Preparation method of low-stress cutting tool coating
The Cr-CrN composite coating was prepared by high-power pulse magnetron sputtering technology, and the ratio of metal ions to inert gas ions in the plasma was adjusted, which solved the problem that residual stress and overall performance in the cutting tool coating was difficult to meet at the same time, and achieved the Lower stress coating and higher service life.
Patent Information
- Application Number
- CN202411090238.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
AI Technical Summary
现有技术难以在切削刀具涂层中同时降低残余应力和提高整体性能,导致涂层在使用过程中容易剥落或开裂,影响刀具的可靠性和使用寿命。
The Cr-CrN composite coating is prepared by high-power pulsed magnetron sputtering technology. By adjusting the ratio of metal ions to inert gas ions in the plasma, the residual stress of the coating is reduced, and the hardness, elastic modulus of the coating is improved. Binding power.
It significantly reduces the residual stress of the coating, improves hardness, elastic modulus and bonding force, extends the service life of the tool, and improves the overall performance of the coating, solving the problem of increased stress when the coating thickness increases.
Smart Images

Figure CN119020742A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tool manufacturing, and in particular to a method for preparing a low-stress cutting tool coating. Background Art
[0002] The vapor deposition technology is used to deposit refractory metal or non-metallic compound coatings on the surface of tools such as cemented carbide, high-speed steel (HSS) and ceramics to improve the surface properties of the materials, solve the damage and wear problems under high-speed cutting, heavy cutting and extremely high-speed and high-temperature processing conditions, and effectively increase the reliability and service life of cutting tools. Tool coatings should have high surface hardness, good wear resistance, heat resistance and oxidation resistance. However, during the service process, the coating often fails due to unstable factors such as peeling or cracking. A large number of industrial examples and studies have shown that the high residual stress generated during the preparation process of the coating is the main reason for its failure.
[0003] As early as the 1990s, some scholars proposed that during the deposition process of coatings, high-energy inert gas ions (Ar + ) clamping at lattice defects or interstitial positions will cause excessive residual compressive stress in the coating, while metal ions (film-forming ions) can reduce the growth stress generated during the deposition process because they are mainly combined at lattice positions, and metal ion irradiation also has all the advantages of inert gas ion bombardment.
[0004] At present, there are two main directions for preparing low stress coatings:
[0005] First, from the perspective of coating structure design, for example, Chinese patent CN116180075A uses an alternating multilayer structure to release the internal stress of the coating by combining soft and hard methods. However, this method generally requires the coating to have a large thickness and the process flow is relatively complicated.
[0006] The second is from the perspective of coating deposition parameters. For example, CN108411265A uses magnetron sputtering technology, which reduces the ion bombardment energy by reducing the bias voltage, thereby reducing the coating stress. For magnetron sputtering, the size of the ion bombardment energy affects the coating density and mechanical properties such as hardness and elastic modulus. The low-stress coating obtained by reducing the ion bombardment energy will inevitably suffer a loss in overall performance. Therefore, it is necessary to propose a new method for preparing a low-stress coating.
[0007] To sum up, it is necessary to make further innovations on existing technologies. Summary of the invention
[0008] In view of the technical problems existing in the above-mentioned background technology, the present invention proposes a method for preparing a low-stress cutting tool coating. The method has a reasonable concept and utilizes a high-power pulsed magnetron sputtering method to prepare a Cr-CrN composite coating. While reducing the residual stress of the coating, the hardness, elastic modulus and bonding strength of the coating are improved, thereby solving the problem that the residual stress and overall performance of the current cutting tool coating are difficult to meet industrial requirements at the same time.
[0009] In order to solve the above technical problems, the present invention provides a method for preparing a low-stress cutting tool coating, which mainly comprises the following steps:
[0010] (1) Pre-select the substrate and pre-treat it;
[0011] (2) placing the pretreated substrate in a vacuum chamber, introducing high-purity argon gas into the vacuum chamber, first cleaning the pretreated substrate by high-power pulsed magnetron sputtering, and then cleaning the target material after the high-power pulsed magnetron sputtering;
[0012] (3) In a vacuum chamber, high-power pulsed magnetron sputtering is performed on the surface of the cleaned substrate using a Cr target to deposit a Cr transition layer;
[0013] (4) introducing high-purity nitrogen into the vacuum chamber, and then using a Cr target to perform high-power pulsed magnetron sputtering on the surface where the Cr transition layer has been deposited, so as to deposit a layer of CrN coating;
[0014] (5) The substrate obtained after the deposition of the Cr transition layer and the CrN coating is cooled in a vacuum chamber and then taken out, and finally a low-stress Cr-CrN composite coating is prepared on the surface of the substrate.
[0015] The method for preparing the low-stress cutting tool coating, wherein: the process of pre-treating the substrate in step (1) is: first mechanically grinding the substrate, then polishing the ground substrate, then ultrasonically cleaning the polished substrate, and then drying the substrate after ultrasonic cleaning.
[0016] The method for preparing the low-stress cutting tool coating comprises the following steps: the mechanical grinding is performed by using 150# to 2300# water-treated sandpaper; and the polishing is performed by using 0.2 μm to 0.4 μm diamond polishing paste.
[0017] The method for preparing the low-stress cutting tool coating, wherein the process of ultrasonic cleaning the substrate is: firstly, the substrate is ultrasonically cleaned in acetone for 10 minutes to 20 minutes to remove dirt, then ultrasonically cleaned in deionized water for 3 minutes to 10 minutes to rinse, and finally ultrasonically cleaned in ethanol for 5 minutes to 15 minutes to dehydrate.
[0018] The method for preparing the low stress cutting tool coating, wherein the specific process of step (2) is as follows: first, the vacuum chamber is evacuated to a vacuum degree of 1×10 -3 Pa~5×10 -3 Pa, 150-200sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 40%-60%, so that the working vacuum is 1.0-1.5Pa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -800V--600V is applied to the substrate, and a Cr target is used for sputtering for 10min-20min to clean its surface, and the substrate surface is facing the Cr target during cleaning; then the bias power supply is turned off, and the DC Cr target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-3A, the argon flow rate is adjusted to 120-200sccm, the main valve angle is adjusted to 70%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
[0019] The method for preparing the low stress cutting tool coating, wherein the specific process of step (3) is as follows: in a vacuum chamber, the flow rate of argon gas introduced into the vacuum chamber is maintained at 120-150 sccm, the main valve angle of the vacuum chamber is set at 70%-90%, the working vacuum pressure is set at 0.4-0.6 Pa, the Cr target is connected to a high power pulse power supply, and the surface of the substrate is rotated to the opposite side of the Cr target by a rotating device. At this time, the distance between the Cr target and the substrate is set at 70mm-100mm, the power supply parameters of the Cr target are set to voltage 700-800V, pulse width 80-100μs, frequency 80-100Hz, the bias voltage of the substrate is set to -100--150V, and the surface of the substrate is sputtered for 10-20min to deposit a Cr transition layer.
[0020] The method for preparing the low-stress cutting tool coating, wherein the specific process of step (4) is: firstly introducing high-purity nitrogen into the vacuum chamber, and the flow ratio of the high-purity nitrogen to the high-purity argon is in the range of 1:12 to 1:6; then setting the power supply voltage of the Cr target at 600 to 800 V, the pulse width at 60 to 100 μs, and the frequency at 100 to 260 Hz, so that the average power of the Cr target power supply is 0.7 to 1 kW; setting the substrate bias voltage at -80 V to -120 V; setting the vacuum working pressure of the vacuum chamber at 0.4 to 0.6 Pa; setting the distance between the Cr target and the substrate at 70 to 90 mm; and then using the Cr target to sputter on the substrate surface after the Cr transition layer is deposited for 40 to 60 minutes to deposit a CrN coating.
[0021] The method for preparing the low stress cutting tool coating, wherein: in the step (5), the substrate obtained after depositing the Cr transition layer and the CrN coating is cooled in a vacuum chamber for 30 to 60 minutes and then taken out, and finally a low stress Cr-CrN composite coating is prepared on the surface of the substrate.
[0022] The method for preparing the low-stress cutting tool coating comprises the following steps: the size of the Cr target used in the high-power pulse magnetron sputtering is ф72.6×6 mm, and the purity is 99.999%.
[0023] The method for preparing the low-stress cutting tool coating, wherein: the high-purity argon gas is argon gas with a purity of 99.99%; the high-purity nitrogen gas is nitrogen gas with a purity of 99.99%.
[0024] By adopting the above technical solution, the present invention has the following beneficial effects:
[0025] The preparation method of the low-stress cutting tool coating of the present invention is rationally conceived. The low-stress Cr-CrN composite coating can be prepared on the surface of the substrate (such as a cemented carbide substrate, a high-speed steel substrate or a ceramic substrate) of the cutting tool by using high-power pulsed magnetron sputtering technology. Compared with the traditional DC magnetron sputtering, the metal ionization rate of the high-power pulsed magnetron sputtering method used in the present invention is as high as 70%, which is more conducive to improving the flux ratio of metal ions to inert gas ions. Combined with a plasma full spectrum analyzer and an ion flow acquisition device, the coating can effectively monitor and control the ion flux in the plasma during the deposition process, and the residual stress of the coating is significantly reduced, and the hardness, elastic modulus and bonding strength of the coating are effectively improved.
[0026] The present invention is combined with the engineering application background. By depositing a Cr-CrN composite coating on a substrate of cemented carbide, high-speed steel or ceramic, the ratio of metal ions to inert gas ions in the plasma is regulated, and metal ion irradiation is used instead of inert gas ion irradiation, thereby greatly reducing the damage caused by inert gas ion bombardment to the growth of the coating. While effectively reducing the residual stress of the coating, the overall performance of the coating is improved. Moreover, the method has no restrictions on the types of metal ions and has a certain universality.
[0027] Before implementation, the present invention utilizes a high-power pulsed magnetron sputtering method and a plasma full spectrum analyzer, increases the ratio of metal ions to inert gas ions, and utilizes metal ion irradiation to replace inert gas ion irradiation, thereby reducing the residual stress of the coating and improving the mechanical properties of the coating, thereby solving the problem that both the residual stress and the overall performance of the current cutting tool coating are difficult to meet industrial requirements at the same time.
[0028] From the perspective of reducing the growth stress of the coating, the present invention increases the ratio of metal ions to inert gas ions in the plasma, and replaces inert gas ion irradiation with metal ion irradiation, thereby ensuring the advantages of ion irradiation while reducing the harm caused by inert gas ion irradiation, and solving the problem of bonding failure caused by high residual stress on the surface coating of the current cutting tool. Among them, the overall performance of the coating of the cutting tool is greatly related to the thickness and stress state of the coating, but as the thickness increases, the stress of the coating will gradually increase. When the stress reaches a certain limit, the coating will break or fall off, especially in the working state; therefore, the existing preparation method cannot achieve a further increase in the thickness of the coating, and the preparation method of the present invention can obtain a cutting coating with lower stress, because the thickness of the coating can be effectively increased, thereby obtaining beneficial effects such as a longer service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 It is a schematic flow chart of the method for preparing the low stress cutting tool coating of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention is further explained below in conjunction with specific implementation modes.
[0033] like Figure 1 As shown, the present embodiment provides a method for preparing a low stress cutting tool coating, which specifically comprises the following steps:
[0034] S010, pre-select the substrate and pre-treat it. The process of pre-treating the substrate is as follows: first, use 150#~2300# water sandpaper to mechanically grind the substrate; then use 0.2μm~0.4μm diamond polishing paste to polish; then, ultrasonically clean the polished substrate in acetone for 10min~20min to remove dirt, then ultrasonically clean it in deionized water for 3min~10min, and finally ultrasonically clean it in ethanol for 5min~15min to dehydrate; then, dry the substrate after ultrasonic cleaning.
[0035] S020, place the pretreated substrate in a vacuum chamber and evacuate the chamber to a vacuum degree of 1×10 -3 Pa~5×10 -3 Pa, 150-200sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 40%-60%, so that the working vacuum is 1.0-1.5Pa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -800V--600V is applied to the substrate, and a Cr target is used for sputtering for 10min-20min to clean its surface, and the substrate surface is facing the Cr target during cleaning; then the bias power supply is turned off, and the DC Cr target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-3A, the argon flow rate is adjusted to 120-200sccm, the main valve angle is adjusted to 70%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
[0036] S030. In the vacuum chamber, the flow rate of argon gas entering the vacuum chamber is maintained at 120-150 sccm, the main valve angle is 70%-90%, and the working vacuum pressure is 0.4-0.6 Pa; the Cr target is connected to a high-power pulse power supply, and the surface of the substrate is turned to the opposite side of the target material through a rotating device. At this time, the distance between the Cr target and the substrate is 70mm-100mm. When setting high-power pulse magnetron sputtering, the power supply parameters of the Cr target are voltage 700-800V, pulse width 80-100μs, frequency 80-100Hz, and the bias voltage of the substrate is -100--150V. The surface of the substrate is sputtered for 10-20min to deposit a Cr transition layer.
[0037] S040. First, high-purity nitrogen is introduced into the vacuum chamber, and the flow ratio of high-purity nitrogen to high-purity argon is in the range of 1:12 to 1:6; then, the power supply voltage of the Cr target is set at 600 to 800 V, the pulse width is set at 60 to 100 μs, and the frequency is set at 100 to 260 Hz, so that the average power supply power of the Cr target is 0.7 to 1 kW; the substrate bias voltage is set at -80 V to -120 V; the vacuum working pressure of the vacuum chamber is set at 0.4 to 0.6 Pa; the distance between the Cr target and the substrate is set at 70 to 90 mm; then, the Cr target is used to sputter on the surface of the substrate after the Cr transition layer is deposited for 40 to 60 minutes to deposit a CrN coating.
[0038] S050, cooling the substrate obtained after depositing the Cr transition layer and the CrN coating in a vacuum chamber for 30 to 60 minutes and then taking it out, and finally preparing a low-stress Cr-CrN composite coating on the surface of the substrate.
[0039] The size of the Cr target used in the high-power pulsed magnetron sputtering is ф72.6×6 mm, and the purity is 99.999%; the high-purity argon gas is argon gas with a purity of 99.99%, and the high-purity nitrogen gas is nitrogen gas with a purity of 99.99%.
[0040] The present invention utilizes high-power pulsed magnetron sputtering technology and a plasma full spectrum analyzer, and realizes effective regulation of the ratio of metal ions to inert gas ions under the premise of ensuring a high metal ionization rate through regulation of discharge parameters and plasma monitoring; a group of experimental parameters with a large ratio of metal Cr ions to inert gas ions are adopted to prepare a Cr transition layer and a CrN coating respectively, so as to obtain a Cr-CrN composite coating with low stress and excellent overall performance.
[0041] Before implementation, the present invention first uses a plasma full spectrum analyzer to monitor the plasma. The plasma full spectrum analyzer is an analytical device that can detect the plasma distribution spectrum in real time. Before formal preparation, the device will be used to detect and calibrate the plasma under various parameters, select suitable plasma characteristics, determine preparation parameters, and prepare for subsequent experimental settings. The present invention selects 284.3nm wavelength as chromium ions (Cr + ) characteristic spectrum, 520.6nm is the characteristic spectrum of chromium atoms (Cr), 480.0nm is the characteristic spectrum of argon ions (Ar + ) characteristic spectrum. The intensity of each ion is the peak value of the corresponding wavelength in the plasma emission spectrum, using Cr + Strength and Ar + The ratio of the intensity indicates the metal ion (Cr + ) and inert gas ions (Ar +) flux. By adjusting the voltage, frequency, pulse width and power of the Cr target power supply during high-power pulsed magnetron sputtering, the Cr + With high ionization rate, N Cr+ / N Ar+ A larger set of process parameters.
[0042] The present invention can select cemented carbide, high-speed steel (HSS) or ceramic as the substrate, and use a high-power pulsed magnetron sputtering method to first sputter a Cr transition layer on the substrate surface to improve the bonding force between the film and the substrate. The Cr transition layer has better ductility than the Cr-based ceramic coating. Cr plasma deposition can promote the bonding between the Cr-based coating and the substrate material. After the Cr transition layer is deposited, high-purity nitrogen is introduced into the vacuum chamber to prepare the CrN coating. Based on this, the N in the plasma is firstly realized. Cr+ / N Ar+ The regulation from 4.1 to 6.2 reduced the residual stress of the CrN coating from 7.1 GPa to 1.7 GPa, and the hardness, elastic modulus and bonding strength of the coating were effectively improved.
[0043] Example 1
[0044] In Example 1 of the present invention, a chromium target with a size of ф72.6×6 mm and a purity of 99.999% is used, and the gases used are 99.99% high-purity argon and 99.99% high-purity nitrogen. A cemented carbide with a size of 25×25×5 mm is used as a substrate for surface analysis of the coating and mechanical property testing. The preparation process of the low-stress coating is as follows:
[0045] S110, substrate pretreatment
[0046] The cemented carbide substrate was mechanically polished with 150#-2300# water sandpaper, polished with 0.2μm diamond polishing paste, ultrasonically cleaned in acetone for 15 minutes to remove dirt, ultrasonically cleaned in deionized water for 5 minutes to rinse, ultrasonically cleaned in ethanol for 10 minutes to dehydrate, and dried with a hair dryer;
[0047] S120, cleaning target and substrate
[0048] The pretreated substrate was placed in a vacuum chamber and then the vacuum chamber was evacuated to a vacuum degree of 3×10 -3Pa, introduce 180sccm high-purity argon, adjust the main valve angle of the vacuum chamber to 40%, make its working vacuum 1.0Pa, turn on the DC bias power supply loaded on the substrate, apply a bias of -800V on the substrate, and use Cr target for sputtering for 10min, the purpose is to clean the surface of the substrate and increase its surface activity. At this time, the sample surface is facing away from the Cr target; then turn off the bias power supply, turn on the DC Cr target power supply, the DC power supply adopts the constant current mode, set the DC power supply current parameter to 2A, adjust the argon flow rate to 120sccm, adjust the main valve angle to 90%, make the working vacuum 0.4Pa, and the sputtering time is 15min, the purpose is to clean the target material and remove impurities and oxide film on the target material surface.
[0049] S130, Cr transition layer deposition
[0050] In the vacuum chamber, the argon flow rate into the vacuum chamber is maintained at 120sccm, the main valve angle is 90%, the working vacuum pressure is 0.4Pa, the Cr target is connected to a high-power pulse magnetron sputtering power supply, and the surface of the substrate is turned to the opposite side of the Cr target by a rotating device. At this time, the distance between the Cr target and the substrate is 90mm. When setting the power supply parameters of the Cr target for high-power pulse magnetron sputtering, the voltage is 800V, the pulse width is 100μs, and the frequency is 100Hz. The bias voltage of the substrate is 150V, and the surface of the substrate is sputtered for 20min to deposit a Cr transition layer, in order to improve the bonding strength between the film and the substrate.
[0051] S140, CrN coating deposition
[0052] First, high-purity nitrogen is introduced into the vacuum chamber, and a CrN coating is prepared on the substrate by high-power pulsed magnetron sputtering. Specifically, the power supply voltage of the Cr target is 600V, the pulse width is 60μs, the frequency is 100Hz, the substrate bias is -80V, the vacuum working pressure of the vacuum chamber is 0.4Pa, the average power is 0.7kW, the flow ratio of nitrogen to argon is 10:120sccm, the distance between the Cr target and the substrate is 90mm, and the Cr target is used to sputter on the substrate surface after the Cr transition layer is deposited for 60min to deposit the CrN coating.
[0053] S150, cooling and removal
[0054] The substrate obtained after the deposition of the Cr transition layer and the CrN coating is taken out after being vacuum cooled in a vacuum chamber for 30 minutes, and the furnace is filled with gas to open and take out the cemented carbide substrate with the low-stress Cr-CrN composite coating.
[0055] In Example 1 of the present invention, residual stress, hardness, elastic modulus and bonding strength tests were carried out. The results showed that by increasing the ratio of metal ion irradiation to inert gas ion irradiation and replacing inert gas ion irradiation with metal ion irradiation, the residual stress of the CrN coating can be reduced from 7.1 GPa to 1.7 GPa, and the overall toughness (H / E increased from 0.07 to 0.1) and film-base bonding performance are improved.
[0056] From the perspective of reducing coating growth stress, the present invention increases the ratio of metal ions to inert gas ions in plasma and replaces inert gas ion irradiation with metal ion irradiation. While ensuring the advantages of ion irradiation, the harm caused by inert gas ion irradiation is weakened, thus solving the problem of bonding failure of current cutting tool surface coating due to high residual stress.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a low stress cutting tool coating, characterized in that: The main steps include: (1) Pre-select the substrate and pre-treat it; (2) placing the pretreated substrate in a vacuum chamber, introducing high-purity argon gas into the vacuum chamber, first cleaning the pretreated substrate by high-power pulsed magnetron sputtering, and then cleaning the target material after the high-power pulsed magnetron sputtering; (3) In a vacuum chamber, high-power pulsed magnetron sputtering is performed on the surface of the cleaned substrate using a Cr target to deposit a Cr transition layer; (4) introducing high-purity nitrogen into the vacuum chamber, and then using a Cr target to perform high-power pulsed magnetron sputtering on the surface where the Cr transition layer has been deposited, so as to deposit a layer of CrN coating; (5) The substrate obtained after the deposition of the Cr transition layer and the CrN coating is cooled in a vacuum chamber and then taken out, and finally a low-stress Cr-CrN composite coating is prepared on the surface of the substrate.
2. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The process of pre-treating the substrate in step (1) is: first mechanically grinding the substrate, then polishing the ground substrate, then ultrasonically cleaning the polished substrate, and then drying the substrate after ultrasonic cleaning.
3. The method for preparing a low stress cutting tool coating according to claim 2, characterized in that: The mechanical grinding is performed by using 150#-2300# water sandpaper; the polishing is performed by using 0.2μm-0.4μm diamond polishing paste.
4. The method for preparing a low stress cutting tool coating according to claim 2, characterized in that: The process of ultrasonic cleaning the substrate is as follows: firstly, the substrate is ultrasonically cleaned in acetone for 10 to 20 minutes to remove dirt, then ultrasonically cleaned in deionized water for 3 to 10 minutes to rinse, and finally ultrasonically cleaned in ethanol for 5 to 15 minutes to dehydrate.
5. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The specific process of step (2) is as follows: first, the vacuum chamber is evacuated to a vacuum degree of 1×10 -3 Pa~5×10 -3 Pa, 150-200sccm high-purity argon is introduced, the main valve angle of the vacuum chamber is adjusted to 40%-60%, so that the working vacuum is 1.0-1.5Pa, the DC bias power supply loaded on the substrate is turned on, a bias voltage of -800V--600V is applied to the substrate, and a Cr target is used for sputtering for 10min-20min to clean its surface, and the substrate surface is facing the Cr target during cleaning; then the bias power supply is turned off, and the DC Cr target power supply is turned on. The DC power supply adopts a constant current mode, and the current parameter of the DC power supply is set to 1A-3A, the argon flow rate is adjusted to 120-200sccm, the main valve angle is adjusted to 70%-90%, so that the working vacuum is 0.4-0.6Pa, and sputtering is performed for 10-15min to achieve target cleaning.
6. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The specific process of step (3) is as follows: in a vacuum chamber, the flow rate of argon gas introduced into the vacuum chamber is maintained at 120-150 sccm, the main valve angle of the vacuum chamber is set at 70%-90%, the working vacuum pressure is set at 0.4-0.6 Pa, the Cr target is connected to a high-power pulse power supply, and the surface of the substrate is rotated to the opposite side of the Cr target by a rotating device. At this time, the distance between the Cr target and the substrate is set at 70mm-100mm, the power supply parameters of the Cr target are set to voltage 700-800V, pulse width 80-100μs, frequency 80-100Hz, the bias voltage of the substrate is set to -100--150V, and the surface of the substrate is sputtered for 10-20min to deposit a Cr transition layer.
7. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The specific process of step (4) is as follows: firstly, high-purity nitrogen is introduced into the vacuum chamber, and the flow ratio of the high-purity nitrogen to the high-purity argon is in the range of 1:12 to 1:6; then, the power supply voltage of the Cr target is set at 600 to 800 V, the pulse width is set at 60 to 100 μs, and the frequency is set at 100 to 260 Hz, so that the average power of the Cr target power supply is 0.7 to 1 kW; the substrate bias voltage is set at -80 V to -120 V; the vacuum working pressure of the vacuum chamber is set at 0.4 to 0.6 Pa; the distance between the Cr target and the substrate is set at 70 to 90 mm; and then, the Cr target is used to sputter on the substrate surface after the Cr transition layer is deposited for 40 to 60 minutes to deposit a CrN coating.
8. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that In the step (5), the substrate obtained after the deposition of the Cr transition layer and the CrN coating is cooled in a vacuum chamber for 30 to 60 minutes and then taken out, and finally a low-stress Cr-CrN composite coating is prepared on the surface of the substrate.
9. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The size of the Cr target used in the high-power pulse magnetron sputtering is ф72.6×6 mm, and the purity is 99.999%.
10. The method for preparing a low stress cutting tool coating according to claim 1, characterized in that: The high-purity argon gas is argon gas with a purity of 99.99%; the high-purity nitrogen gas is nitrogen gas with a purity of 99.99%.