass of O2 and the ceramic layer powder is 1.1-1.5:1; the specific method of the heat treatment is: heating to 300-500°C at a heating rate of 3-8°C / min, keeping warm for 0.5-2h, then heating to 500-700°C at a heating rate of 3-8°C / min, keeping warm for 0.5-2h, and naturally cooling to room temperature.
[0015] A repeatable ultra-high temperature thermal protective coating as described above is tested 60 times under 1750°C thermal shock conditions, and the coating surface is intact without peeling.
[0016] The present invention includes at least the following beneficial effects: the present invention discloses a repeatable ultra-high temperature thermal protective coating, which realizes the synchronous improvement of coating thickness, temperature and number of repetitions; the present invention adopts spherical thin-walled hollow shell nano t′-YSZ powder and NiCrAlY powder that are easy to melt to mix in different proportions to prepare a gradient intermediate layer, so as to alleviate the difference in melting points of the two initial powders; at the same time, based on the double powder feeding process and the atmospheric plasma spraying process (APS), the gradient coating is prepared in one time and continuously, so as to reduce the difficulty of preparing the gradient coating, ensure that the ceramic powder and the metal powder are evenly distributed during the spraying process, and can achieve synchronous melting; the present invention prepares The repeatable ultra-high temperature thermal protection coating has a metastable tetragonal structure (t'), and presents a gradient structure inside. NiCrAlY particles are evenly dispersed in the gradient structure, and the YSZ at the interfaces of each layer are mutually fused. The ceramic layer and the intermediate layer 2, the intermediate layer 2 and the intermediate layer 1, and the intermediate layer 1 and the bonding layer are tightly connected, and the interface bonding strength is high. After 60 thermal shocks under ultra-high temperature conditions (1750°C), the coating surface is still intact, there is no large-scale peeling, the coating structure has not changed significantly, and no harmful M phase is found inside the coating. The number of times the double-layer coating with the same ceramic layer thickness and the same process is reused is increased by 60 times. In addition, the repeatable ultra-high temperature thermal protection coating of the present invention has the advantages of simple preparation process, low cost, high process maturity, etc., and is expected to be applied in engineering.
[0017] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the double powder feeding process of the present invention;
[0019] Figure 2 The metallographic microstructure of the repeatable ultra-high temperature thermal protection coating prepared in Example 1;
[0020] Figure 3 This is a statistical diagram of the porosity of the repeatable ultra-high temperature thermal protection coating prepared in Example 1;
[0021] Figure 4 This is a microstructure diagram of the double-layer thermal protection coating prepared in Comparative Example 1;
[0022] Figure 5 This is a photo of the repeatable ultra-high temperature thermal protection coating prepared in Example 1 after 60 thermal shock cycle tests;
[0023] Figure 6 This is the thermal shock heating curve of the repeatable ultra-high temperature thermal protective coating prepared in Example 1;
[0024] Figure 7The thermal shock temperature rise curve and the photo after failure of the double-layer thermal protection coating prepared in Comparative Example 1;
[0025] Figure 8 This is the thermal shock temperature rise curve of the three-layer thermal protection coating prepared in Comparative Example 2;
[0026] Fig. 9 This is a photo of the three-layer thermal protection coating prepared in Comparative Example 2 after failure;
[0027] Fig.10 This is the thermal shock temperature rise curve of the three-layer thermal protection coating prepared in Comparative Example 3;
[0028] Fig.11 This is a photo of the three-layer thermal protection coating prepared in Comparative Example 3 after failure;
[0029] Fig.12 XRD diagram of the repeatable ultra-high temperature thermal protection coating prepared in Example 1 after 60 thermal shock cycle tests and in the deposited state (not tested);
[0030] Fig.13 This is a photo of the repeatable ultra-high temperature thermal protective coating prepared in Example 2 after 60 thermal shock cycle tests. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0032] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0033] Figure 1 This is a schematic diagram of the double powder feeding process of the present invention. The powder feeding machine includes two parts. One part is two powder feeding barrels, which are respectively filled with NiCrAlY metal powder and t′-YSZ powder, and the other part is a Y-type conveying pipeline. The powders in the two pipelines are mixed before entering the plasma flame zone. Two powder samples to be delivered are selected, and the powder feeding rate is adjusted so that the powder samples are mixed at the end of the Y-type conveying pipeline according to the set mass ratio, and then enter the plasma flame zone, heated and melted to form a coating.
[0034] In the following embodiments, the spherical thin-walled hollow shell nano t′-YSZ powder used is prepared by the preparation method described in Chinese patent CN202111583210.4, and the spherical thin-walled hollow shell nano t′-YSZ powder has a spherical particle size D50 ≥ 40 μm, a wall thickness ≤ 6 μm, and an average grain size of 20 to 50 nm; the control system used in the atmospheric plasma spraying equipment is Mulitcoat, and the spray gun model used is 3MBTD.
[0035] Example 1
[0036] A repeatable ultra-high temperature thermal protective coating, comprising:
[0037] Adhesive layer: The adhesive layer powder is sprayed on the substrate GH5188 alloy by atmospheric plasma spraying process, and the thickness is about 100 μm; wherein, the substrate has a diameter of 25.4 mm and a thickness of 5 mm, and the surface oxides and oil stains need to be removed before use, and then sandblasted; the adhesive layer powder is Oerlikon Metco Amdry 962 NiCrAlY, and its specific parameters are shown in Table 1; the specific composition of the substrate GH5188 alloy is shown in Table 2; the atmospheric plasma spraying process parameters are shown in Table 3;
[0038] Table 1
[0039] Brand Element Particle size distribution (μm) Applicable temperature (following spraying method) Amdry962 Ni22Cr10Al1.0Y 53~106 ≤980℃(APS) / ≤1050℃(HVOF)
[0040] Table 2
[0041]
[0042] Table 3
[0043]
[0044] Intermediate layer 1: The intermediate layer 1 powder is sprayed on the bonding layer by atmospheric plasma spraying process, and the thickness is about 120 μm; wherein, the intermediate layer 1 powder is a mixture of NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder, and the mass ratio of NiCrAlY and t′-YSZ is 1:1 by adjusting the powder feeding rate; the atmospheric plasma spraying process parameters are shown in Table 4;
[0045] Table 4
[0046]
[0047] Intermediate layer 2: The intermediate layer 2 powder is sprayed on the intermediate layer 1 by atmospheric plasma spraying process, and the thickness is about 120 μm; wherein, the intermediate layer 2 powder is a mixture of NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder, and the mass ratio of NiCrAlY and t′-YSZ is ensured to be 1:2 by adjusting the powder feeding rate; the atmospheric plasma spraying process parameters are shown in Table 5;
[0048] Table 5
[0049]
[0050] Ceramic layer (YSZ layer): The ceramic layer powder is sprayed on the intermediate layer 2 by an atmospheric plasma spraying process, and the thickness is about 900 μm; wherein the ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder; the atmospheric plasma spraying process parameters are shown in Table 6.
[0051] Table 6
[0052]
[0053] Metallographic microstructure: The polished sample was placed in a metallographic microscope for testing and analysis. The selected metallographic microscope was a Leica inverted metallographic microscope, and the equipment model was DMI8C. The metallographic microstructure of the repeatable ultra-high temperature thermal protection coating prepared in Example 1 is as follows: Figure 2 As shown, it can be seen that the coating prepared by double-powder atmospheric plasma spraying includes four layers: ceramic layer, intermediate layer 2, intermediate layer 1 and bonding layer. The metal particles and ceramic particles are evenly distributed, the interface is tightly bonded, and there is no stratification between the layers; the thicknesses of the bonding layer, intermediate layer 1, intermediate layer 2, and ceramic layer are ~79μm, ~119μm, ~141μm, and ~848μm, respectively; the NiCrAlY content of intermediate layer 1 is higher than that of intermediate layer 2, but there is no obvious interface stratification. According to Image J image analysis statistics, the NiCrAlY contents of intermediate layer 1 and intermediate layer 2 account for ~41% and ~25%, respectively.
[0054] Porosity statistics: Image J image analysis software was used to select SEM photos of appropriate magnifications for porosity statistics of the ceramic layer. This method is based on the fact that the contrast between pores and sample particles in the backscattering mode of the microscope is quite different. Image analysis software is used to adjust the contrast and perform statistical analysis on the pores of the coating. Figure 3 As shown, the porosity of the ceramic layer of the repeatable ultra-high temperature thermal protection coating prepared in Example 1 is calculated to be ∼12%.
[0055] Comparative Example 1
[0056] A double-layer thermal protection coating, comprising:
[0057] Adhesive layer: The adhesive layer powder is sprayed on the substrate GH5188 alloy by atmospheric plasma spraying process, and its thickness is the same as that of the adhesive layer in Example 1; wherein the substrate has a diameter of 25.4 mm and a thickness of 5 mm, and the surface oxides and oil stains need to be removed before use, and then sandblasted; the adhesive layer powder is Oerlikon Metco Amdry 962 grade NiCrAlY, and its specific parameters are shown in Table 1; the specific composition of the substrate GH5188 alloy is shown in Table 2; the atmospheric plasma spraying process parameters are shown in Table 3;
[0058] Ceramic layer (YSZ layer): The ceramic layer powder is sprayed on the bonding layer by an atmospheric plasma spraying process, and its thickness is the same as the total thickness of the intermediate layer 1 + intermediate layer 2 + ceramic layer in Example 1; wherein the ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder; the atmospheric plasma spraying process parameters are shown in Table 6.
[0059] The microstructure of the double-layer thermal protection coating prepared in this comparative example is shown in FIG. Figure 4 shown.
[0060] Comparative Example 2
[0061] A three-layer thermal protection coating comprising:
[0062] Adhesive layer: The adhesive layer powder is sprayed on the substrate GH5188 alloy by atmospheric plasma spraying process, and its thickness is the same as that of the adhesive layer in Example 1; wherein the substrate has a diameter of 25.4 mm and a thickness of 5 mm, and the surface oxides and oil stains need to be removed before use, and then sandblasted; the adhesive layer powder is Oerlikon Metco Amdry 962 grade NiCrAlY, and its specific parameters are shown in Table 1; the specific composition of the substrate GH5188 alloy is shown in Table 2; the atmospheric plasma spraying process parameters are shown in Table 3;
[0063] Intermediate layer: prepared by spraying intermediate layer powder on the bonding layer by atmospheric plasma spraying process, and its thickness is the same as the total thickness of intermediate layer 1 + intermediate layer 2 in Example 1; wherein, the intermediate layer powder is obtained by mixing NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder, and the mass ratio of NiCrAlY and t′-YSZ is ensured to be 1:1 by adjusting the powder feeding rate; the atmospheric plasma spraying process parameters are shown in Table 4;
[0064] Ceramic layer (YSZ layer): The ceramic layer powder is sprayed on the bonding layer by an atmospheric plasma spraying process, and its thickness is the same as that of the ceramic layer in Example 1; wherein the ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder; the atmospheric plasma spraying process parameters are shown in Table 6.
[0065] Comparative Example 3
[0066] A three-layer thermal protection coating comprising:
[0067] Adhesive layer: The adhesive layer powder is sprayed on the substrate GH5188 alloy by atmospheric plasma spraying process, and its thickness is the same as that of the adhesive layer in Example 1; wherein the substrate has a diameter of 25.4 mm and a thickness of 5 mm, and the surface oxides and oil stains need to be removed before use, and then sandblasted; the adhesive layer powder is Oerlikon Metco Amdry 962 grade NiCrAlY, and its specific parameters are shown in Table 1; the specific composition of the substrate GH5188 alloy is shown in Table 2; the atmospheric plasma spraying process parameters are shown in Table 3;
[0068] Intermediate layer: prepared by spraying intermediate layer powder on the bonding layer by atmospheric plasma spraying process, and its thickness is the same as the total thickness of intermediate layer 1 + intermediate layer 2 in Example 1; wherein, the intermediate layer powder is obtained by mixing NiCrAlY and spherical thin-walled hollow shell nano t′-YSZ powder, and the mass ratio of NiCrAlY and t′-YSZ is ensured to be 1:2 by adjusting the powder feeding rate; the atmospheric plasma spraying process parameters are shown in Table 5;
[0069] Ceramic layer (YSZ layer): The ceramic layer powder is sprayed on the bonding layer by an atmospheric plasma spraying process, and its thickness is the same as that of the ceramic layer in Example 1; wherein the ceramic layer powder is a spherical thin-walled hollow shell nano t′-YSZ powder; the atmospheric plasma spraying process parameters are shown in Table 6.
[0070] Gas thermal shock cycle experiment: The instrument used is the DWRZ03 thermal shock tester produced by Shaanxi Dewei Automation Co., Ltd. The thermal shock tester uses propane as fuel, oxygen as a combustion aid, and cooling gas for temperature control. Propane is pressurized and atomized by high-pressure inert gas and then pre-mixed with oxygen in the mixing chamber. Finally, the mixed gas enters the combustion chamber for combustion, and high-temperature and high-speed gas is sprayed out through a supersonic gas spray gun. The temperature is controlled by controlling the oxygen and propane gas content and the cooling gas flow rate, and the cooling gas is aimed at the back center of the coating. During the assessment, the heating time is 100s, the constant temperature time at 1750℃ is 120s, and the coating is cooled by cooling gas for 400s before thermal shock, and the cycle is repeated.
[0071] The repeatable ultra-high temperature thermal protective coating prepared in Example 1, the double-layer thermal protective coating prepared in Comparative Example 1, and the three-layer thermal protective coating prepared in Comparative Examples 2-3 were subjected to a 1750°C thermal shock cycle test, and the test parameters are shown in Table 7. The test results show that the repeatable ultra-high temperature thermal protective coating prepared in Example 1 was relatively intact after 60 thermal shocks under the 1750°C thermal shock test conditions, with only a little peeling at the edge of the coating, and no large-scale peeling ( Figure 5 ), the curve with 60 heat shocks still matches the curve with 10 heat shocks ( Figure 6), indicating that the coating can still be used normally after 60 tests at 1750°C. The coating has the advantage of being reusable. The vertical crack density of the coating increases with the number of tests. When the number of tests reaches 60, the vertical crack density of the coating reaches ~0.84mm -1 The average vertical crack depth reached 496 μm; the double-layer thermal protection coating of comparative example 1 was only maintained at 1750°C for 10 seconds before the entire coating peeled off. After peeling, the surface temperature of the coating dropped to about 1550°C under the action of cooling gas ( Figure 7 ); The three-layer thermal protection coating of Comparative Example 2 began to peel off after only one cycle at 1750°C, and failed during the second assessment ( Figure 8 ), the coating photos after failure are as follows Fig. 9 As shown, the coating cannot be reused at high temperature; the three-layer thermal protection coating of comparative example 3 peeled off in a large area after only one cycle at 1750°C, and failed during the second assessment ( Fig.10 ), the coating photos after failure are as follows Fig.11 As shown, the coating cannot be reused at high temperatures. Compared with comparative examples 1-3, the repeatable ultra-high temperature thermal protective coating of Example 1 of the present invention has better thermal shock resistance and achieves ultra-high temperature repeatability of the coating. This is attributed to the continuous interface of the coating prepared by the double powder feeding process, which has high-strength interface bonding ability. At the same time, the gradient structure of the intermediate layer 1 and the intermediate layer 2 alleviates the mismatch of the thermal expansion coefficient of the ceramic layer interface and improves the high temperature thermal shock resistance of the coating.
[0072] Table 7
[0073] Temperature / ℃ Propane flow / SLM Oxygen flow / SLM Cooling air flow H / h 1750 2.6 7.7 3500
[0074] XRD test: Place the sample in an aluminum plate and place it in parallel in an X-ray powder diffractometer, and perform tests at 2θ=10-90° and 2θ=72-76° respectively; the former is to determine whether the sample has a monoclinic phase (m), and the latter is to determine whether the sample has a cubic phase (c). The selected X-ray powder diffractometer is the X′Pert PRO model produced by PANalytical in the Netherlands. Fig.12 From the XRD diagrams of the repeatable ultra-high temperature thermal protective coating prepared in Example 1 after 60 times of 1750°C thermal shock test and in the deposited state (not tested), it can be seen that the grain size is reduced after the test. The particle size of the coating prepared by spraying is 72nm, and the particle size of the coating after 60 thermal shock tests is 44nm. No phase change occurs in the coating before and after the test.
[0075] Example 2
[0076] In this embodiment, the ceramic layer powder is pretreated before use, and the remaining steps are the same as those in Embodiment 1; wherein the specific method for pretreatment of the ceramic layer powder is: 0.83 Y 0.01 Ce 0.16 O2 and spherical thin-walled hollow shell nano t′-YSZ powder were mixed in a mass ratio of 5:5:90, deionized water and polyethylene glycol 4000 were added, mixed and ground for 1 hour, spray dried at 320 ° C and then heat treated to obtain a pretreated ceramic layer powder; wherein the mass of polyethylene glycol 4000 and HfO2, Zr 0.83 Y 0.01 Ce 0.16 The total mass ratio of O2 and spherical thin-walled hollow shell nano t′-YSZ powder is 1:50, and the mass of deionized water is 0.83 Y 0.01 Ce 0.16 The total mass ratio of O2 to spherical thin-walled hollow shell nano t′-YSZ powder is 1.2:1; the specific method of heat treatment is: heating to 400℃ at a heating rate of 5℃ / min, keeping warm for 1h, then heating to 600℃ at a heating rate of 5℃ / min, keeping warm for 1h, and naturally cooling to room temperature; Zr 0.83 Y 0.01 Ce 0.16 O2 is prepared by the preparation method described in Chinese patent CN2022100932710.
[0077] In this embodiment, a certain proportion of HfO2 and Zr are doped into t′-YSZ powder. 0.83 Y 0.01 Ce 0.16 O2 is beneficial to improve the bonding strength of the coating and improve the microstructure of the coating. Polyethylene glycol 4000 is used as an additive to improve the mixing uniformity between the powders. The coating formed by the powders during spraying is more uniform and stable, and the coating is less likely to peel off under high-temperature thermal shock. The repeatable ultra-high temperature thermal protective coating prepared in Example 2 was subjected to a 1750°C thermal shock cycle test, and the test parameters are shown in Table 7. Fig.13 As shown, after 60 thermal shocks, the coating was intact without peeling. Compared with Example 1, the repeatable ultra-high temperature thermal protective coating prepared in Example 2 has better thermal shock resistance.
[0078] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A repeatable ultra-high temperature thermal protective coating, characterized in that: include: A bonding layer is prepared on a substrate, an intermediate layer is prepared on the bonding layer, and a ceramic layer is prepared on the intermediate layer; wherein the number of the intermediate layers is ≥2.
2. A repeatable ultra-high temperature thermal protective coating as claimed in claim 1, characterized in that: The bonding layer is prepared by spraying bonding layer powder on the substrate using an atmospheric plasma spraying process, and the thickness of the bonding layer is 70 to 120 μm.
3. A repeatable ultra-high temperature thermal protective coating as claimed in claim 2, characterized in that: The bonding layer powder is Oerlikon Metco Amdry 962 brand NiCrAlY, and its composition is Ni22Cr10Al1.0Y.
4. A repeatable ultra-high temperature thermal protective coating as claimed in claim 3, characterized in that: The substrate is GH5188 alloy.
5. A repeatable ultra-high temperature thermal protective coating as claimed in claim 2, characterized in that: The preparation method of the intermediate layer is: using an atmospheric plasma spraying process, spraying the intermediate layer powder on the bonding layer to prepare a first intermediate layer, then spraying on the first intermediate layer to prepare a second intermediate layer, and continuing to spray to prepare an intermediate layer with a number of layers ≥ 2, each of which has a thickness of 80 to 150 μm.
6. A repeatable ultra-high temperature thermal protective coating as claimed in claim 5, characterized in that: The ceramic layer is prepared by spraying ceramic layer powder on the middle layer using an atmospheric plasma spraying process, and the thickness of the ceramic layer is 800-1000 μm.
7. A repeatable ultra-high temperature thermal protective coating as claimed in claim 6, characterized in that: The ceramic layer powder is spherical thin-walled hollow shell nano t′-YSZ powder.
8. A repeatable ultra-high temperature thermal protective coating as claimed in claim 7, characterized in that: The intermediate layer powder is obtained by mixing the bonding layer powder and the ceramic layer powder in a mass ratio of 1:0.5 to 5, and the bonding layer powder content in the intermediate layer powder gradually decreases as the number of intermediate layers increases, and the ceramic layer powder content gradually increases as the number of intermediate layers increases; wherein, the atmospheric plasma spraying process adopts a Y-type conveying pipe to deliver powder, and the bonding layer powder and the ceramic layer powder are independently and simultaneously delivered through the Y-type conveying pipe, and the powder delivery rate is adjusted so that the two powders are mixed according to the set mass ratio before entering the plasma flame zone.
9. A repeatable ultra-high temperature thermal protective coating as claimed in claim 8, characterized in that: The process parameters of the atmospheric plasma spraying are: current 400-600A, voltage 60-80V, nitrogen flow rate 40-60 liters / minute, hydrogen flow rate 3-5 liters / minute, spraying distance 100-150mm, bonding layer powder feeding rate 0-40g / min, ceramic layer powder feeding rate 0-35g / min, and gun speed 500-700mm / s.
10. A repeatable ultra-high temperature thermal protective coating according to any one of claims 1 to 9, characterized in that: The repeatable ultra-high temperature thermal protective coating was tested 60 times under a 1750° C. thermal shock condition, and the coating surface was intact without peeling.
Citation Information
Cited By
Multi-system powder enhanced thermal protection damping coating and preparation method thereof
CN121379331A
A multi-system powder reinforced thermal protection and vibration damping coating and a method for preparing the same
CN121379331B