Chemical heat treatment method for preparing titanium alloy through powder metallurgy
Through secondary chemical heat treatment and temperature control phase change principle, combined with the use of boron carbide and cerium oxide, a high-density fine needle-shaped α-phase matrix structure is formed, which solves the hardness and wear resistance of α-type or near-α-type powder metallurgical titanium alloys The problem of insufficient significantly improves its surface performance.
Patent Information
- Application Number
- CN202411151574.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively improve the hardness and wear resistance of α-type or near-α-type powder metallurgical titanium alloys, which limits its application in mechanical structures and wear-resistant components.
The secondary chemical heat treatment method is adopted to achieve the phase transformation of the β phase at high temperature through the principle of temperature control phase change, and a highly dense fine needle-shaped α-phase matrix structure is formed during the cooling process, and boron carbide and cerium oxide are used as chemical heat treatment reagents. , cerium oxide is added during the second chemical heat treatment to improve the surface hardness and wear resistance of the titanium alloy.
The hardness and wear resistance of powder metallurgy titanium alloys have been significantly improved, and the problems of low hardness and poor wear resistance of traditional powder metallurgy titanium alloys have been overcome, and the chemical heat treatment strength of α-type or near-α-type high-temperature titanium alloys have been improved.
Smart Images

Figure CN119020722A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a chemical heat treatment method for titanium alloy produced by powder metallurgy. Background Art
[0002] Mixed element powder metallurgy (PM) is one of the most effective methods for low-cost preparation of titanium alloy parts. PM technology has a series of advantages such as significant energy saving, material saving, excellent performance, high product precision, strong applicability and good stability. However, due to the presence of porosity (porosity less than 3%), PM products have lower hardness and wear resistance than corresponding forgings or castings, which seriously reduces the surface properties of powder metallurgy titanium alloys and limits the application of powder metallurgy titanium alloys in engineering.
[0003] In order to improve the hardness and wear resistance of titanium alloys made by powder metallurgy, the current research on titanium alloy surface strengthening focuses on laser surface strengthening technology, surface mechanical strengthening technology, surface deposition technology, surface chemical heat treatment technology, etc. Among them, surface chemical heat treatment technology is widely used due to its simple method, the formed coating is not easy to fall off and has good wear resistance, especially in the process of boronizing to form dual-phase ceramic materials (TiB and TiB 2 ) can greatly improve the hardness and wear resistance of the material surface, so it can be used as an effective means to improve the surface performance of powder metallurgy titanium alloys.
[0004] Near-α titanium alloys have excellent high-temperature creep resistance, good thermal stability, high strength-to-weight ratio and good corrosion resistance, and are widely used in aerospace engine components, aircraft partitions and ribs. At present, the research methods of surface chemical heat treatment of titanium alloys are mainly aimed at β and α+β titanium alloys, and there are few reports on surface chemical heat treatment methods for α or near-α alloys serving at high temperatures. Due to the large amount of α phase (HCP crystal) structure distributed in the alloy structure, it is difficult to achieve the effect of surface strengthening by conventional surface penetrant strengthening methods, which limits its wide application in wear-resistant parts such as certain mechanical structures, transmission gears, bearings and brakes.
[0005] Therefore, there is an urgent need to provide a method that can simultaneously improve the hardness and wear resistance of α-type or near-α-type powder metallurgy titanium alloys. Summary of the invention
[0006] In order to solve the above technical problems, the present invention proposes a chemical heat treatment method for powder metallurgy titanium alloy, which adopts a secondary chemical heat treatment method to realize the phase transformation of β phase at high temperature through the temperature-controlled phase transformation principle, and form a highly dense and fine needle-shaped α phase matrix structure during the cooling process, thereby further improving the surface hardness and wear resistance of the titanium alloy. It not only overcomes the problems of low hardness and poor wear resistance of traditional powder metallurgy titanium alloys, but also solves the problem that the strength of α-type and near-α-type high-temperature titanium alloys cannot be improved by chemical heat treatment.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] The technical solution of the present invention:
[0009] A chemical heat treatment method for titanium alloy produced by powder metallurgy, comprising the following steps:
[0010] The surface of the powder metallurgy titanium alloy is treated by secondary chemical heat treatment and room temperature cooling to synergistically improve its hardness and wear resistance;
[0011] The chemical heat treatment reagent used in the first chemical heat treatment is boron carbide (B 4 C);
[0012] The chemical heat treatment reagent used in the second chemical heat treatment is boron carbide (B 4 C) and cerium oxide (CeO 2 ) of the mixture; wherein the mass percentage of cerium oxide is 6%-8%.
[0013] Beneficial effect: Since powder metallurgy products generally have pores, the present invention performs a second chemical heat treatment on the basis of improving the density of the powder metallurgy titanium alloy by the first chemical heat treatment, which significantly improves the heat treatment effect and synergistically improves the hardness and wear resistance of the powder metallurgy titanium alloy. Specifically, the chemical heat treatment reagent used in the first chemical heat treatment does not add cerium oxide, the main purpose is to reduce the porosity of the powder metallurgy titanium alloy, but the wear resistance reflected by the first chemical heat treatment is not good, so in order to further improve the wear resistance of the titanium alloy, cerium oxide is added during the second chemical heat treatment to improve the chemical heat treatment effect.
[0014] Preferably, the powder metallurgy titanium alloy is α-type or near-α-type.
[0015] Preferably, the cerium oxide (CeO 2 ) is 6% or 8% by mass.
[0016] Beneficial effects: Cerium oxide is often used as a catalyst for chemical reactions due to its low electronegativity, strong chemical activity and strong reducing properties. Adding cerium oxide to chemical heat treatment reagents can promote the diffusion of surface active atoms into the body and improve the surface properties of the material.
[0017] Preferably, the method comprises the following steps:
[0018] (1) Pre-treating the surface of powder metallurgy titanium alloy;
[0019] (2) preparing chemical heat treatment reagents;
[0020] (3) placing the powder metallurgy titanium alloy treated in step (1) and the chemical heat treatment reagent prepared in step (2) into a mold for pressing and molding, then placing the molded sample into a corundum crucible, and then filling the corundum crucible with more than 50% of the volume of the chemical heat treatment reagent, sealing, and placing in a graphite container;
[0021] (4) placing the graphite container in a high temperature furnace for chemical heat treatment;
[0022] (5) Taking out the sample after chemical heat treatment and cooling it at room temperature, thus completing the first chemical heat treatment;
[0023] (6) Repeat steps (1) to (5) to perform a second chemical heat treatment.
[0024] The principle involved in the above technical solution is: due to the common porosity problem of powder metallurgy titanium alloy, the powder metallurgy titanium alloy exhibits problems such as low thickness of the infiltration layer, low hardness, and poor wear resistance when undergoing chemical heat treatment. Therefore, the present invention can effectively improve the density of powder metallurgy when performing a primary chemical heat treatment, so that the thickness of the infiltration layer and the wear resistance of the titanium alloy can be significantly improved when performing a secondary chemical heat treatment. Therefore, the present invention performs a secondary chemical heat treatment based on the primary chemical heat treatment, which effectively improves the chemical heat treatment effect and wear resistance of the powder metallurgy titanium alloy.
[0025] Preferably, the pretreatment includes grinding and polishing and ultrasonic cleaning; after the grinding and polishing, the roughness Ra of the surface of the powder metallurgy titanium alloy reaches 0.1-0.2 μm.
[0026] Beneficial effects: The powder metallurgy titanium alloy pretreatment defined in the present invention is mainly to remove oil, rust and oxide film on the surface of the titanium alloy to make the surface shiny.
[0027] Preferably, the preparation process of the chemical heat treatment reagent is: putting the chemical heat treatment reagent into a ball mill mixer and mixing the mixture so that the particle size of the chemical heat treatment reagent reaches 5-10 μm.
[0028] Preferably, the conditions in the mixing process are: putting the chemical heat treatment reagent into a planetary ball mill mixer, the ball-to-material ratio is 1:5, the mixer speed is 280-300 r / min, and the mixing time is 5-30 min.
[0029] Preferably, the mass ratio of the powder metallurgy titanium alloy treated in step (1) to the chemical heat treatment reagent prepared in step (2) is 1:5 to 1:10.
[0030] Preferably, in step (3), before pressing and molding, 50% of chemical heat treatment reagent, powder metallurgy titanium alloy and 50% of chemical heat treatment reagent are placed in the mold in the following order: 50% of the chemical heat treatment reagent is 50% of the total mass of the chemical heat treatment reagent, excluding the mass of the powder metallurgy titanium alloy.
[0031] Preferably, the pressure of the compression molding in step (3) is 25-30 MPa.
[0032] Preferably, the sealing process in step (3) uses high temperature resistant inorganic glue for sealing, and then stands to cure for 5-10 hours.
[0033] Preferably, the high temperature resistant inorganic glue is purchased directly from Shenzhen Xinwei Electronic Materials Factory and is made of off-white solid powder and white liquid in a ratio of 2:1.
[0034] Preferably, the chemical heat treatment process in step (4) is as follows: heating to 1000-1100° C. at a heating rate of 5-8° C. / min, and keeping at this temperature for 5-15 hours.
[0035] Beneficial effect: The present invention controls the chemical heat treatment temperature (T) to be close to the β phase transition temperature (T β =1020℃) β -50℃ <T<T β In the range of +100℃, this can not only accelerate the diffusion of boron atoms and improve the heat treatment effect, but also transform part of the α phase into the β phase, and form a needle-shaped martensite matrix structure in the subsequent high-temperature cooling process, thereby improving the surface hardness, wear resistance and density of the titanium alloy.
[0036] Compared with the prior art, the present invention has the following advantages and technical effects:
[0037] 1. Compared with the primary chemical heat treatment, the secondary chemical heat treatment adopted in the present invention can effectively increase the thickness of the boride and improve the wear resistance, thereby improving the effect of the chemical heat treatment.
[0038] 2. The temperature-controlled phase change principle is used to achieve the phase transformation of the β phase at high temperature, and a highly dense, fine, needle-shaped α phase matrix structure is formed during the cooling process to improve the wear resistance and hardness of the titanium alloy.
[0039] 3. The sample reagent is pressed into tablets using a press to increase the contact area between the titanium alloy surface and the boron element, thereby enhancing the chemical heat treatment.
[0040] 4. For powder metallurgy near-α titanium alloy, the wear resistance is improved by 58-60% when 6wt% and 8wt% of catalyst (cerium oxide) are used. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0042] Figure 1 This is a schematic diagram of X-ray diffractometer (XRD) detection of the titanium alloy after two chemical heat treatments in Example 1;
[0043] Figure 2 The titanium alloy layer after two chemical heat treatments in Example 1 (the dual-phase ceramic material TiB and TiB formed in the matrix after chemical heat treatment) 2 ) SEM schematic diagram;
[0044] Figure 3 This is a comparison chart of the wear resistance of titanium alloys after being treated in Example 1, Comparative Example 1 and Comparative Example 9;
[0045] Figure 4 This is a comparison chart of the hardness of the titanium alloys obtained by processing Example 1, Comparative Example 1, Comparative Example 4 and Comparative Example 6. DETAILED DESCRIPTION
[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0047] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0050] The present invention provides a chemical heat treatment method for titanium alloy produced by powder metallurgy, comprising the following steps:
[0051] (1) Pre-treating the surface of powder metallurgy titanium alloy;
[0052] (2) preparing chemical heat treatment reagents;
[0053] (3) Pressing and molding: placing the powder metallurgy titanium alloy treated in step (1) and the chemical heat treatment reagent prepared in step (2) into a mold for pressing and molding, and then sealing the powder metallurgy titanium alloy coated with the chemical heat treatment reagent and the remaining chemical heat treatment reagent together, and leaving them to stand for 5-10 hours;
[0054] (4) Chemical heat treatment: subjecting the chemical heat treatment reagent pressed and formed in step (3) to chemical heat treatment at a holding temperature of 1000-1100° C. for 5-15 h;
[0055] (5) Sampling and cooling, i.e., completing the first chemical heat treatment;
[0056] (6) Secondary chemical heat treatment: The sample in step (5) is subjected to secondary chemical heat treatment.
[0057] In one specific embodiment, in step (1), the pretreatment includes grinding and polishing and ultrasonic cleaning.
[0058] In a specific embodiment, after grinding and polishing, the roughness Ra of the surface of the powder metallurgy titanium alloy reaches 0.1-0.2μm. The method of grinding and polishing can be: first, use 80-2000 mesh sandpaper to grind the surface of the titanium alloy from low to high, so that the surface roughness Ra of the titanium alloy reaches 6.5-8μm, and then use 6000-15000 mesh diamond grinding paste to polish the surface of the titanium alloy on a polishing machine, wherein the polishing machine speed is 800-1200r / min, the pressure is 5-10N, and the surface roughness Ra of the titanium alloy reaches 0.1-0.2μm. This grinding and polishing method is only an example, as long as any grinding and polishing method that can achieve a roughness Ra of 0.1-0.2μm after grinding and polishing is within the protection scope of the present invention.
[0059] In one specific embodiment, in step (2), the chemical heat treatment reagent is a boron supply agent, and the boron supply agent is boron carbide (B 4 C).
[0060] In a specific embodiment, in step (2), the preparation process of the chemical heat treatment reagent is: placing the chemical heat treatment reagent into a planetary ball mill mixer, the ball-to-material ratio is 1:5, the mixer speed is 280-300r / min, the mixing time is 5-30min, so that the particle size of the chemical heat treatment reagent reaches 5-10μm.
[0061] In a specific embodiment, in step (3), the mass ratio of the powder metallurgy titanium alloy to the chemical heat treatment reagent is 1:5 to 1:10.
[0062] In a specific embodiment, in step (3), the following are placed in order from top to bottom: 50% chemical heat treatment reagent, powder metallurgy titanium alloy, and 50% chemical heat treatment reagent are placed in a mold for compression molding.
[0063] In a specific embodiment, the powder metallurgy titanium alloy after pretreatment in step (1) is in the form of a sheet. The size of the powder metallurgy product is: 12mm×10mm×3mm. The powder metallurgy near-α titanium alloy is recorded in terms of mass percentage as: Ti-5.1Al-2.0Sn-3.7Zr-0.3Mo.
[0064] In one specific embodiment, in step (3), the pressure during the compression molding process is 25-30 MPa.
[0065] In one specific embodiment, in step (3), before the chemical heat treatment, the pressed sample is placed at the bottom of a corundum crucible, and then filled with a chemical heat treatment reagent that accounts for more than 50% of the volume of the corundum crucible; finally, the corundum crucible is sealed with a high-temperature resistant inorganic glue, and then placed in a graphite container, and allowed to stand and solidify at room temperature for 5-10 hours;
[0066] Among them, the high-temperature resistant inorganic glue is a two-component inorganic aluminosilicate material, which is made of grayish white solid and white liquid in a ratio of 2:1, and has a heat resistance temperature of up to 1700℃.
[0067] In one specific embodiment, in step (4), the heating rate of the heating process is 5-8°C / min.
[0068] In a specific embodiment, in step (5), after the heat treatment of the sample is completed, the sample is immediately taken out of the high-temperature furnace and cooled at room temperature.
[0069] In a specific embodiment, in step (6), the sample taken out in step (5) needs to be surface treated, firstly, the particulate matter remaining on the surface of the sample after the first chemical heat treatment is removed, then the surface is polished with sandpaper, and finally the surface of the powder metallurgy titanium alloy is polished on a polishing machine with diamond grinding paste, the polishing machine speed is 800-1200r / min, the pressure is 8-10N, so that the surface roughness Ra reaches 0.1-0.2μm.
[0070] In one specific embodiment, in step (6), the preparation process of boron carbide in the chemical heat treatment reagent is consistent with step (2), except that the chemical heat treatment reagent used in the second chemical heat treatment process also includes 6-8% wt. cerium oxide.
[0071] In one specific embodiment, in step (6), the compression molding process is consistent with step (3).
[0072] In one specific embodiment, in step (6), the heat treatment process is consistent with step (4).
[0073] In one specific embodiment, in step (6), the cooling method is the same as that in step (5).
[0074] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0075] Example 1
[0076] A chemical heat treatment method for titanium alloy produced by powder metallurgy, comprising the following steps:
[0077] 1. The surface of the powder metallurgy near-α titanium alloy was pretreated to obtain a titanium alloy with a size of 12mm×10mm×3mm; the mass percentage was recorded as: Ti-5.1Al-2.0Sn-3.7Zr-0.3Mo. The specific pretreatment process is as follows:
[0078] First, the surface of the powder metallurgy titanium alloy is polished with sandpaper of 800 mesh, 1000 mesh, 1200 mesh and 1500 mesh respectively, so that the surface roughness Ra of the powder metallurgy titanium alloy reaches 6.5-8 μm, and then the surface of the powder metallurgy titanium alloy is polished on a polishing machine with diamond grinding paste of 4000 mesh, 6000 mesh and 10000 mesh, and the speed of the polishing machine is 1200 r / min and the pressure is 10N, so that the surface roughness Ra of the powder metallurgy titanium alloy reaches 0.1-0.2 μm; and the powder metallurgy titanium alloy material after grinding and polishing is cleaned with an ultrasonic cleaning machine;
[0079] 2. Preparation of Chemical Heat Treatment Reagents
[0080] Boron carbide powder (B 4 C) Mixing the materials in a planetary ball mill mixer (ball to material ratio of 1:5) at a speed of 300 r / min for 30 min to make the particle size reach 5-10 μm, in preparation for chemical reagent pressing and molding;
[0081] 3. Pressing
[0082] The chemical heat treatment reagent prepared in step 2 and the powder metallurgy titanium alloy pre-treated in step 1 are placed in a mold in a mass ratio of 8:1 (in order from top to bottom: 50% chemical heat treatment reagent, powder metallurgy titanium alloy, and 50% chemical heat treatment reagent) and pressed into shape at a molding pressure of 28Mpa, and then the molded sample is placed in a corundum crucible, and then filled with 80% of the volume of the corundum crucible. The chemical heat treatment reagent, finally, is used to seal the corundum crucible with a high-temperature resistant inorganic glue (a two-component inorganic aluminosilicate material, which is made of gray solid powder (alumina, silicon dioxide, zirconium dioxide, calcium carbonate) and white liquid sodium silicate in a mass ratio of 2:1, and the heat-resistant temperature reaches 1700°C), and the crucible is placed in a graphite container and left to stand for 10 hours at room temperature for solidification;
[0083] 4. First chemical heat treatment
[0084] The sealed graphite container in step 3 is placed in a high temperature furnace for high temperature heating at a heating rate of 7°C / min, and then kept warm after heating to 1000°C for 5 hours;
[0085] 5. Sampling and cooling
[0086] The sample in step 4 is taken out from the high temperature furnace and cooled at room temperature;
[0087] 6. Second chemical heat treatment
[0088] 1) Perform surface pretreatment on the sample after cooling in step 5
[0089] First, the residual particulate matter on the surface of the sample after the first chemical heat treatment was removed, and then the surface was polished with sandpaper. Finally, the surface of the powder metallurgy titanium alloy was polished on a polishing machine with a diamond grinding paste. The polishing machine speed was 1200r / min and the pressure was 10N, so that the surface roughness Ra reached 0.1-0.2μm;
[0090] 2) Boron carbide powder (B 4 C) Grind on a planetary ball mill to a particle size of 21-37 μm (400-650 mesh), then mix the ground boron carbide powder with rare earth powder (CeO) with a particle size of 5-10 μm in a fixed closed container. 2 ) are mixed uniformly; wherein CeO 2 The mass percentage of powder is 6%;
[0091] 3) placing the chemical heat treatment reagent prepared in step 2) and the powder metallurgy titanium alloy pre-treated in step 1) into a mold in a mass ratio of 8:1 (in order from top to bottom: 50% chemical heat treatment reagent, powder metallurgy titanium alloy, 50% chemical heat treatment reagent) and pressing them into shape; then placing the molded sample into a corundum crucible, and then filling it with 80% of the volume of the corundum crucible with chemical heat treatment reagent, and finally sealing the corundum crucible with a high temperature resistant inorganic glue, placing it in a graphite container, and standing it at room temperature for 10 hours;
[0092] 4) placing the graphite container of step 3) in a high temperature furnace for high temperature heating at a heating rate of 8°C / min, heating to 1100°C and then keeping the temperature for 15h.
[0093] 5) Take samples and cool them down.
[0094] According to the test, the friction coefficient of the powder metallurgy titanium alloy after the secondary chemical heat treatment of this embodiment is 0.70.
[0095] Figure 1 The X-ray diffractometer (XRD) detection schematic diagram of the titanium alloy after two chemical heat treatments in Example 1; it can be seen from the figure that the diffusion layer is mainly composed of dual-phase TiB 2 peak and TiB peak;
[0096] Figure 2 This is a SEM schematic diagram of the titanium alloy diffusion layer after two chemical heat treatments in Example 1; it can be seen from the figure that the titanium alloy diffusion layer forms a highly dense fine needle-shaped α-phase matrix structure, which can improve the wear resistance and hardness of the titanium alloy;
[0097] The following are comparative examples 1-9, which adopt the same method as Example 1, except for the chemical heat treatment time, temperature, catalyst content, molding pressure, and cooling method. The various parameters in comparative examples 1-9 are summarized as shown in Table 1. (In Table 1, comparative example 1 is an untreated original titanium alloy; comparative examples 2-9 are one chemical heat treatment; and Example 1 is two chemical heat treatments)
[0098] Table 1
[0099]
[0100] The performance comparison of the powder metallurgy titanium alloys after treatment in Example 1 and Comparative Examples 1-9 is shown in Table 2.
[0101] Table 2 Performance comparison of samples prepared in Example 1 and Comparative Examples 1-9
[0102]
[0103] It can be seen from Table 2 that the performance of the powder metallurgy titanium alloy treated by the surface strengthening method of the present invention is higher than that of the original powder metallurgy titanium alloy. This is because a large amount of α phase is transformed into β phase during the high-temperature chemical heat treatment process, and a large amount of high-density acicular martensitic matrix structure is generated during the cooling process. These high-density acicular martensitic matrix structures not only improve the hardness and wear resistance of the sample, but also reduce the porosity of the powder metallurgy titanium alloy, thereby greatly improving the service life of the powder metallurgy titanium alloy.
[0104] Figure 3 The figure is a comparison chart of the wear resistance of the titanium alloys after being treated in Example 1, Comparative Example 1 and Comparative Example 9; it can be seen from the figure that the wear resistance of the titanium alloy after the secondary chemical heat treatment in Example 1 of the present invention is better than that in Comparative Example 9 and the original titanium alloy;
[0105] Figure 4 It is a hardness comparison chart of the titanium alloy obtained by Example 1, Comparative Example 1, Comparative Example 4, Comparative Example 6 and Example 1 after one heat treatment (Step 1 to Step 5 of Example 1); it can be seen from the figure that the hardness of the titanium alloy after two heat treatments of Example 1 of the present invention is significantly improved, and it is found through Comparative Examples 4 and Comparative Examples 6 that increasing the chemical heat treatment temperature can significantly improve the hardness of the titanium alloy.
[0106] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A chemical heat treatment method for titanium alloy produced by powder metallurgy, characterized in that: The following steps are involved: The surface of powder metallurgy titanium alloy is treated by secondary chemical heat treatment and room temperature cooling to improve its hardness and wear resistance; The chemical heat treatment reagent used in the first chemical heat treatment is boron carbide; The chemical heat treatment reagent used in the second chemical heat treatment is a mixture of boron carbide and cerium oxide, wherein the mass percentage of cerium oxide is 6%-8%.
2. The chemical heat treatment method of powder metallurgy titanium alloy according to claim 1, characterized in that: The powder metallurgy titanium alloy is α-type or nearly α-type.
3. The chemical heat treatment method of titanium alloy produced by powder metallurgy according to claim 1, characterized in that: The following steps are involved: (1) Pre-treating the surface of powder metallurgy titanium alloy; (2) preparing chemical heat treatment reagents; (3) placing the powder metallurgy titanium alloy treated in step (1) and the chemical heat treatment reagent prepared in step (2) into a mold for pressing and molding, then placing the molded sample into a corundum crucible, and then filling the corundum crucible with more than 50% of the volume of the chemical heat treatment reagent, sealing, and placing in a graphite container; (4) placing the graphite container in a high temperature furnace for chemical heat treatment; (5) Taking out the sample after chemical heat treatment and cooling it at room temperature, thus completing the first chemical heat treatment; (6) Repeat steps (1) to (5) to perform a second chemical heat treatment.
4. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 3, characterized in that: The pre-treatment includes grinding and polishing and ultrasonic cleaning; After the grinding and polishing, the roughness Ra of the surface of the powder metallurgy titanium alloy is 0.1-0.2 μm.
5. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 3, characterized in that: The preparation process of the chemical heat treatment reagent in step (2) is as follows: the chemical heat treatment reagent is placed in a planetary ball mill mixer and mixed to make the particle size of the chemical heat treatment reagent reach 5-10 μm.
6. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 5, characterized in that: The conditions in the mixing process are: the ball-to-material ratio is 1:5, the mixer speed is 280-300 r / min, and the mixing time is 5-30 min.
7. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 3, characterized in that: The mass ratio of the powder metallurgy titanium alloy treated in step (1) to the chemical heat treatment reagent prepared in step (2) is 1:5 to 1:
10.
8. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 3, characterized in that: In step (3), before compression molding, 50 wt.% chemical heat treatment reagent, powder metallurgy titanium alloy and 50 wt.% chemical heat treatment reagent are placed in the mold from bottom to top in this order.
9. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 8, characterized in that: The pressure of the compression molding is 25-30MPa.
10. The chemical heat treatment method for titanium alloy produced by powder metallurgy according to claim 3, characterized in that: The chemical heat treatment process in step (4) is: heating to 1000-1100°C at a heating rate of 5-8°C / min, and keeping at this temperature for 5-15h.