Surface treatment method

CN119020778APending Publication Date: 2024-11-26SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410577132.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In semiconductor manufacturing processes, the prior art is difficult to effectively prevent component surface defects and particle problems caused by fluorine radicals.

Method used

By using a remote plasma source in the process chamber to generate fluorine plasma, a protective layer containing magnesium fluoride is formed, with a magnesium content of 0.5 wt% to 5.5 wt% and a thickness of 100 nm to 300 nm to prevent fluorine radical penetration and reduce particles generate.

Benefits of technology

The life cycle of the component is extended, the particle and surface roughness changes in the process chamber are reduced, the process conditions are maintained, and the film deposition rate is prevented.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020778A_ABST
    Figure CN119020778A_ABST
Patent Text Reader

Abstract

A method of surface treatment includes: providing a component in a first process chamber; generating a fluorine plasma using a remote plasma source connected to the first process chamber; and forming a protective layer on a surface of the component by providing the fluorine plasma to the first process chamber, where the protective layer includes magnesium fluoride, where the magnesium content of the component is from about 0.5 wt% to about 5.5 wt%, and where the thickness of the protective layer is from about 100 nm to about 300 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for surface treatment. Background Art

[0002] As the temperature of semiconductor manufacturing processes increases, cleaning process temperatures also increase to achieve process efficiency. Fluorine radicals used in cleaning processes may cause fluorine on the surface of components to cause component defects and particle problems in semiconductor processes, and therefore techniques are needed to prevent these problems. Summary of the invention

[0003] A method for surface treatment is provided. The method may include forming a protective layer by high temperature plasma pretreatment to suppress fluorine on the surface of a component exposed to plasma among components of a process chamber.

[0004] According to one aspect of the present disclosure, a method for surface treatment includes: providing a component in a first process chamber; generating fluorine plasma using a remote plasma source connected to the first process chamber; and forming a protective layer on a surface of the component by providing the fluorine plasma to the first process chamber, wherein the protective layer includes magnesium fluoride, wherein the magnesium content of the component is about 0.5 wt % to about 5.5 wt %, and wherein the thickness of the protective layer is about 100 nm to about 300 nm.

[0005] According to one aspect of the present disclosure, a method of surface treatment includes: installing a component in a process chamber; generating fluorine plasma using a remote plasma source connected to the process chamber; and forming a protective layer on a surface of the component by providing the fluorine plasma to the process chamber, wherein the protective layer includes magnesium fluoride, wherein the magnesium content of the component is about 0.5 wt % to about 5.5 wt %, and wherein the thickness of the protective layer is about 100 nm to about 300 nm.

[0006] According to one aspect of the present disclosure, a method of surface treatment includes: providing a component including a bulk layer containing aluminum and magnesium in a process chamber; annealing the component to form a surface region on the bulk layer including a magnesium content higher than the magnesium content of the bulk layer; generating a fluorine plasma using a remote plasma source connected to the process chamber; and forming a protective layer on the surface region by providing the fluorine plasma to the process chamber, wherein the protective layer includes magnesium fluoride, wherein the magnesium content of the component is about 0.5 wt % to about 5.5 wt %, and wherein the thickness of the protective layer is about 100 nm to about 300 nm.

[0007] According to an embodiment of the present disclosure, magnesium fluoride can be formed on the surface of a component including aluminum, thereby preventing fluorine radicals from penetrating into the component and preventing aluminum fluoride from forming. Therefore, the life cycle of the component can be extended, and particles in the process chamber can be prevented and reduced.

[0008] Suppressing aluminum fluoride with a protective layer can reduce the variation of the surface roughness of the component, thereby maintaining constant conditions in the process chamber. When performing thin film deposition using a deposition process during semiconductor processing, roughness variations of the fluorinated showerhead may cause temperature variations in the substrate or chamber impedance, thereby preventing a decrease in the film deposition rate, thereby reducing time-related variations in the semiconductor manufacturing process.

[0009] The advantages and effects of the present disclosure are not limited to the foregoing and may be more easily understood in the course of describing specific embodiments of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The above and other aspects, features and advantages of the present disclosure will be more clearly understood from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0011] Figure 1 is a flow chart showing a method of surface treatment according to an embodiment of the present disclosure;

[0012] Figure 2 is a schematic configuration diagram of a surface treatment apparatus according to an embodiment of the present disclosure;

[0013] Figures 3 to 5 is a diagram showing a surface treatment method according to an embodiment of the present disclosure;

[0014] Figure 6 is a flow chart showing a method of surface treatment according to an embodiment of the present disclosure;

[0015] Figure 7 and Figure 8 is a view showing a surface treatment method according to an embodiment of the present disclosure; and

[0016] Fig. 9 is a view illustrating an annealing method according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0017] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. The embodiments described herein are non-limiting example embodiments, and therefore, the present disclosure is not limited thereto and may be implemented in various other forms.

[0018] Although the terms "first", "second", etc. may be used to describe various elements or components in this article, these elements or components should not be limited by these terms. These terms are only used to distinguish one element or component from another element or component. Therefore, without departing from the technical spirit of the present disclosure, the first element or component discussed below may be referred to as the second element or component.

[0019] When an element or layer is referred to as being “on,” “over,” “up,” “under,” “below,” “connected to,” or “coupled to” another element or layer, it may be directly on, over, over, under, under, connected to, or coupled to the other element or layer, or intervening elements or layers may be present. In contrast, when an element is referred to as being “directly on,” “directly over,” “directly on,” “directly under,” “directly under,” “directly under,” “directly connected to,” or “directly coupled to” another element or layer, there are no intervening elements or layers.

[0020] The terms "include" and "comprises" and their derivatives refer to unlimited inclusion. The term "or" is an inclusive term meaning "and / or". The phrase "associated with..." and its derivatives refer to including, being included, interconnected with..., containing, being contained within, being connected to or connected with..., being coupled to or coupled with..., being communicable with..., cooperating with..., interlaced, juxtaposed, close to, being combined with or combined with..., having, having... attributes, having a relationship with... or with..., etc. When used with a list of items, the phrase "at least one of..." means that different combinations of one or more of the listed items can be used, and only one item in the list may be needed. In one embodiment, "at least one of A, B, and C" includes any one of the following combinations: A, B, C, A and B, A and C, B and C, A and B and C, and any variants thereof. Similarly, the term "group" means one or more. Therefore, the group of items can be a single item or a collection of two or more items.

[0021] In the detailed description, components described with reference to terms such as "component", "unit", "module", "block", "er or or", and the functional blocks shown in the drawings will be implemented using software, hardware, or a combination thereof. In one embodiment, the software may be machine code, firmware, embedded code, and application software. In one embodiment, the hardware may include circuits, electronic circuits, processors, computers, integrated circuits, integrated circuit cores, pressure sensors, inertial sensors, micro-electromechanical systems (MEMS), passive components, or a combination thereof.

[0022] Figure 1is a flowchart illustrating a method of surface treatment according to an embodiment of the present disclosure.

[0023] exist Figure 1 In the present invention, the method for surface treatment of a component according to an embodiment of the present disclosure may include: providing a component in a process chamber connected to a remote plasma source (operation S110); generating fluorine plasma from the remote plasma source (operation S120); heating the component (operation S130); and forming a protective layer on the surface of the component by providing the generated fluorine plasma to the process chamber (operation S140).

[0024] Figures 3 to 5 is a diagram illustrating a surface treatment method according to an embodiment of the present disclosure.

[0025] Figure 2 is a schematic configuration diagram of a surface treatment apparatus according to an embodiment of the present disclosure. Figure 3 A process chamber of a processing device 1 according to an embodiment is shown.

[0026] exist Figure 2 In the embodiment, the processing device 1 according to the present disclosure may include a plurality of process chambers 11 to 14. At least one of the plurality of process chambers 11 to 14 may be a process chamber for surface treatment. In addition, in an embodiment, at least one of the plurality of process chambers 11 to 14 may be a process chamber for performing a semiconductor device manufacturing process.

[0027] The transfer chamber 20 and the load-lock chamber 40 may include a transfer robot 30, and the transfer robot 30 of the transfer chamber 20 and the load-lock chamber 40 may transfer components and substrates W as process objects. In one embodiment, the transfer robot 30 of the transfer chamber 20 may remove process objects such as substrates W from the load-lock chamber 40, and transfer the process objects to a plurality of process chambers 11 to 14, or transfer the process objects between the plurality of process chambers 11 to 14. In an embodiment of the present disclosure, the transfer robot 30 may be a handler. The transfer robot 30 may include a chuck for fixing the process object, and a plurality of protrusions contacting the process object may be formed on the upper portion of the chuck. The transfer robot 30 may also include a linear stage for transferring the process object.

[0028] Figure 3 The process chamber 100 shown in FIG. Figure 2 One process chamber among the multiple process chambers 11 to 14 shown in FIG.

[0029] In an embodiment of the present disclosure, the process chamber 100 may include a housing 102, an outlet 104, a support 110, a focus ring 120, an insulating ring 130, a support ring 135, an edge ring 140, an isolator 150, a showerhead 160, a first power supply 170, and a second power supply 180. The housing 102 may provide a space therein in which a surface treatment process such as plasma fluoride treatment is performed. The outlet 104 may discharge byproducts generated in the above process.

[0030] The support member 110 may support an object to be processed. In an embodiment of the present disclosure, the object to be processed may be a component constituting the process chamber 100. The support member 110 may be an electrostatic chuck, and may include a lower electrode 112 and a heater 114.

[0031] The support 110 may heat the object to be processed placed thereon. In one embodiment, the object to be processed may be heated by a heater 114 disposed in the support 110. A flow path through which a coolant flows may be formed in the support 110, and the object to be processed may be cooled by the coolant. In some embodiments of the present disclosure, the heater 114 may be disposed outside the support 110.

[0032] The focus ring 120 may be disposed to surround an edge of an upper surface of the support 110. The focus ring 120 may surround a portion of the support 110 on which an object to be processed is disposed. That is, the focus ring 120 may have an annular shape surrounding an upper portion of the support 110. The focus ring 120 may prevent damage to the support 110 during a plasma treatment process.

[0033] In one embodiment, when the focus ring 120 includes a conductive material, the focus ring 120 may have an electrode property as a conductor through which current flows. The focus ring 120 may be used to expand the electric field region formed between the lower electrode 112 and the showerhead 160 so that the object to be processed is uniformly processed as a whole. The focus ring 120 may be formed of a semiconductor material such as silicon (Si), silicon carbide (SiC), and gallium arsenide (GaAs).

[0034] The insulating ring 130 may have an annular shape to surround the outer peripheral surface of the focus ring 120. The insulating ring 130 may include a material different from that of the focus ring 120. More specifically, in an etching process using plasma, the insulating ring 130 may include a material having etching resistance compared to the focus ring 120. In one embodiment, the insulating ring 130 may include quartz.

[0035] The edge ring 140 may have a ring shape surrounding a lower portion of the support 110. The edge ring 140 may be disposed below the focus ring 120 and the insulation ring 130, and may support the focus ring 120 and the insulation ring 130. The edge ring 140 may include a metal material.

[0036] The insulation ring 130 may be supported by a support ring 135. The support ring 135 may contact a portion of a lower surface of the insulation ring 130. The support ring 135 may be disposed to surround an outer peripheral surface of the edge ring 140. The support ring 135 may include a material resistant to etching in a plasma etching gas, such as quartz, but the present disclosure is not limited thereto.

[0037] The isolator 150 may be disposed below the support 110. The isolator 150 may include an insulating material, such as ceramic. The focus ring 120, the insulating ring 130, the support ring 135, and the edge ring 140 may form a ring structure. In some embodiments of the present disclosure, the ring structure and the isolator 150 may include aluminum (Al) and magnesium (Mg).

[0038] The shower head 160 may be disposed in an upper portion of the process chamber 100 and may be disposed to face the support member 110. The shower head 160 may be used as an RF electrode for spraying a process gas onto an object to be processed or generating plasma. In one embodiment, the lower electrode 112 may be connected to a first power source 170, the shower head 160 may be connected to a second power source 180, and the lower electrode 112 and the shower head 160 may be used to generate plasma in the process chamber 100. The shower head 160 may be formed of a conductive material or may include a metal electrode. In one embodiment, the shower head 160 may be made of aluminum (Al) or an alloy including aluminum (Al). In an embodiment of the present disclosure, a heater may be included in the shower head 160 to heat the shower head 160.

[0039] In an embodiment of the present disclosure, the process chamber 100 may be connected to a remote plasma source 200 and a gas supply unit 210. In one embodiment, the gas supply unit 210 may provide a source gas g1 to the remote plasma source 200. The remote plasma source 200 may be connected to a third power source 220 and may form plasma from the source gas g1. The plasma formed in the remote plasma source 200 may be provided to a space in the process chamber 100 through the showerhead 160.

[0040] In an embodiment of the present disclosure, the process chamber 100 may further include a liner. The liner may have a cylindrical shape whose upper and lower surfaces are open. In one embodiment, an inner portion of the liner may be disposed around the isolator 150 and the support ring 135, and an outer portion of the liner may be disposed along a side wall of the process chamber 100. The liner may be used to prevent the process chamber 100 from being damaged by arc discharge. In one embodiment, the liner may include a conductive material, such as aluminum (Al).

[0041] In the following, reference will be made to Figure 1 , Figure 3 , Figure 4 and Figure 5 A method of surface treatment of a component is described. Surface treatment of a component may be performed prior to installing or replacing the component in a semiconductor manufacturing process chamber.

[0042] exist Figure 1 and Figure 3 In the process chamber 100 connected to the remote plasma source 200, a component 300 may be provided (operation S110). In the present specification, a "component" may refer to a component constituting a process chamber. In one embodiment, the component 300 may be a component constituting a deposition process chamber or an etching process chamber among the plurality of process chambers 11 to 14. Since the component 300 is provided in the process chamber 100 for surface treatment, after the surface treatment is completed, the component 300 may be installed in a process chamber that is the same as or different from the process chamber 100 in which the surface treatment is performed.

[0043] In an embodiment of the present disclosure, the component 300 may be formed of aluminum (Al), or may be formed of an aluminum alloy including aluminum (Al). In an embodiment, in addition to aluminum (Al), the component 300 may also include materials such as magnesium (Mg), silicon (Si), chromium (Cr), and copper (Cu).

[0044] In some embodiments of the present disclosure, the component 300 may be a component including aluminum (Al), such as the nozzle 160, the inner wall of the housing 102, the inner wall of the outlet 104, the liner, or the heater 114. In an embodiment of the present disclosure, the component 300 may include aluminum (Al) and magnesium (Mg), and the content of magnesium (Mg) may be about 0.5 to about 5.5 wt% by weight (wt%). In an embodiment of the present disclosure, the magnesium (Mg) content of the component 300 may be about 0.5 wt% to about 2 wt%, or about 2 wt% to about 5.5 wt%.

[0045] In an embodiment of the present disclosure, the component 300 may be disposed on the upper surface of the support 110. Since the component 300 is disposed on the support 110 to heat the component 300, the position of the component 300 is not limited thereto. Figure 3 The shape of the component 300 shown in FIG. 1 is exemplary, and the present disclosure is not limited thereto. In some embodiments of the present disclosure, the component 300 may be disposed at a position other than the upper surface of the support member 110. In one embodiment, the component 300 may be surface-treated while being installed in the process chamber 100. When the nozzle 160 is surface-treated, the surface treatment may be performed while the nozzle 160 is installed to face the support member 110 in the process chamber 100, such as Figure 3 shown.

[0046] exist Figure 1 and Figure 4 In the embodiment, fluorine plasma may be generated in the remote plasma source 200 (operation S120). In one embodiment, the gas supply unit 210 may provide a source gas g1 to the remote plasma source 200. The source gas g1 may be a gas containing fluorine to form fluorine plasma. In one embodiment, the source gas g1 may include NF 3 , SF 6 CF 4 , CHF 3 , CH 3 F, CH 2 F 2 , C 2 F 6 , C 4 F 8 , HF, C 2 F 4 , C 3 F 6 and C 4 F 8 In the embodiment of the present disclosure, the source gas g1 may include NF 3 The third power source 220 connected to the remote plasma source 200 may operate at a power of about 1000 W to about 30000 W. The remote plasma source 200 receiving the source gas g1 may form fluorine plasma including fluorine radicals.

[0047] In addition, the component 300 may be heated (operation S130). Heating the component 300 (operation S130) may be performed simultaneously with generating the fluorine plasma (operation S120). In one embodiment, the component 300 may be heated at a temperature of about 380°C to about 500°C. The component 300 may be heated by methods such as conduction, convection, or radiation. In one embodiment, the component 300 may receive heat through the support 110, or may be heated by other means. By heating the component 300, magnesium (Mg) atoms contained in the component 300 may move to the surface of the component 300 to generate and increase the surface segregation of magnesium (Mg). In one embodiment, when heating a component 300 having a magnesium (Mg) content of about 1wt%, the magnesium (Mg) content on the surface of the component 300 may increase to about 4wt%. When the component 300 is heated at a temperature of 380°C or less, the surface segregation phenomenon may not be sufficient. In one embodiment, when exposed to fluorine plasma, the (dense) protective layer 330 described below may not be formed, or the thickness of the protective layer 330 may not be thick enough. When the component 300 is heated at a temperature of 500° C. or higher, physical properties of the component 300 may be impaired and strength thereof may be reduced.

[0048] exist Figure 1 and Figure 5 In the process chamber 100, the generated plasma may be provided to form a protective layer 330 on the surface of the component 300 (operation S140). In one embodiment, the gas supply unit 210 may provide a carrier gas to the remote plasma source 200, and a gas g2 including fluorine plasma and a carrier gas may be provided into the process chamber 100 through the showerhead 160. The carrier gas may include an inert gas. In one embodiment, the carrier gas may include argon (Ar), helium (HHe), and nitrogen (N 2 ) at least one of the following. The pressure of the fluorine plasma provided to the process chamber 100 may be about 0.5 Torr to about 10 Torr. Note that "Torr" is a unit of pressure precisely defined as 1 / 760 of a standard atmospheric pressure (101325 Pa). The flow rate of the fluorine plasma and the carrier gas may be about 1000 sccm to 15000 sccm. Note that "sccm" (standard cubic centimeter per minute) is a unit used to define the flow rate of a fluid. 1 sccm is equivalent to 1 cm 3 STP The time for providing the fluorine plasma into the process chamber 100 may be about 1 minute to about 1000 minutes.

[0049] Heating the component (operation S130) may be performed before plasma is provided to the process chamber 100, and may be continued in the operation (operation S140) of forming the protective layer 330. In one embodiment, the component 300 may be heated at a temperature of about 380°C to about 500°C while fluorine plasma is provided to the process chamber 100.

[0050] The fluorine plasma provided into the process chamber 100 may react with magnesium (Mg) contained in the component 300 to form the protective layer 330. In an embodiment of the present disclosure, the protective layer 330 may include magnesium fluoride (MgF 2 The protective layer 330 may be formed on the entire surface or a portion of the surface of the component 300 .

[0051] When the component 300 including aluminum (Al) is used, aluminum fluoride (AlF) may be formed by a cleaning gas including fluorine (F) during a cleaning process. 3 ). Aluminum fluoride (AlF 3 ) can form a porous layer on the surface of the component 300. Fluorine radicals can penetrate into aluminum fluoride (AlF 3 ) to cause continuous fluorination, aluminum fluoride (AlF 3 ) may evaporate at a high temperature to cause aluminum particles in the process chamber 100, and the surface roughness of the component 300 may increase. However, according to an embodiment of the present disclosure, magnesium fluoride (MgF 2 ) may be formed on the surface of the component 300. Since the protective layer 330 is not a porous layer but a dense layer, it is possible to prevent fluorine radicals from penetrating into the component 300, and thus it is possible to suppress the formation of magnesium fluoride (MgF 2 ) is fluorinated. Therefore, defects in semiconductor devices can be reduced by reducing particles in process chamber 100. In addition, time-related changes in the process can be reduced by maintaining constant conditions on the surface of the component. In one embodiment, during a deposition process (such as chemical vapor deposition (CVD), atomic vapor deposition (ALD), and physical vapor deposition (PVD)) during a semiconductor process, changes in emissivity caused by the formation of aluminum fluoride in showerhead 160 can be suppressed to constantly maintain the temperature of the substrate during the semiconductor manufacturing process, thereby maintaining a film deposition rate of the semiconductor device.

[0052] In an embodiment of the present disclosure, the thickness of the protective layer 330 may be about 100 nm to about 300 nm. In an embodiment, the porosity of the protective layer 330 may be about 0.1% to about 1%. In an embodiment, the protective layer 330 does not include aluminum fluoride (AlF 3 ), and may include magnesium fluoride (MgF 2 ) single layer.

[0053] In the embodiments of the present disclosure, magnesium fluoride (MgF 2 ) can also be formed on the surface of the aluminum-containing component among the components of the process chamber 100 by the above-mentioned surface treatment method.

[0054] In an embodiment of the present disclosure, a seasoning process may be performed in the process chamber 100 in which the process of forming the protective layer (operation S140) has been performed. In one embodiment, the process of forming the protective layer 330 (operation S140) may be performed in a state where the component 300 is installed in the process chamber 100, and the process chamber 100 may be cleaned by the process of forming the protective layer 330 (operation S140), so that a separate seasoning process is not required.

[0055] The aging process refers to the process of replacing the component 300 of the process chamber 100 and before forming the circuit element by repeating the deposition process and using a NF 3 The cleaning process of the cleaning gas forms a fluoride layer on the surface of the inner wall of the process chamber 100. This means that a constant state of the process chamber 100 is maintained. As in the embodiment of the present disclosure, when the surface treatment is performed in a state where the component 300 is installed in the process chamber 100, the aging process can be omitted.

[0056] In some embodiments of the present disclosure, after forming the protective layer 330, the component 300 may be installed in a process chamber different from the process chamber 100 in which the process of forming the protective layer 330 (operation S130) is performed. In this case, since magnesium fluoride (MgF 2 ) is formed on the surface of the component 300, so the aging process can be omitted or the time of the aging process can be reduced after the component 300 is mounted.

[0057] Generally, as the semiconductor device manufacturing process is repeated, components in the process chamber may deteriorate. In one embodiment, a fluorine-containing gas may be used during the etching and dry cleaning processes, and the components in the process chamber may react with fluorine radicals generated from the gas to be fluorinated. As a result, aluminum fluoride (AlF 3 ), and aluminum fluoride (AlF 3 ) may evaporate at high temperatures, which may result in particles in the process chamber and may cause defects in the semiconductor device. In addition, when a deposition process is performed using a fluorinated showerhead, changes in emissivity due to changes in surface roughness may result in changes in the temperature of the substrate and may reduce the deposition rate of the thin film.

[0058] However, according to an embodiment of the present disclosure, magnesium fluoride (MgF2 ) can be formed on the surface of the component including aluminum, and the protective layer can prevent the aluminum included in the component from being fluorinated. Therefore, even if the semiconductor manufacturing process and the cleaning process of the process chamber are repeated, the conditions in the chamber can be kept constant. In addition, the reduction in the deposition rate of the thin film can be prevented, and the generation of particles in the process chamber can be prevented and reduced. Therefore, defects in semiconductor devices manufactured in the process chamber can be prevented and reduced.

[0059] Figure 6 is a flowchart illustrating a method of surface treatment according to an embodiment of the present disclosure.

[0060] exist Figure 6 In the method of surface treatment according to an embodiment of the present disclosure, the component 300 may be provided in a process chamber connected to a remote plasma source 200 (operation S110); annealing the component 300 (operation S220); generating plasma through the remote plasma source 200 (operation S230); and forming a protective layer 330 on the surface of the component 300 by providing the generated plasma to the process chamber (operation S240). Since operations S110, S230, and S240 may be similar to those of reference 1, Figure 1 The operations described are the same or similar, so their detailed descriptions may be omitted.

[0061] Figure 7 and Figure 8 is a view illustrating a surface treatment method according to an embodiment of the present disclosure.

[0062] exist Figure 6 and Figure 7 In an embodiment of the present disclosure, after the component 300 is provided in the process chamber 100 (operation S110), the component 300 may be annealed (operation S220). In one embodiment, the component 300 may be annealed in a vacuum state in the inner space of the process chamber 100. In an embodiment of the present disclosure, the component 300 may be heated at a temperature of about 380° C. to about 500° C. The pressure in the process chamber 100 may be about 5 mTorr to about 50 mTorr. The annealing time may be about 1 hour to about 5 hours.

[0063] like Figure 7As shown, the component 300 may include a surface region 320 near the surface S and a main layer 310 below the surface region 320. The main layer 310 may include aluminum (Al), magnesium (Mg), and other metal elements. As described above, when the component 300 is heated, surface segregation may occur. Therefore, magnesium (Mg) included in the main layer 310 may move to the surface S to form a surface region 320 having a magnesium (Mg) content that is relatively higher than that of the main layer 310. In one embodiment, when a component 300 having a magnesium (Mg) content of 1 wt% or less is annealed, the magnesium (Mg) content on the surface S of the component 300 may increase to 4 wt% or more.

[0064] exist Figure 6 and Figure 8 In the process, plasma may be provided to the process chamber 100 to form a protective layer 330 on the surface of the component 300 (operation S240). The protective layer 330 may be formed in the surface region 320. As described above, the protective layer 330 may include magnesium fluoride (MgF 2 ) and can prevent aluminum fluoride (AlF 3 )’s formation.

[0065] In reference Figure 1 In the surface treatment method described above, a Figure 7 and Figure 8 Surface area 320 and protective layer 330 are shown.

[0066] Table 1:

[0067] Mg content <![CDATA[AlF 3 Form]]> <![CDATA[MgF 2 Thickness(t)]]> Comparative Example 1 Mg<0.5wt% O t=44~54nm Comparative Example 2 0.5wt%<Mg<2.0wt% O - Example 1 of the present disclosure 0.5wt%<Mg<2.0wt% X t=100~150nm Example 2 of the present disclosure 2.0wt% <Mg<5.5wt% X t=240~330nm Comparative Example 3 Mg>5.5wt% - -

[0068] Table 1 shows the results of forming the protective layer according to the examples of the present disclosure and the comparative examples of the present disclosure. The components used in the examples of the present disclosure and the comparative examples of Table 1 are metals including aluminum (Al) and magnesium (Mg).

[0069] In Table 1, for Comparative Example 1, the content of magnesium (Mg) is 0.5 wt % or less. As a result of the surface treatment of the component of Comparative Example 1, a surface layer including magnesium fluoride (MgF 2 ) protective layer, but magnesium fluoride (MgF 2 ) has a thickness of 44 nm to 54 nm and cannot prevent the penetration of fluorine radicals. That is, magnesium fluoride (MgF 2 ) reacts with fluorine radicals to form aluminum fluoride (AlF 3 ).

[0070] For Comparative Example 2 and Example 1 of the present disclosure, the content of magnesium (Mg) was 0.5 wt % or more and 2.0 wt % or less. Before the surface treatment process, the component of Comparative Example 2 was not subjected to an annealing process, but the component of Example 1 of the present disclosure was subjected to an annealing process.

[0071] In the component of Comparative Example 2, magnesium fluoride (MgF 2 ) and aluminum fluoride (AlF 3 ). Magnesium fluoride (MgF 2 ) and aluminum fluoride (AlF 3 ) exist in a mixed state to form a porous layer. However, magnesium fluoride (MgF 2 ) is formed on the surface of the component of Example 1 of the present disclosure to have a thickness of 100 nm to 150 nm, and no aluminum fluoride (AlF 3 ).

[0072] In the case of Example 2 of the present disclosure, the content of magnesium (Mg) is 2.0 wt % or more and 5.5 wt % or less. As a result of the surface treatment of the component of Example 2 of the present disclosure, magnesium fluoride (MgF 2 ) is formed to have a thickness between 240 nm and 330 nm, and no aluminum fluoride (AlF 3 ).

[0073] In the case of Comparative Example 3, the content of magnesium (Mg) is 5.5 wt % or more. As a result of the surface treatment of the component of Comparative Example 3, magnesium fluoride (MgF 2 ) without forming aluminum fluoride (AlF 3 ). However, when a component includes 5.5 wt % or more of magnesium (Mg), it may be easily corroded and cracked at high temperatures.

[0074] Therefore, the content of magnesium (Mg) of the component according to the embodiment of the present disclosure may be about 0.5 wt % to about 5.5 wt %. Here, the content of magnesium (Mg) of the component may refer to the content of magnesium (Mg) in the body layer 310 .

[0075] Fig. 9 is a view illustrating an annealing method according to an embodiment of the present disclosure. Fig. 9 The magnesium (Mg) content of the surface of the component according to the heating temperature is shown.

[0076] exist Fig. 9 According to Example 3 of the present disclosure, before annealing (corresponding to Fig. 9 The content of magnesium (Mg) on ​​the surface of the component having only Al in the embodiment of the present invention may be about 1 wt %. Fig. 9As shown, the content of magnesium (Mg) on ​​the surface of the component increases as the temperature increases, and when the temperature of the component is about 460° C., the content of magnesium (Mg) is about 3 wt %.

[0077] According to Example 4 of the present disclosure, the content of magnesium (Mg) on ​​the surface of the component before annealing may be about 3 wt %. The content of magnesium (Mg) on ​​the surface of the component increases with increasing temperature, and when the temperature of the component is about 460° C., the content of magnesium (Mg) may be about 6 wt %.

[0078] Therefore, in order to increase the forming speed and thickness of the protective layer, the component may be heated at about 380° C. or higher. In addition, as described above, the component heating temperature may be about 500° C. or lower to prevent the strength of the component from being reduced.

[0079] Table 2:

[0080]

[0081]

[0082] Table 2 shows the comparison of the protective layer formation and high temperature cleaning process (repeated 200 times) according to the examples and comparative examples of the present disclosure. 2 ) and the results of fluorine radical penetration. The surface roughness before surface treatment was evaluated in samples controlled to 0.1 μm. The components used in the examples and comparative examples of the present disclosure of Table 2 are metals including aluminum (Al) and magnesium (Mg).

[0083] In Table 2, in Comparative Example 4, after direct plasma is formed in the process chamber, a plasma in which magnesium fluoride (MgF 2 ) and aluminum fluoride (AlF 3 ) porous layer. After surface treatment, the surface roughness increased to 0.33. The change in surface roughness of the component may affect the semiconductor manufacturing process. Due to the cleaning process, magnesium fluoride (MgF 2 ) and aluminum fluoride (AlF 3 ) induces time-dependent changes in the mixed fluoride layer. 3 ) is partially etched and magnesium fluoride (MgF 2 ) grows, but magnesium fluoride (MgF 2 ) did not form a dense monolayer.

[0084] In the case of Example 5 of the present disclosure, a fluorine plasma including fluorine radicals formed by remote plasma is used, and magnesium fluoride (MgF 2 ) forms a dense monolayer with a thickness of 165 nm on the surface of the component. After the cleaning process, magnesium fluoride (MgF2 ) was maintained at 213 nm, similar to the thickness before the surface treatment. In the case of Example 5 of the present disclosure, the surface roughness of the component was almost unchanged before and after the protective layer was formed and before and after the cleaning process. Since the surface roughness and composition did not change after the cleaning process, the conditions of the semiconductor device process chamber can be kept constant without degradation of the component.

[0085] In the case of Comparative Example 5, fluorine ions were implanted into the surface of the component by an ion implantation process in a process chamber. Magnesium fluoride (MgF 2 ) forms a dense monolayer with a thickness of 75 nm on the surface of the component. After surface treatment, the surface roughness increases to 0.37. After the cleaning process, magnesium fluoride (MgF 2 ) increased to 150 nm to 230 nm, and the surface roughness increased to 0.44. As described above, the change in the surface roughness of the component may affect the semiconductor manufacturing process.

[0086] Comparing the results of Comparative Example 4 and Example 5, it can be seen that the surface roughness of the component according to Example 5 of the present disclosure using the remote plasma source 200 is almost unchanged, and magnesium fluoride (MgF 2 ).

[0087] The present disclosure is not limited to the above embodiments and drawings, but is limited by the appended claims. Therefore, without departing from the scope of the present disclosure defined by the appended claims, a person of ordinary skill in the art may make various substitutions, modifications or changes, and these substitutions, modifications or changes should be interpreted as being included within the scope of the present disclosure.

Claims

1. A surface treatment method, the surface treatment method include: providing a component in a first process chamber; generating a fluorine plasma using a remote plasma source connected to the first process chamber; as well as forming a protective layer on a surface of the component by providing the fluorine plasma to the first process chamber, Wherein, the protective layer comprises magnesium fluoride, wherein the magnesium content of the component is 0.5wt% to 5.5wt%, and Wherein, the thickness of the protective layer is 100nm to 300nm.

2. The surface treatment method according to claim 1, in, Forming the protective layer includes heating the component at a temperature of 380°C to 500°C.

3. The surface treatment method according to claim 1, in, Forming the protection layer includes maintaining a pressure of the first process chamber at 0.5 Torr to 10 Torr.

4. The surface treatment method according to claim 1, further comprising: include: The component is heated by an annealing process before the fluorine plasma is provided to the first process chamber. 5 . The surface treatment method according to claim 4 , further comprising increasing the magnesium content of the surface of the component by the annealing process. 6 . The surface treatment method according to claim 4 , further comprising performing the annealing process for 1 hour to 5 hours. 7 . The surface treatment method according to claim 4 , further comprising performing the annealing process at a pressure of 5 mTorr to 50 mTorr.

8. The surface treatment method according to claim 1, in, The component includes a bulk layer comprising aluminum and magnesium, and Wherein, the protective layer is arranged on the main body layer.

9. The surface treatment method according to claim 8, in, The protective layer does not include aluminum fluoride.

10. The surface treatment method according to claim 1, further comprising providing a source gas to the remote plasma source, in, The fluorine plasma is generated from the source gas.

11. The surface treatment method according to claim 10, in, The source gas includes NF 3 , SF 6 CF 4 , CHF 3 , CH 3 F, CH 2 F 2 , C 2 F 6 , C 4 F 8 , HF, C 2 F 4 , C 3 F 6 and C 4 F 8 At least one of . 12 . The surface treatment method according to claim 1 , further comprising installing the component on which the protection layer is formed in a second process chamber.

13. The surface treatment method according to claim 1, in, The porosity of the protective layer is 0.1% to 1%.

14. The method of claim 1, further comprising operating a power supply connected to the remote plasma source at a power of 1000W to 30000W.

15. The surface treatment method according to claim 1, in, The first process chamber includes a support member, the support member includes a heater, and Wherein, the component is arranged on the support member.

16. A surface treatment method, the surface treatment method include: Installing components in process chambers; generating a fluorine plasma using a remote plasma source connected to the process chamber; as well as forming a protective layer on a surface of the component by providing the fluorine plasma to the process chamber, Wherein, the protective layer comprises magnesium fluoride, wherein the magnesium content of the component is 0.5wt% to 5.5wt%, and Wherein, the thickness of the protective layer is 100nm to 300nm.

17. The surface treatment method according to claim 16, in, Installing the component in the process chamber includes installing the component in the process chamber including: a housing; a support member, the support member being located at a lower portion of the housing; a ring structure, the ring structure surrounding a side surface of the support member, and an isolator, the isolator being disposed below the support member; a spray head, the spray head being located at an upper portion of the housing and facing the support member; and an outlet located on a side wall of the housing, Wherein, the component includes at least one of a first inner wall of the shell, a second inner wall of the outlet, the ring structure, the isolator and the nozzle.

18. The surface treatment method according to claim 16, in, The protective layer is a single layer containing magnesium fluoride but not aluminum fluoride.

19. A surface treatment method, the surface treatment method include: providing a component including a bulk layer including aluminum and magnesium in a process chamber; annealing the component to form a surface region on the bulk layer comprising a magnesium content greater than a magnesium content of the bulk layer; generating a fluorine plasma using a remote plasma source coupled to the process chamber; and forming a protective layer on the surface region by providing the fluorine plasma to the process chamber, Wherein, the protective layer comprises magnesium fluoride, wherein the magnesium content of the component is 0.5wt% to 5.5wt%, and Wherein, the thickness of the protective layer is 100nm to 300nm.

20. The surface treatment method according to claim 19, in, The protective layer is disposed on the body layer and does not include aluminum fluoride.