Bismuth ferrite film material as well as preparation method and application thereof

By directly depositing bismuth ferrite films on transparent glass substrates, the performance degradation and material toxicity problems caused by high-temperature preparation were solved, and transparent bismuth ferrite films prepared at low temperatures were realized. These films are suitable for semiconductor integration and display devices and exhibit excellent ferroelectric and piezoelectric properties.

CN119020743APending Publication Date: 2024-11-26QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411137875.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The high-temperature preparation and annealing of existing perovskite-type transparent piezoelectric film materials damage the properties of conductive glass, and lead-based materials are toxic, limiting their application and compatibility in semiconductor integration technology.

Method used

Bismuth ferrite films are directly deposited on transparent glass substrates using radio frequency magnetron sputtering technology, avoiding high-temperature annealing. Bismuth ferrite films are also deposited on indium tin oxide layers. The preparation process is simple, the materials do not require an additional buffer layer, and the raw materials are inexpensive and readily available.

Benefits of technology

A transparent bismuth ferrite film material prepared at low temperature has been achieved, which maintains high transparency and excellent ferroelectric and piezoelectric properties. It is compatible with semiconductor integration processes, environmentally friendly, and suitable for flat panel displays and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020743A_ABST
    Figure CN119020743A_ABST
Patent Text Reader

Abstract

The invention belongs to the technology of electronic material development and thin film material preparation, and particularly relates to a bismuth ferrite film material and a preparation method and application thereof.A bismuth ferrite film is deposited on a transparent glass substrate attached with an indium tin oxide conductive thin film at the temperature of 350-550 DEG C through the radio frequency magnetron sputtering technology, and after the transparent glass substrate is cooled to the room temperature, the bismuth ferrite film material is obtained; and sputtering and depositing a platinum thin layer on the bismuth ferrite film. The preparation temperature is low, high-temperature annealing treatment is not needed, an additional buffer layer does not need to be introduced, the preparation process is simple, all needed raw materials are cheap and easy to obtain, and the transparent piezoelectric film particularly has high transparency and excellent ferroelectric and piezoelectric properties and shows huge application potential in the field of transparent piezoelectric film devices, especially flat panel displays with tactile feedback.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to electronic material development and thin film material preparation technology, and specifically relates to a bismuth ferrite film material and a preparation method and application thereof. Background Art

[0002] Semiconductor transparent materials have good electrical properties, light transmittance and low production cost, and are now widely used in the photovoltaic industry, smart color-changing glass and touch screens. With the in-depth study of magnetron sputtering technology and thin-film piezoelectric micro-electromechanical systems, it is found that perovskite-type ferroelectric and piezoelectric film materials deposited on transparent glass will also produce piezoelectric response, and have comparable performance to piezoelectric film materials deposited on semiconductor silicon substrates, such as sensitive response speed, wide operating voltage range (several to more than ten volts), and large piezoelectric displacement response amplitude (submicron or micron level); in particular, the prepared piezoelectric film material has high transparency, which greatly broadens the application field of piezoelectric devices.

[0003] One of the main problems currently limiting the industrial application of perovskite transparent piezoelectric film materials is the high process temperature and subsequent annealing heat treatment, which will seriously damage the electrical conductivity of the conductive glass and cause it to undergo significant destructive deformation, ultimately leading to the failure of the piezoelectric properties of the material and its devices. At the same time, this high-temperature preparation has hindered the application of piezoelectric materials in mainstream silicon-based semiconductor integration technology, making it incompatible with semiconductor integration processes. Although lead zirconate titanate (PZT), the mainstream piezoelectric material today, has a high piezoelectric coefficient, the toxicity generated by these lead-based materials and their devices during use and recycling undoubtedly poses a severe challenge to human life and health and environmental protection.

[0004] Lead-free bismuth ferrite (BiFeO3) is an attractive environmentally friendly piezoelectric material. Compared with lead zirconate titanate-based thin film materials, bismuth ferrite thin films have simpler chemical compositions, higher Curie temperatures T c , especially its larger intrinsic polarization (~100μC / cm 2 ) and a smaller dielectric constant ε r These characteristics make bismuth ferrite film have better piezoelectric response stability and energy conversion efficiency than lead zirconate titanate-based film materials. However, the deposition of bismuth ferrite film still cannot avoid high-temperature preparation and annealing. Prior art, such as the Chinese invention patents with application publication numbers CN 111525024 A and CN 105336845 A, usually introduces conductive oxides such as lanthanum nickelate and strontium ruthenate as a buffer layer between the piezoelectric film and the substrate in order to reduce the heat treatment temperature of the piezoelectric film material. However, the introduction of the buffer layer will cause the transparency of the conductive glass to drop sharply or even completely lose. Summary of the invention

[0005] The present invention aims to solve the above-mentioned problems of material performance deterioration and limited use scenarios caused by high-temperature preparation and annealing treatment, introduction of buffer layers, and toxic elements contained in the material itself, and provides a simple preparation method for an environmentally friendly transparent bismuth ferrite film material with mild preparation conditions and excellent ferroelectric / piezoelectric properties. The piezoelectric film material is directly deposited on a transparent glass substrate with a conductive indium tin oxide layer. The preparation temperature is low and no high-temperature annealing treatment is required. No additional buffer layer needs to be introduced. The preparation process is simple, and all the raw materials required are cheap and easy to obtain. In particular, it has high transparency and excellent ferroelectric and piezoelectric properties, and shows great application potential in the field of transparent piezoelectric film devices, especially flat-panel displays with tactile feedback.

[0006] The present invention is implemented by the following technical solutions:

[0007] In the first aspect, the implementation of the present invention provides a bismuth ferrite film material, including a substrate, a bottom electrode, a piezoelectric film and a top electrode, wherein the substrate is transparent glass, the bottom electrode is a transparent indium tin oxide layer, the piezoelectric film is a bismuth ferrite film, and the top electrode is a thin layer of metal platinum; wherein the bismuth ferrite film is directly deposited on the bottom electrode.

[0008] In some embodiments, the substrate has a thickness of 0.6-1.2 mm and a width of 1-3 mm; the indium tin oxide layer has a thickness of 150-200 nm, the bismuth ferrite film layer has a thickness of 0.8-1.5 μm, and the platinum thin layer has a thickness of 10-50 nm.

[0009] In some embodiments, the polarization strength of the bismuth ferrite film is up to 78 μC / cm 2 , transverse piezoelectric coefficient is 1.7C / m 2 ; The transmittance in the visible light wavelength range is above 58%.

[0010] In some embodiments, the bismuth ferrite film material includes a substrate, a bottom electrode, a piezoelectric film and a top electrode, wherein the substrate is transparent glass, the bottom electrode is a transparent indium tin oxide layer, the piezoelectric film is a bismuth ferrite film, and the top electrode is a thin layer of metal platinum.

[0011] In a second aspect, the present invention provides a method for preparing the bismuth ferrite film material according to the first aspect, comprising the following steps:

[0012] (1) Using a transparent glass substrate with an indium tin oxide conductive layer as a substrate, heating the substrate to 350-550° C. in an inert atmosphere;

[0013] (2) using bismuth ferrite ceramic as a sputtering target, and depositing a bismuth ferrite film on the substrate in step (1) by using radio frequency magnetron sputtering technology; and cooling the obtained bismuth ferrite film to room temperature;

[0014] (3) Using metal platinum as a target, a thin layer of platinum top electrode is sputtered and deposited on the bismuth ferrite film after the cooling treatment in step (2) by using magnetron sputtering technology.

[0015] In some embodiments, in step (1), the substrate is placed in a magnetron sputtering chamber and the chamber is evacuated to a pressure lower than 2×10 -4 Pa; introduce argon gas, the argon gas flow rate is 40-80 sccm, the heating pressure is 1-3 Pa; the heating rate is 5-10°C / min.

[0016] In some embodiments, in step (2), the bismuth ferrite ceramic Bi n In FeO3, the molar ratio of Bi element to Fe element is 1.05-1.1; the conditions of the RF magnetron sputtering are: the sputtering atmosphere is a mixed gas of argon and oxygen, and the volume ratio of argon and oxygen is (30-110): (5-30); the argon flow rate is 40-80sccm, the oxygen flow rate is 5-25sccm, the gas pressure is 0.1-1.5Pa, the sputtering power is 60-150W, the sputtering time is 2-6h, and the deposition temperature is 350-550°C.

[0017] In some embodiments, in step (2), the cooling treatment conditions are: the atmosphere is oxygen, the flow rate is 15 to 60 sccm, the gas pressure is 1.0 to 10 Pa, and the cooling rate is 2 to 8°C / min.

[0018] In some embodiments, in step (3), the conditions of magnetron sputtering are: the sputtering atmosphere is argon, the argon flow rate is 20-60 sccm, the sputtering pressure is 0.1-1.0 Pa, the sputtering power is 30-100 W, the deposition time is 30-120 s, and the temperature is room temperature.

[0019] In some embodiments, the substrate has a thickness of 0.6-1.2 mm and a width of 1-3 mm; the indium tin oxide layer has a thickness of 150-200 nm, the bismuth ferrite film layer has a thickness of 0.8-1.5 μm, and the platinum thin layer has a thickness of 10-50 nm.

[0020] In a third aspect, the implementation of the present invention provides the use of the bismuth ferrite film material described in the first aspect in a transparent piezoelectric film device.

[0021] In some embodiments, the application is in a display, a photovoltaic product, or an intelligent photochromic glass; preferably, the display is a flat-panel display with tactile feedback.

[0022] The beneficial effects of the present invention are:

[0023] (1) The preparation temperature of the bismuth ferrite film material provided by the present invention is not higher than 550°C, and no high-temperature annealing treatment is required, which effectively avoids the problem of deterioration of the conductivity and deformation of the conductive glass matrix caused by high-temperature heat treatment, thereby causing the piezoelectric properties of the material and its device to fail. At the same time, medium and low temperature preparation is conducive to the integrated compatibility and industrial application of semiconductor devices.

[0024] (2) The present invention deposits the bismuth ferrite film directly on a transparent glass substrate with an indium tin oxide conductive layer, without the need to introduce an oxide buffer layer such as lanthanum nickelate or strontium ruthenate. The prepared piezoelectric film material has high transparency and the preparation process is simple and easy.

[0025] (3) The bismuth ferrite film material provided by the present invention does not contain any toxic elements and is very friendly to human health and the environment during the preparation, processing, use and recycling of the material and its devices.

[0026] (4) The raw materials required for the bismuth ferrite film material provided by the present invention are all commercially available and inexpensive, which is more economically advantageous than the bismuth ferrite film materials that are mostly integrated on semiconductor silicon or expensive single crystal oxide substrates.

[0027] (5) The radio frequency magnetron sputtering technology adopted in the present invention is suitable for preparing large-size, high-quality piezoelectric film materials, has high compatibility with semiconductor integration processes, and is suitable for industrial mass production.

[0028] (6) The bismuth ferrite film material provided by the present invention will not be affected by the changes in parameters such as cantilever beam width, top electrode platinum thin layer thickness, bismuth ferrite target material stoichiometry, cooling atmosphere, and cold cooling rate (without exceeding the set parameter range) and other parameters, such as polarization intensity, transverse piezoelectric coefficient, and transmittance.

[0029] The method of the present invention is further described in detail below through the accompanying drawings and exemplary embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is an XRD scan of the bismuth ferrite film prepared in Example 1 of the present invention;

[0031] Figure 2 The surface and cross-sectional scanning microscope images of the bismuth ferrite film prepared in Example 1 of the present invention;

[0032] Figure 3 The hysteresis loop and polarization reversal current diagram of the bismuth ferrite film material prepared in Example 1 of the present invention;

[0033] Figure 4 This is a graph of the tip displacement of the cantilever beam and the transverse piezoelectric coefficient of the bismuth ferrite film material prepared in Example 1 of the present invention. The lower right illustration is a schematic diagram of the transverse piezoelectric testing device, and the upper left illustration is a transmittance curve and actual picture of the prepared bismuth ferrite film material. DETAILED DESCRIPTION

[0034] The following is further described with reference to the embodiments.

[0035] The raw materials required for the bismuth ferrite film material provided by the invention are all commercially available products.

[0036] Example 1

[0037] A method for preparing a bismuth ferrite film material comprises the following steps:

[0038] (1) Matrix treatment

[0039] Substrate cleaning and installation: A commercially available transparent glass with an indium tin oxide conductive layer was used as the substrate, with a size of 20 mm (length) × 3 mm (width) × 0.7 mm (thickness). Its surface was cleaned with high-purity nitrogen gas and then placed in the sample holder of the magnetron sputtering chamber;

[0040] Vacuuming: Start the mechanical pump and molecular pump of the magnetron sputtering instrument in sequence to pump the chamber pressure to the back vacuum (less than 2×10 -4 Pa) to ensure sufficient cleanliness in the chamber;

[0041] Gas: After the backside is evacuated to vacuum, argon gas is introduced into the chamber. The argon gas flow rate is controlled to 40 sccm and the chamber pressure is adjusted to 2.5 Pa.

[0042] Heating: The conductive glass substrate is heated and maintained at 550°C, and the heating rate is controlled at 5°C / min.

[0043] (2) Preparation of bismuth ferrite film

[0044] After the glass substrate is heated to the set temperature, a mixed gas of argon and oxygen is introduced into the chamber, the argon flow rate is adjusted to 60 sccm, the oxygen flow rate is adjusted to 15 sccm, and the chamber pressure is reduced to 0.3 Pa. A bismuth ferrite oxide ceramic (chemical composition is Bi) with an excess of 5% mol of bismuth element is prepared. 1.05 FeO3) was used as a sputtering target, and a bismuth ferrite film was directly deposited on a transparent glass substrate with an indium tin oxide conductive layer. The sputtering power was controlled to 100 W and the sputtering time was 6 h. After the sputtering deposition was completed, the chamber atmosphere was adjusted to oxygen with a flow rate of 40 sccm and a chamber pressure of 2.5 Pa, and then cooled to room temperature at a rate of 5 °C / min.

[0045] (3) Top electrode preparation

[0046] A thin layer of metal platinum with a size of 15 mm (length) × 3 mm (width) is sputtered on the surface of the bismuth ferrite film prepared in step (2) as a top electrode. The sputtering atmosphere is argon, the flow rate is 40 sccm, the sputtering pressure is 0.3 Pa, the sputtering power is 55 W, the deposition time is 1 min, and the sample is taken out after the sputtering is completed.

[0047] Example 2

[0048] The difference from Example 1 is that the thickness of the glass substrate used in step (1) is 1.1 mm, and the other steps and process parameters are the same as those in Example 1.

[0049] Example 3

[0050] The difference from Example 1 is that in step (1), the glass substrate is heated and maintained at 450° C., and the other steps and process parameters are the same as those in Example 1.

[0051] Example 4

[0052] The difference from Example 1 is that in step (1), the glass substrate is heated and maintained at 500° C., and the other steps and process parameters are the same as those in Example 1.

[0053] Example 5

[0054] The difference from Example 1 is that the sputtering deposition time of the bismuth ferrite film in step (2) is 2 hours, and the other steps and process parameters are the same as those in Example 1.

[0055] Example 6

[0056] The difference from Example 1 is that the sputtering deposition time of the bismuth ferrite film in step (2) is 4 hours, and the other steps and process parameters are the same as those in Example 1.

[0057] Reference ratio

[0058] The transmittance of commercially available conductive glass without depositing bismuth ferrite piezoelectric film material is 88%.

[0059] Performance Testing

[0060] The bismuth ferrite film materials prepared in Examples 1 to 6 and the commercially available conductive glass of the reference example were subjected to performance tests. The test results are shown in Table 1.

[0061] Transverse piezoelectric test: The bismuth ferrite film cantilever beam samples prepared in Examples 1 to 6 were placed on a fixture for piezoelectric performance testing. The test conditions were: AC voltage of 4 to 10 V (peak-to-peak) and frequency of 500 Hz.

[0062] Polarization strength test: The bismuth ferrite film samples prepared in Examples 1 to 6 were placed on a ferroelectric tester probe station for polarization strength test.

[0063] The test conditions are: the maximum voltage is the voltage that the bismuth ferrite film sample can withstand, the frequency is 2kHz, and the area of ​​the gold dot top electrode used is 0.000314cm 2 .

[0064] Infrared transmittance test: The bismuth ferrite film samples prepared in Examples 1 to 6 and the commercially available conductive glass of the reference example were placed in an ultraviolet-visible-near-infrared spectrophotometer for testing.

[0065] The test conditions are as follows: the light source is near ultraviolet, visible and near infrared light source, and the wavelength is 300-1000nm.

[0066] Table 1 Properties of bismuth ferrite film

[0067]

[0068]

[0069] After testing, the transparent bismuth ferrite film material prepared in Example 1 has excellent piezoelectric and ferroelectric properties and a stable structure. Figure 1 This is the XRD pattern of the transparent bismuth ferrite film material prepared in Example 1. The bismuth ferrite film material is in a randomly oriented polycrystalline state without any impurity phase. The sharp diffraction peaks and high peak intensity indicate good crystallinity. Figure 2 The surface and cross-sectional scanning electron microscope images of the bismuth ferrite film prepared in Example 1 show that uniform and dense grains can be observed on the surface. From the cross-sectional view, it can be seen that the thickness of the indium tin oxide conductive layer is 170 nm, and the thickness of the bismuth ferrite film layer is 1.2 μm. Figure 3 It shows that the bismuth ferrite film prepared in Example 1 has strong ferroelectricity and large polarization strength (~78μC / cm 2 ); Figure 4 The tip displacement of the cantilever beam of the bismuth ferrite film material prepared in Example 1 and the calculated transverse piezoelectric coefficient and transmittance curve are shown in Figure 1. The prepared transparent bismuth ferrite film exhibits a large tip displacement. The calculated transverse piezoelectric coefficient e is 0.04 when the bias voltage is 10 V. 31,f Up to 1.7C / m 2 , showing excellent lateral piezoelectric performance. The lower right illustration is a schematic diagram of the lateral piezoelectric test device; the upper left illustration is a physical picture of the prepared transparent bismuth ferrite film material and the transmittance test curve, indicating that the transmittance of the transparent bismuth ferrite film material can reach ~60% in the visible light wavelength range.

[0070] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. The above description is only a preferred embodiment of the present invention, but is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A bismuth ferrite film material, characterized in that: It includes a substrate, a bottom electrode, a piezoelectric film and a top electrode, wherein the substrate is transparent glass, the bottom electrode is a transparent indium tin oxide layer, the piezoelectric film is a bismuth ferrite film, and the top electrode is a metal platinum thin layer; wherein the bismuth ferrite film is directly deposited on the bottom electrode.

2. The bismuth ferrite film material according to claim 1, characterized in that: The thickness of the substrate is 0.6-1.2 mm; the thickness of the indium tin oxide layer is 150-200 nm; the thickness of the bismuth ferrite film layer is 0.8-1.5 μm; and the thickness of the platinum thin layer is 10-50 nm.

3. The bismuth ferrite film material according to claim 1, characterized in that The polarization strength of the bismuth ferrite film is 78 μC / cm 2 , transverse piezoelectric coefficient is 1.7C / m 2 ; The transmittance in the visible light wavelength range is over 58%.

4. A method for preparing the bismuth ferrite film material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Using a transparent glass substrate with an indium tin oxide conductive layer as a substrate, heating the substrate to 350-550° C. in an inert atmosphere; (2) using bismuth ferrite ceramic as a sputtering target, and depositing a bismuth ferrite film on the substrate in step (1) by using radio frequency magnetron sputtering technology; and cooling the obtained bismuth ferrite film to room temperature; (3) Using metal platinum as a target, a thin layer of platinum top electrode is sputtered and deposited on the bismuth ferrite film after the cooling treatment in step (2) by using magnetron sputtering technology.

5. The preparation method according to claim 4, characterized in that: In step (1), the substrate is placed in a magnetron sputtering chamber and evacuated until the chamber pressure is less than 2×10 -4 Pa; introduce argon gas, the argon gas flow rate is 40-80 sccm, the heating pressure is 1-3 Pa; the heating rate is 5-10°C / min.

6. The preparation method according to claim 4, characterized in that: In step (2), in the bismuth ferrite ceramic, the molar ratio of Bi element to Fe element is 1.05-1.1; the conditions of the radio frequency magnetron sputtering are: the sputtering atmosphere is a mixed gas of argon and oxygen, and the volume ratio of argon and oxygen is (30-110): (5-30); the argon flow rate is 40-80sccm, the oxygen flow rate is 5-25sccm, the gas pressure is 0.1-1.5Pa, the sputtering power is 60-150W, and the sputtering time is 2-6h; the deposition temperature is 350-550°C.

7. The preparation method according to claim 4, characterized in that: In step (2), the cooling treatment conditions are: the atmosphere is oxygen, the flow rate is 15 to 60 sccm, the gas pressure is 1.0 to 10 Pa, and the cooling rate is 2 to 8°C / min.

8. The preparation method according to claim 4, characterized in that: In step (3), the conditions of magnetron sputtering are: the sputtering atmosphere is argon, the argon flow rate is 20-60 sccm, the sputtering pressure is 0.1-1.0 Pa, the sputtering power is 30-100 W, the deposition time is 30-120 s, and the temperature is room temperature.

9. The preparation method according to claim 4, characterized in that: The substrate has a thickness of 0.6-1.2 mm and a width of 1-3 mm; the indium tin oxide layer has a thickness of 150-200 nm, the bismuth ferrite film layer has a thickness of 0.8-1.5 μm, and the platinum thin layer has a thickness of 10-50 nm.

10. Use of the bismuth ferrite film material according to any one of claims 1 to 3 in a transparent piezoelectric film device, characterized in that: Application in displays, photovoltaic products, and smart color-changing glass; preferably, the display is a flat-panel display with tactile feedback.