Flexible substrate photo-thermal conversion film and preparation method and application thereof

By forming Cu and Ag doped MoS2 composite film on the flexible cotton fabric substrate and performing heat treatment, the problems of low absorption and high emissivity of the flexible photothermal conversion materials are solved, and efficient photothermal conversion efficiency and good flexibility are achieved suitable for wearable electronic devices.

CN119020740APending Publication Date: 2024-11-26SHAANXI UNIV OF SCI & TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410937825.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing flexible photothermal conversion materials have problems such as low absorption, high emissivity and low photothermal conversion efficiency, which limit their performance in practical applications, especially in wearable electronic devices.

Method used

Co-sputtering method is used to form Cu and Ag-doped MoS2 composite film on the flexible cotton fabric substrate, and its photothermal performance is optimized through heat treatment, the doping concentration and distribution of Cu and Ag are controlled, and the flexibility and photothermal conversion of the film are improved. efficiency.

Benefits of technology

It achieves efficient photothermal conversion efficiency. The maximum surface temperature of the film can reach 85℃ at 1sun, the photothermal conversion efficiency reaches more than 82%, and has good durability and flexibility, which is suitable for wearable electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a flexible substrate photothermal conversion film and a preparation method and application thereof, and belongs to the technical field of photothermal conversion film preparation. According to the preparation method disclosed by the invention, a Cu, Ag and MoS2 atom co-sputtering method is adopted, the Cu and Ag doped MoS2 composite film is formed on the surface of the flexible substrate, and the flexible substrate and a co-sputtering method preparation process are adopted, so that the film has excellent flexibility and bendability and is suitable for the fields of wearable electronic equipment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photothermal conversion film preparation, and specifically relates to a flexible substrate photothermal conversion film and a preparation method and application thereof. Background Art

[0002] With the rapid development of wearable electronic Internet of Things, flexible photothermal conversion materials have attracted much attention due to their unique advantages. However, existing flexible photothermal conversion materials often have problems such as low absorptivity, high emissivity, and low photothermal conversion efficiency, which limits their performance in practical applications. Therefore, the development of an efficient and stable flexible photothermal conversion material is of great practical significance.

[0003] In recent years, molybdenum disulfide (MoS2), as a typical two-dimensional layered material, has attracted much attention due to its excellent optical, electrical and mechanical properties. However, the photothermal conversion efficiency of pure MoS2 is limited, and performance optimization needs to be achieved through doping and other means. Silver (Ag) and copper (Cu), as common metal doping elements, can effectively improve the light absorption capacity and photothermal conversion efficiency of MoS2. In this study, Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 co-doped photothermal conversion films were successfully prepared on a flexible cotton substrate by co-sputtering. This method not only achieves the effective combination of metal elements and MoS2, but also ensures the flexibility and lightness of the film. By precisely controlling the sputtering conditions, the doping amount and distribution of metal elements in the film can be regulated to optimize its photothermal performance.

[0004] For example, the Chinese patent application with publication number CN 110408158 A discloses a carbon nanotube-based photothermal conversion material and its preparation method. The material uses the excellent thermal conductivity and light absorption properties of carbon nanotubes to achieve efficient photothermal conversion. According to the patent, the prepared photothermal conversion material can rapidly increase its surface temperature under specific lighting conditions and has high photothermal conversion efficiency and stability. However, despite the breakthrough in performance of carbon nanotube-based photothermal conversion materials, their preparation cost is high and their flexibility still needs to be improved in certain application scenarios. Summary of the invention

[0005] The object of the present invention is to provide a flexible substrate photothermal conversion film and a preparation method and application thereof, so as to solve the technical problem that the existing photothermal conversion films used on flexible substrates have poor flexibility.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing a flexible substrate light-to-heat conversion film, comprising the following steps:

[0008] Co-sputtering Cu, Ag and MoS2 atoms onto a flexible substrate to form a Cu- and Ag-doped MoS2 composite film on the flexible substrate;

[0009] The Cu and Ag doped MoS2 composite film is then heat treated to obtain a flexible substrate photothermal conversion film.

[0010] Furthermore, before the Cu, Ag and MoS2 atoms are co-sputtered onto the flexible substrate, the flexible substrate is cleaned by ultrasonic cleaning for 20 min to 30 min.

[0011] Furthermore, the flexible substrate is one of cotton cloth, polyimide film or polyester film.

[0012] Furthermore, the surface roughness of the flexible substrate is less than 30 nm; the co-sputtering time is 20 to 40 minutes, and the power is 90 to 110 W.

[0013] Furthermore, the co-sputtering of Cu, Ag and MoS2 atoms is performed by co-sputtering a Cu target, an Ag target and a MoS2 target; the distances between the Cu target, the Ag target and the MoS2 target and the substrate are 7 to 10 cm respectively.

[0014] Furthermore, the vacuum degree during the co-sputtering is >1×10^-4Pa, and the gas pressure is 0.8Pa~1.0Pa; in the Cu- and Ag-doped MoS2 composite film, the Cu doping concentration is 1%~5%, and the Ag doping concentration is 0.5%~3%, calculated in atomic percentage.

[0015] Furthermore, the heat treatment is an annealing treatment; the temperature of the annealing treatment is 400-600°C and the time is 1-2h.

[0016] The invention also discloses a flexible substrate light-to-heat conversion film prepared by the above preparation method.

[0017] Furthermore, when the Cu doping concentration in the Cu- and Ag-doped MoS2 composite film is 3% and the Ag doping concentration is 2%, the maximum surface temperature of the flexible substrate photothermal conversion film under 1 sun is 85°C, and the photothermal conversion efficiency reaches more than 82%.

[0018] The present invention also discloses the application of the above-mentioned flexible substrate light-heat conversion film in wearable electronic devices.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention discloses a method for preparing a flexible substrate light-heat conversion film, which adopts a method of co-sputtering of Cu, Ag and MoS2 atoms to form a Cu- and Ag-doped MoS2 composite film on the surface of a flexible substrate. The flexible substrate and co-sputtering preparation process are adopted to make the film have excellent flexibility and bendability, and is suitable for fields such as wearable electronic devices.

[0021] Furthermore, the present invention achieves high absorptivity, low emissivity and efficient light-to-heat conversion capability of the film by optimizing the doping concentrations of Cu and Ag. The film maintains stable performance after mechanical treatment and has good durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is an EDS image of the flexible substrate light-to-heat conversion film prepared in Example 1 of the present invention;

[0023] Figure 2 The temperature variation curve of metal-doped MoS2 thin film on flexible substrate under different light intensities;

[0024] Among them: a-0.5sun; b-1sun; c-1.5sun; d-infrared photo;

[0025] Figure 3 Schematic diagram of the wear and stretching process;

[0026] Figure 4 The temperature change curve, infrared image and contact angle image of the metal-doped MoS2 thin film tape on cotton cloth prepared in Example 1 before and after being adhered and torn 100 times under 1 sun;

[0027] Among them: a1~a2: Ag-MoS2; b1~b2: Cu-MoS2; c1~c2: Ag-Cu-MoS2. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0033] The present invention provides a method for preparing a flexible substrate photothermal conversion film, which adopts a co-sputtering method to deposit Cu, Ag and MoS2 target materials on a flexible substrate, and realizes precise control of the doping concentration of Cu and Ag by controlling the sputtering power, sputtering time and the distance between the target materials.

[0034] The main steps include:

[0035] Preparation of flexible substrate: Select materials with excellent flexibility and thermal stability as the substrate, such as cotton cloth, polyimide (PI) film or polyester (PET) film, etc. Clean the flexible substrate to remove surface impurities and ensure that the substrate is flat and smooth;

[0036] Preparation of target materials: Prepare Cu, Ag and MoS2 targets respectively to ensure that the purity and quality of the targets meet the preparation requirements;

[0037] Preparation of thin films by co-sputtering: Place a flexible substrate in a vacuum chamber of a sputtering device, install Cu, Ag and MoS2 targets at corresponding positions of a sputtering gun, adjust the power of the sputtering gun so that Cu, Ag and MoS2 atoms are co-sputtered onto the flexible substrate in a certain proportion, and control the sputtering time to form a Cu- and Ag-doped MoS2 composite film;

[0038] Annealing treatment: The prepared Cu and Ag doped MoS2 composite film is placed in an annealing furnace for high temperature annealing treatment. The annealing temperature is controlled at 400-600°C and the holding time is 1-2 hours. Through the annealing treatment, the crystallization of the film and the uniform distribution of the doping atoms are promoted, thereby improving the photothermal conversion performance of the film.

[0039] Preferably, the surface roughness of the flexible substrate is <30 nm.

[0040] Preferably, the vacuum degree in the deposition chamber is >1×10^-4Pa.

[0041] Preferably, the ultrasonic cleaning time is 20 min to 30 min.

[0042] Preferably, the working gas pressure is 0.8Pa-1.0Pa.

[0043] Preferably, the sputtering power is 90-110 W, and the sputtering time is 20-40 min.

[0044] like Figure 2 As shown in the figure, by precisely controlling the doping concentrations of Cu and Ag, the film performance is optimized. When the Cu doping concentration is 3% and the Ag doping concentration is 2%, the maximum surface temperature of the film can reach 96.2°C under 1sun, the photothermal conversion efficiency reaches more than 82%, and it has good durability.

[0045] Performance testing and characterization:

[0046] The prepared Cu and Ag co-doped MoS2 photothermal conversion film was subjected to performance tests, including absorptivity, emissivity, photothermal conversion efficiency, etc. The optical and thermal properties of the film were characterized by using spectrometers, infrared thermal imagers and other equipment. At the same time, the film was subjected to mechanical property tests to evaluate its practical application performance in wearable electronic devices and other fields. Performance tests were carried out, including absorptivity, emissivity, photothermal conversion efficiency, etc. The optical and thermal properties of the film were characterized by using spectrometers, infrared thermal imagers and other equipment. At the same time, the film was subjected to mechanical property tests to evaluate its practical application performance in wearable electronic devices and other fields.

[0047] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0048] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0049] Example 1

[0050] A method for preparing a flexible substrate light-to-heat conversion film comprises the following steps:

[0051] Select a material with excellent flexibility and thermal stability as the substrate, such as cotton cloth, polyimide (PI) film or polyester (PET) film, etc. In this embodiment, polyimide is used; the polyimide substrate is ultrasonically cleaned for 20 minutes to remove surface impurities and ensure that the substrate is flat and smooth with a roughness of less than 30nm;

[0052] Prepare Cu, Ag and MoS2 targets respectively to ensure that the purity and quality of the targets meet the preparation requirements.

[0053] (Purity: 99.99%);

[0054] The flexible substrate was placed in the vacuum chamber of the sputtering equipment, and the Cu, Ag and MoS2 targets were installed at the corresponding positions of the sputtering gun. The sputtering gun power was adjusted to 100 W and the sputtering time was 30 min, so that Cu, Ag and MoS2 atoms were co-sputtered onto the flexible substrate in a certain proportion to form a Cu- and Ag-doped MoS2 composite film.

[0055] The prepared Cu and Ag-doped MoS2 composite film was placed in an annealing furnace for high-temperature annealing treatment. The annealing temperature was controlled at 400°C and the holding time was 1.5 hours. The annealing treatment promoted the crystallization of the film and the uniform distribution of doped atoms, improved the photothermal conversion performance of the film, and finally obtained a flexible substrate photothermal conversion film (Ag-Cu-MoS2 film).

[0056] In this embodiment, the Cu doping concentration in the Cu-Ag doped MoS2 composite film is 3%, and the Ag doping concentration is 2%.

[0057] The prepared flexible substrate wear-resistant Ag-Cu-MoS2 film was tested for performance, including absorptivity, emissivity, photothermal conversion efficiency, etc. The optical and thermal properties of the film were characterized using spectrometers, infrared thermal imagers and other equipment. At the same time, the film was tested for mechanical properties to evaluate its practical application performance in wearable electronic devices and other fields.

[0058] EDS images of Ag-Cu-MoS2 films are shown in Figure 1. There are many small particles distributed on the surface. From the yellow-green color of the mapping diagram, it can be seen that the particles are mainly Ag, Cu and S elements. A large amount of O elements can be observed on the surface of the large particle polymer, which indicates that the Ag and Cu atoms on the surface of the film are concentrated on the surface and react with O2 in the air to form oxides. Similarly, the Mo element is difficult to observe on the surface. The analysis of the relevant element content from high to low shows that the proportions of Ag, O, S, Cu, and Mo are 33.52%, 23.45%, 18.91%, 12.78% and 11.734% respectively. The degree of oxidation of the film is slightly lighter, and the content of Cu particles is much lower than that of Ag particles. This may be because when the three targets are co-sputtered, although Cu is more active than Ag, the magnetic field of Ag is stronger than that of Cu. At the same time, the magnetic field of the Cu target is weaker and less likely to be sputtered using the RF power supply. Therefore; for the Ag-Cu-MoS2 film, the internal Ag and Cu atoms diffuse to the surface of the film, resulting in a large number of Ag NPs and Cu NPs distributed on the surface, which are easy to react with O2 in the air to form oxides.

[0059] Example 2

[0060] A method for preparing a flexible substrate light-to-heat conversion film comprises the following steps:

[0061] A piece of polyimide (PI) film with a size of 10cm x 10cm was selected as a flexible substrate. The PI substrate was immersed in ethanol and ultrasonically cleaned for 25 minutes using an ultrasonic cleaner to remove oil and impurities on the surface. Subsequently, the PI substrate was rinsed with deionized water to ensure that the ethanol was completely removed. Finally, the surface of the PI substrate was blown dry with nitrogen and placed on a dust-free clean bench for standby use to ensure that the substrate was flat and smooth with a roughness of <30nm.

[0062] Prepare Cu, Ag and MoS2 targets respectively to ensure that the purity and quality of the targets meet the preparation requirements.

[0063] (Purity: 99.99%);

[0064] The flexible substrate was placed in the vacuum chamber of the sputtering equipment, and the Cu, Ag and MoS2 targets were installed at the corresponding positions of the sputtering gun. The sputtering gun power was adjusted to 100W and the sputtering time was 30min, so that Cu, Ag and MoS2 atoms were co-sputtered onto the flexible substrate in a certain proportion to form a Cu- and Ag-doped MoS2 composite film; the Cu doping concentration was 2%, and the Ag doping concentration was 1.5%;

[0065] The prepared Cu and Ag doped MoS2 composite film is placed in an annealing furnace for high-temperature annealing treatment. The annealing temperature is set to 500°C and maintained for 1.5 hours. The annealing treatment promotes the crystallization of the film and the uniform distribution of doped atoms, thereby improving the photothermal conversion performance of the film, and finally obtaining a flexible substrate photothermal conversion film (Ag-Cu-MoS2 film).

[0066] Example 3

[0067] A method for preparing a flexible substrate light-to-heat conversion film comprises the following steps:

[0068] A piece of polyimide (PI) film with a size of 10cm x 10cm was selected as a flexible substrate. The PI substrate was immersed in ethanol and ultrasonically cleaned for 25 minutes using an ultrasonic cleaner to remove oil and impurities on the surface. Subsequently, the PI substrate was rinsed with deionized water to ensure that the ethanol was completely removed. Finally, the surface of the PI substrate was blown dry with nitrogen and placed on a dust-free clean bench for standby use to ensure that the substrate was flat and smooth with a roughness of <30nm.

[0069] Prepare Cu, Ag and MoS2 targets respectively to ensure that the purity and quality of the targets meet the preparation requirements.

[0070] (Purity: 99.99%);

[0071] The flexible substrate was placed in the vacuum chamber of the sputtering equipment, and the Cu, Ag and MoS2 targets were installed at the corresponding positions of the sputtering gun. The sputtering gun power was adjusted to 100W and the sputtering time was 40min, so that Cu, Ag and MoS2 atoms were co-sputtered onto the flexible substrate in a certain proportion to form a Cu- and Ag-doped MoS2 composite film; the Cu doping concentration was 2%, and the Ag doping concentration was 1.5%;

[0072] The prepared Cu and Ag doped MoS2 composite film is placed in an annealing furnace for high-temperature annealing treatment. The annealing temperature is set to 500°C and maintained for 1.5 hours. The annealing treatment promotes the crystallization of the film and the uniform distribution of doped atoms, thereby improving the photothermal conversion performance of the film, and finally obtaining a flexible substrate photothermal conversion film (Ag-Cu-MoS2 film).

[0073] Example 4

[0074] Different from Example 2, in this embodiment, the annealing temperature is 600° C., the time is 1.5 h, and the other steps and parameters remain unchanged to obtain a flexible substrate photothermal conversion film (Ag-Cu-MoS2 film).

[0075] Example 5

[0076] Different from Example 2, a polyester (PET) film is used as a flexible substrate in this embodiment. First, the PET substrate is ultrasonically cleaned in the same way as the PI substrate in Example 2. After cleaning, the surface of the PET substrate is dried with nitrogen and placed on a dust-free clean bench for standby use; the remaining steps and parameters remain unchanged to obtain a flexible substrate photothermal conversion film (Ag-Cu-MoS2 film).

[0077] Comparative example: Preparation of Ag / Cu doped MoS2 thin film by magnetron sputtering

[0078] Before coating, the substrate is surface treated. First, the substrate material (Al wafer, silicon wafer) is placed in an ethanol solution for ultrasonic cleaning for 30 minutes, then placed in the vacuum chamber of the coating machine, and the bias cleaning is turned on for 20 minutes. Both ultrasonic and bias cleaning are to remove impurities on the substrate surface and improve the bonding strength and density of the film. During the entire deposition process, the substrate heating temperature is kept at 200°C, the argon flow rate is 107sccm, the MoS2 target power is 200W, the Ag (Cu) target power is 30W, and the working pressure is set to 0.6~1.0Pa. Through this deposition method, Ag (Cu) doped MoS2 films under different working pressures are obtained.

[0079] The surface temperature variation diagram of Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 films is shown in Figure 2 . By measuring the real-time temperature of the flexible metal-doped MoS2 film under simulated different solar illumination conditions, it can be used to evaluate the photothermal conversion ability of the film. As the illumination time increases, the surface temperature of the film slowly rises to the maximum temperature and maintains it. The maximum temperatures of the Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 film surfaces under 1 sun are 96.2℃, 88.4℃ and 90.7℃ respectively; obviously, the film itself has good photothermal absorption performance. Figure 2 d is the infrared photos of Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 films under different sunlight. Under 1 sun, the infrared temperatures of Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 films are 90.5℃, 84.4℃ and 82.5℃ respectively; due to the high thermal emissivity of cotton cloth, the infrared temperature is not much different from the actual temperature, but it can still be seen that the temperature difference of Ag-Cu-MoS2 film is greater than that of Ag-MoS2 and Cu-MoS2 films, indicating that the selective absorption ability of Ag-Cu-MoS2 film is stronger.

[0080] The temperature change curve, infrared image and contact angle image of Ag-Cu-MoS2 film before and after wear are shown in Figure 3-4 ; Use 400-grit sandpaper to rub the film surface. Figure 4(a1), (b1), and (c1) are the temperature change curves of the Ag-MoS2, Cu-MoS2, and Ag-Cu-MoS2 film surfaces, respectively. Compared with the samples without adhesion and tearing, except for the Ag-MoS2 film, which has a larger temperature drop, the temperature difference of the other samples is not much, and the rate of temperature rise and fall of the film after sandpaper friction is the same as before.

[0081] Figure 4 (a2), (b2), (c2) Photos of the samples before and after wear, infrared camera photos when heated to the highest temperature, and contact angle diagrams. The surface of the sample becomes rough after wear, and the fibrous tissue can be observed with the naked eye. The color changes from the original black gray to light gray, which has a certain effect on the light absorption of the film. The infrared camera photos show that the maximum temperatures of Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 films at 1sun before wear are 86.6℃, 90.5℃, and 89.9℃, respectively, and the temperatures after wear are 82.2℃, 89.9℃, and 82.4℃, respectively, with little change. Comparing the contact angle diagrams of the samples before and after wear, the contact angles of Ag-MoS2, Cu-MoS2 and Ag-Cu-MoS2 films before wear are 138.5°, 151.2°, and 152.9°, respectively, and the contact angle temperatures after wear are 144.2°, 169.5°, and 158.8°, respectively. The contact angle of the sample after tearing increases significantly, because the surface fiber structure is destroyed, resulting in an increase in surface roughness, but the film is still relatively stable, so the contact angle increases significantly. This shows that the overall structure of the film is not destroyed after the wear treatment, and it can still maintain good photothermal conversion performance and photothermal stability.

[0082] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a flexible substrate light-to-heat conversion film, characterized in that: The following steps are involved: Co-sputtering Cu, Ag and MoS2 atoms onto a flexible substrate to form a Cu- and Ag-doped MoS2 composite film on the flexible substrate; The Cu and Ag doped MoS2 composite film is then heat treated to obtain a flexible substrate photothermal conversion film.

2. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: Before the Cu, Ag and MoS2 atoms are co-sputtered onto the flexible substrate, the flexible substrate is cleaned by ultrasonic cleaning for 20 min to 30 min.

3. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: The flexible substrate is one of cotton cloth, polyimide film or polyester film.

4. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: The surface roughness of the flexible substrate is less than 30nm; the co-sputtering time is 20 to 40 minutes, and the power is 90 to 110W.

5. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: The co-sputtering of Cu, Ag and MoS2 atoms is carried out by co-sputtering a Cu target, an Ag target and a MoS2 target; the distances between the Cu target, the Ag target and the MoS2 target and the substrate are 7 to 10 cm respectively.

6. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: The vacuum degree during the co-sputtering is >1×10^-4Pa, and the gas pressure is 0.8Pa~1.0Pa; In the Cu-Ag doped MoS2 composite film, the Cu doping concentration is 1% to 5%, and the Ag doping concentration is 0.5% to 3%, calculated in atomic percentage.

7. The method for preparing a flexible substrate light-to-heat conversion film according to claim 1, characterized in that: The heat treatment is annealing; the temperature of the annealing is 400-600°C and the time is 1-2h.

8. A flexible substrate light-to-heat conversion film, characterized in that: The preparation method is described in any one of claims 1 to 6.

9. The flexible substrate light-to-heat conversion film according to claim 8, characterized in that: When the Cu doping concentration in the Cu- and Ag-doped MoS2 composite film is 3% and the Ag doping concentration is 2%, the maximum surface temperature of the flexible substrate photothermal conversion film under 1 sun is 85°C, and the photothermal conversion efficiency reaches more than 82%.

10. Use of the flexible substrate photothermal conversion film according to claim 8 or 9 in wearable electronic devices.

Citation Information

Patent Citations

  • Preparation method of thermal shrinkage film with high degradation rate

    CN110408158A

  • Petal-like molybdenum disulfide film as well as preparation method and application thereof

    CN108893974A

  • Preparation method of two-dimensional molybdenum disulfide thin film

    CN110344000A

  • Flexible photo-thermal conversion composite film as well as preparation method and application thereof

    CN110669304A

  • Metal-doped molybdenum disulfide super-smooth film and preparation method thereof

    CN113088911A