Novel gallium source degassing method
The multi-step heating and degassing method removes impurities and oxides from the gallium source, which solves the problem of the number of defects and large-size defects in the GaAs epitaxial layer, and significantly improves the device performance.
Patent Information
- Application Number
- CN202411126716.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The higher number of defects and large-size defects in GaAs semiconductor materials lead to degradation of device performance, especially due to the difficulty in effectively reducing epitaxial layer defects caused by sputtering of gallium sources and volatilization of gallium oxide.
The gallium source was removed by multi-step heating and degassing method, and the Ga source was subjected to multiple heating and cooling treatments under vacuum conditions. The GaAs epitaxial layer was grown in the growth room. The number of defects was verified by characterizing Surfscan and electron microscope. The reduction.
The number of defects and large-size defects in the GaAs epitaxial layer is significantly reduced, and the device performance is improved. Especially after the third step of degassing, the number of defects >5μm size is greatly reduced.
Smart Images

Figure HDA0004996624880000011 
Figure HDA0004996624880000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of group III compound materials, and in particular to a novel gallium source degassing method. Background Art
[0002] Semiconductor devices made of silicon (Si) materials have limits on the temperature and power they can withstand, which hinders their widespread application. They are also difficult to improve through device structure. Therefore, researchers have turned their attention to other semiconductor materials, making III-V compound semiconductor materials one of the hot topics of research. Among them, gallium arsenide (GaAs) is a direct bandgap semiconductor material with high photoelectric conversion efficiency, good high temperature resistance, and the ability to withstand high operating power. In addition, GaAs semiconductor materials have high electron mobility and are widely used in high-frequency devices and other fields.
[0003] For GaAs semiconductor materials, a high number of defects and large defect sizes, especially large-size defects (>2μm), will greatly reduce the performance of the device. Studies have shown that defects in GaAs epitaxial layers come from the epitaxial substrate and Ga source. The substrate will have surface atomic contamination and particles, and for the Ga source, it may be related to the sputtering of the Ga source and the volatilization of gallium oxide. Therefore, how to effectively reduce the number of defects and large-size defects in the GaAs epitaxial layer and improve device performance has become a technical problem that urgently needs to be solved. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide a novel gallium source degassing method, compared with before degassing, the number and size of defects in the grown GaAs epitaxial layer after degassing are significantly reduced.
[0005] The present invention provides a novel gallium source degassing method, comprising the following steps:
[0006] A) Gallium source degassing:
[0007] A1) placing a silicon wafer on a molybdenum tray and moving it to a sample injection chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sample injection chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.;
[0008] A2) transferring the silicon wafer treated in step A1) to a growth chamber, and heating the silicon wafer to 450-550° C. under vacuum conditions;
[0009] The source furnace equipped with Ga source is heated for the first time: the tip area on the source furnace is heated to 680-720°C, and the base area on the source furnace is heated to 480-520°C; and the heating rate of the tip area is greater than the heating rate of the base area; after keeping warm for a period of time, the source furnace equipped with Ga source is heated for the second time: the tip area on the source furnace is heated to 880-920°C, and the base area on the source furnace is heated to 660-700°C;
[0010] A3) Turn on the Ga source and As source switches at the same time, open the As source valve position to 100mil, and maintain the degassing time for 40 to 50 minutes. Then, turn off the Ga source and As source switches at the same time, set the As source valve position to 0 to 5mil, and maintain the time for 4 to 6 minutes to complete the first step of degassing;
[0011] A4) The source furnace equipped with Ga source is heated for the third time: the tip area on the source furnace is heated to 1100-1140°C, and the base area on the source furnace is heated to 840-880°C; then, the switches of Ga source and As source are turned on at the same time, the valve position of As source is opened to 150mil, and the degassing time is maintained for 30-40min, and then the switches of Ga source and As source are turned off at the same time, the valve position of As source is set to 0-5mil, and the time is maintained for 4-6min, and the second step of degassing is completed;
[0012] A5) The source furnace equipped with Ga source is heated for the fourth time: the tip area on the source furnace is heated to 1220-1260°C, and the base area on the source furnace is heated to 955-995°C; then, the Ga source and As source switches are turned on at the same time, the As source valve position is opened to 200mil, and the degassing time is maintained for 20-30min, and then the Ga source and As source switches are turned off at the same time, and the time is maintained for 4-6min, completing the third step of degassing;
[0013] A6) Cool the tip area on the source furnace to 1100-1140°C, and cool the base area on the source furnace to 840-880°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 150mil, and maintain the degassing time for 30-40min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0014] A7) Cool the tip area on the source furnace to 880-920°C, and cool the base area on the source furnace to 660-700°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 100mil, and maintain the degassing time for 20-30min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0015] A8) Cooling the tip area on the source furnace to 580-620°C, and cooling the base area on the source furnace to 480-520°C, to complete the degassing of the Ga source;
[0016] B) Growth of GaAs epitaxial layer:
[0017] After the GaAs substrate is deoxidized, the Ga and As source furnace switches are turned on at the same time to grow a GaAs epitaxial layer.
[0018] Preferably, in step A1), the degassing time in the injection chamber is 1.5 to 2.5 hours, and the degassing time in the buffer chamber is 25 to 35 minutes.
[0019] Preferably, in step A2), the vacuum condition is 3×10 -10 ~7×10 -10 Torr;
[0020] The silicon wafer temperature rise rate is 10-20°C / min.
[0021] Preferably, in step A2), during the first heating, the heating rate of the tip region and the base region is 10-18°C / min;
[0022] The insulation time is 8 to 12 minutes;
[0023] In the second heating, the heating rate of the tip and base regions is 6-12°C / min;
[0024] During the first heating process and the second heating process, the power ratio between the tip region and the base region of the Ga source is 9 to 9.2.
[0025] Preferably, in step A4), during the third heating, the heating rate of the tip region and the base region is 10-18°C / min;
[0026] During the third heating process, the power ratio between the tip region and the base region of the Ga source was 9 to 9.2.
[0027] Preferably, in step A5), during the fourth heating, the heating rate of the tip region and the base region is 6-12°C / min;
[0028] During the fourth heating process, the power ratio between the tip region and the base region of the Ga source was 9 to 9.2.
[0029] Preferably, in step A6), the rate of temperature reduction of the tip region and the base region is 3-5°C / min;
[0030] In step A7), the temperature of the tip region and the base region is reduced at a rate of 3 to 5°C / min;
[0031] In step A8), the tip region and the base region are cooled at a rate of 3-5°C / min.
[0032] Preferably, in step B), the GaAs substrate is deoxidized, comprising:
[0033] B1) placing a GaAs non-doped substrate on a molybdenum tray, and moving it to a sampling chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sampling chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.;
[0034] B2) transferring the GaAs substrate processed in step B1) to a growth chamber, heating the GaAs substrate to 250-350° C. under vacuum conditions; then, turning on the As source switch, and setting the valve position to 30 mil;
[0035] B3) heating the GaAs substrate processed in step B2) to 350-450° C., and then raising the valve position to 50 mil;
[0036] B4) heating the GaAs substrate processed in step B3) to 500-570° C., and then raising the valve position to 70 mil;
[0037] B5) heating the GaAs substrate treated in step B4) to 580-630°C, raising the valve position to 100-180 mil, and completing the deoxidation of the GaAs substrate at 600-620°C.
[0038] Preferably, in step B1), the degassing time in the injection chamber is 1.5 to 2.5 hours, and the degassing time in the buffer chamber is 25 to 35 minutes;
[0039] In step B2), the vacuum condition is 3×10 -10 ~7×10 -10 Torr;
[0040] The heating rate of GaAs substrate is 10-20℃ / min;
[0041] Step B2) The temperature of the treated GaAs substrate is raised at a rate of 10-20° C. / min;
[0042] Step B3) The temperature of the treated GaAs substrate is raised at a rate of 8-12°C / min;
[0043] The heating rate of the GaAs substrate after step B4) is 3-7°C / min.
[0044] Preferably, in step B), the growth rate of growing the GaAs epitaxial layer is 0.8 to 1.2 ML / s;
[0045] After the growth of the GaAs epitaxial layer is completed, the method further includes: closing the Ga source furnace switch and cooling down in an As atmosphere; the temperature after cooling down is 130-170°C.
[0046] The present invention provides a novel gallium source degassing method, including gallium source degassing and growth of GaAs epitaxial layer, specifically including the following steps: A) gallium source degassing: A1) placing a silicon wafer on a molybdenum tray, and moving it to a sampling chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sampling chamber is 150-200°C, and the degassing temperature of the buffer chamber is 300-350°C; A2) transferring the silicon wafer treated in step A1) to a growth chamber, and heating the silicon wafer to 450-550°C under vacuum conditions; heating a source furnace equipped with a Ga source for the first time: heating a tip area on the source furnace to 680-720°C, and heating a base area on the source furnace to 480-520°C; and the heating rate of the tip area is greater than that of the base area. domain heating rate; after keeping warm for a period of time, the source furnace equipped with Ga source is heated for the second time: the tip area on the source furnace is heated to 880-920°C, and the base area on the source furnace is heated to 660-700°C; A3) the switches of Ga source and As source are turned on at the same time, the valve position of As source is opened to 100mil, and the degassing time is maintained for 40-50min, then, the switches of Ga source and As source are turned off at the same time, the valve position of As source is set to 0mil, and the maintenance time is 4-6min, completing the first step of degassing; A4) the source furnace equipped with Ga source is heated for the third time: the tip area on the source furnace is heated to 1100-1140°C, and the base area on the source furnace is heated to 840-880°C; then, Open the switches of Ga source and As source, open the valve position of As source to 150mil, maintain the degassing time for 30 to 40min, then close the switches of Ga source and As source at the same time, set the valve position of As source to 0mil, maintain the time for 4 to 6min, and complete the second step of degassing; A5) Heat up the source furnace equipped with Ga source for the fourth time: heat the tip area on the source furnace to 1220 to 1260℃, and heat the base area on the source furnace to 955 to 995℃; then, open the switches of Ga source and As source at the same time, open the valve position of As source to 200mil, maintain the degassing time for 20 to 30min, then close the switches of Ga source and As source at the same time, maintain the time for 4 to 6min, and complete the third step of degassing; A6) The tip area on the furnace is cooled to 1100-1140°C, and the base area on the source furnace is cooled to 840-880°C; the switches of the Ga source and the As source are turned on at the same time, the valve position of the As source is opened to 150mil, and the degassing time is maintained for 30-40min. After completion, the switches of the Ga source and the As source are turned off at the same time, and the valve position of the As source is set to 0mil; A7) The tip area on the source furnace is cooled to 880-920°C, and the base area on the source furnace is cooled to 660-700°C; the switches of the Ga source and the As source are turned on at the same time, the valve position of the As source is opened to 100mil, and the degassing time is maintained for 20-30min. After completion, the switches of the Ga source and the As source are turned off at the same time, and the valve position of the As source is set to 0mil;A8) Cool the tip area on the source furnace to 580-620°C, and cool the base area on the source furnace to 480-520°C to complete the degassing of the Ga source; B) Growth of GaAs epitaxial layer: After deoxidizing the GaAs substrate, turn on the Ga and As source furnace switches at the same time to grow the GaAs epitaxial layer. ;
[0047] The present invention performs multi-step temperature-raising degassing on a Ga source in a growth chamber under vacuum conditions to remove impurities and oxides in the Ga source, and grows a GaAs epitaxial layer material through an epitaxial device. The degassing method of the present invention is verified by a defect analyzer (Surfscan) and an electron microscope characterization method, and can effectively reduce the number of defects and the number of large-size defects in the GaAs epitaxial layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 Surfscan images and defect count images of GaAs materials before and after gallium source degassing;
[0049] Figure 2 Electron microscope images of GaAs material before and after gallium source degassing. DETAILED DESCRIPTION
[0050] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] The present invention provides a novel gallium source degassing method, including gallium source degassing and growth of GaAs epitaxial layer, specifically comprising the following steps:
[0052] A) Gallium source degassing:
[0053] A1) placing a silicon wafer on a molybdenum tray and moving it to a sample injection chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sample injection chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.;
[0054] A2) transferring the silicon wafer treated in step A1) to a growth chamber, and heating the silicon wafer to 450-550° C. under vacuum conditions;
[0055] The source furnace equipped with Ga source is heated for the first time: the tip area on the source furnace is heated to 680-720°C, and the base area on the source furnace is heated to 480-520°C; and the heating rate of the tip area is greater than the heating rate of the base area; after keeping warm for a period of time, the source furnace equipped with Ga source is heated for the second time: the tip area on the source furnace is heated to 880-920°C, and the base area on the source furnace is heated to 660-700°C;
[0056] A3) Turn on the Ga source and As source switches at the same time, open the As source valve position to 100mil, and maintain the degassing time for 40 to 50 minutes. Then, turn off the Ga source and As source switches at the same time, set the As source valve position to 0mil, and maintain the time for 4 to 6 minutes to complete the first step of degassing;
[0057] A4) The source furnace equipped with Ga source is heated for the third time: the tip area on the source furnace is heated to 1100-1140°C, and the base area on the source furnace is heated to 840-880°C; then, the switches of Ga source and As source are turned on at the same time, the valve position of As source is opened to 150mil, and the degassing time is maintained for 30-40min, and then the switches of Ga source and As source are turned off at the same time, the valve position of As source is set to 0mil, and the time is maintained for 4-6min, and the second step of degassing is completed;
[0058] A5) The source furnace equipped with Ga source is heated for the fourth time: the tip area on the source furnace is heated to 1220-1260°C, and the base area on the source furnace is heated to 955-995°C; then, the Ga source and As source switches are turned on at the same time, the As source valve position is opened to 200mil, and the degassing time is maintained for 20-30min, and then the Ga source and As source switches are turned off at the same time, and the time is maintained for 4-6min, completing the third step of degassing;
[0059] A6) Cool the tip area on the source furnace to 1100-1140°C, and cool the base area on the source furnace to 840-880°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 150mil, and maintain the degassing time for 30-40min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0060] A7) Cool the tip area on the source furnace to 880-920°C, and cool the base area on the source furnace to 660-700°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 100mil, and maintain the degassing time for 20-30min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0061] A8) Cooling the tip area on the source furnace to 580-620°C, and cooling the base area on the source furnace to 480-520°C, to complete the degassing of the Ga source;
[0062] B) Growth of GaAs epitaxial layer:
[0063] After the GaAs substrate is deoxidized, the Ga and As source furnace switches are turned on at the same time to grow a GaAs epitaxial layer.
[0064] In step A1):
[0065] In some embodiments of the present invention, the size of the silicon wafer is 4 inches.
[0066] The present invention uses a trolley to transport and sequentially move to a sample feeding chamber and a buffer chamber, and performs preliminary low-temperature degassing in the sample feeding chamber and the buffer chamber to reduce moisture in the silicon wafer and the molybdenum tray.
[0067] In some embodiments, the degassing temperature in the injection chamber is 200°C; and the degassing temperature in the buffer chamber is 300°C.
[0068] The degassing time in the injection chamber is 1.5 to 2.5 hours, such as 2 hours, and the degassing time in the buffer chamber is 25 to 35 minutes, such as 30 minutes.
[0069] In step A2):
[0070] The silicon wafer processed in step A1) is transferred to the growth chamber of the molecular beam epitaxy equipment. The vacuum environment in the chamber is 3×10 -10 ~7×10 -10 Torr, for example 5×10 -10 Torr. The silicon wafer is the substrate. Steps A2) to A8) are all performed under the vacuum environment.
[0071] The silicon wafer is heated at a rate of 10-20°C / min, such as 15°C / min.
[0072] In the first heating, the heating rate of the tip region and the base region is 10-18°C / min. In the present invention, the heating rate of the tip region is greater than the heating rate of the base region, mainly to prevent the heating rate from being too fast, resulting in source material accumulation at the Ga source furnace mouth.
[0073] The insulation time is 8 to 12 minutes, for example 10 minutes.
[0074] During the second heating, the heating rates of the tip region and the base region are 6 to 12°C / min.
[0075] During the first and second heating processes, TDK observed the current and voltage values of the Ga source tip region and the base region, and maintained the power ratio of the Ga source tip region and the base region at 9 to 9.2.
[0076] In step A3):
[0077] The switches of the Ga source and As source are turned on, and the As source valve position is opened to 100 mil in order to generate GaAs compounds to be deposited on the silicon wafer and reduce the contamination in the growth chamber.
[0078] In certain embodiments of the present invention, the degassing time is maintained for 45 min.
[0079] In certain embodiments of the present invention, the As source valve position is set to 0 mil and maintained for 5 minutes.
[0080] The first step of degassing is mainly to remove other impurities in the Ga source.
[0081] In step A4):
[0082] During the third heating, the heating rates of the tip and base regions were 10-18°C / min.
[0083] During the third heating process, TDK observed the current and voltage values of the Ga source tip area and base area, and kept the power ratio of the Ga source tip area and base area at 9 to 9.2.
[0084] In certain embodiments of the present invention, step A4) is repeated twice.
[0085] The second step of degassing is mainly to remove compound impurities generated by Ga.
[0086] In step A5):
[0087] In the fourth heating, the heating rates of the tip region and the base region were 6-12°C / min.
[0088] During the fourth heating process, TDK observed the current and voltage values of the Ga source tip region and the base region, and maintained the power ratio of the Ga source tip region and the base region at 9 to 9.2.
[0089] In certain embodiments of the present invention, step A5) is repeated 3 times.
[0090] The third step of degassing can greatly reduce defects >5μm in size, mainly to suppress the sputtering of Ga source.
[0091] In step A6):
[0092] The cooling rate of the tip area and the base area is 3 to 5°C / min.
[0093] In step A7):
[0094] The cooling rate of the tip area and the base area is 3 to 5°C / min.
[0095] In step A8):
[0096] The cooling rate of the tip area and the base area is 3 to 5°C / min.
[0097] In step B):
[0098] Deoxidize the GaAs substrate, including:
[0099] B1) placing a GaAs non-doped substrate on a molybdenum tray, and moving it to a sampling chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sampling chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.;
[0100] B2) transferring the GaAs substrate processed in step B1) to a growth chamber, heating the GaAs substrate to 250-350° C. under vacuum conditions; then, turning on the As source switch, and setting the valve position to 30 mil;
[0101] B3) heating the GaAs substrate processed in step B2) to 350-450° C., and then raising the valve position to 50 mil;
[0102] B4) heating the GaAs substrate processed in step B3) to 500-570° C., and then raising the valve position to 70 mil;
[0103] B5) heating the GaAs substrate treated in step B4) to 580-630°C, raising the valve position to 100 mil, and completing the deoxidation of the GaAs substrate at 600-620°C.
[0104] In step B1):
[0105] The size of the GaAs non-doped substrate is 4 inches.
[0106] The GaAs undoped substrate is placed on a molybdenum tray, transported by a trolley, and moved to the injection chamber and the buffer chamber in sequence, and preliminary low-temperature degassing is performed in the injection chamber and the buffer chamber to reduce the moisture in the GaAs substrate and the molybdenum tray.
[0107] In some embodiments, the degassing temperature in the injection chamber is 200°C; and the degassing temperature in the buffer chamber is 300°C.
[0108] The degassing time in the injection chamber is 1.5 to 2.5 hours, such as 2 hours, and the degassing time in the buffer chamber is 25 to 35 minutes, such as 30 minutes.
[0109] In step B2):
[0110] The GaAs substrate processed in step B1) is transferred to the growth chamber of the epitaxial equipment, and the vacuum environment in the chamber is 3×10 -10 ~7×10 -10 Torr, for example 5×10 -10 Steps B2) to B5) are all carried out under the vacuum environment.
[0111] In some embodiments of the present invention, the GaAs substrate is rotated and heated to 250-350° C. Specifically, the temperature after heating is 300° C. The heating rate of the GaAs substrate is 10-20° C. / min, such as 15° C. / min. Then, the As source switch is turned on, and the valve position is set to 30 mil to suppress the formation of oxides during the deoxidation process of GaAs.
[0112] In step B3):
[0113] Step B2) The heating rate of the treated GaAs substrate is 10-20°C / min, such as 15°C / min. The temperature after heating is specifically 400°C.
[0114] In step B4):
[0115] Step B3) The temperature of the treated GaAs substrate is increased at a rate of 8-12°C / min, such as 10°C / min, to a temperature of 550°C.
[0116] In step B5):
[0117] Step B4) The temperature of the treated GaAs substrate is increased at a rate of 3-7°C / min, such as 5°C / min, and the temperature after the increase is specifically 600°C.
[0118] In certain embodiments of the present invention, deoxidation of the GaAs substrate is accomplished at 610°C.
[0119] In the present invention, after the deoxidation of the GaAs substrate is completed, the Ga and As source furnace switches are turned on at the same time to grow a GaAs epitaxial layer. The growth rate is 0.8 to 1.2 ML / s, such as 1 ML / s. In some embodiments, the thickness of the GaAs epitaxial layer is 500 nm.
[0120] After the growth of the GaAs epitaxial layer is completed, the process further includes: turning off the Ga source furnace switch and cooling down in an As atmosphere. The cooling rate is 18-22°C / min, such as 20°C / min. The temperature after cooling down is 150-200°C, such as 200°C.
[0121] The present invention is carried out under ultra-high vacuum (3×10 -10 ~7×10 -10 Torr), a Ga source is subjected to multi-step temperature degassing in a growth chamber to remove impurities and oxides in the Ga source, and a GaAs epitaxial layer material is grown by an epitaxial device. A defect analyzer (Surfscan) and an electron microscope characterization method are used to verify that the degassing method of the present invention can effectively reduce the number of defects and the number of large-size defects in the GaAs epitaxial layer.
[0122] In order to further illustrate the present invention, a novel gallium source degassing method provided by the present invention is described in detail below in conjunction with embodiments, but it should not be understood as limiting the scope of protection of the present invention.
[0123] Example 1
[0124] A novel method for degassing gallium sources:
[0125] 1) Gallium source degassing:
[0126] 1-1) Place a 4-inch silicon wafer on a molybdenum tray, transfer it by a trolley, and move it to the injection chamber and the buffer chamber in turn, and perform preliminary low-temperature degassing in the injection chamber and the buffer chamber; the degassing temperature in the injection chamber is 200°C and the time is 2h; the degassing temperature in the buffer chamber is 300°C and the time is 30min;
[0127] 1-2) The silicon wafer processed in 1-1) is transferred to the growth chamber of the molecular beam epitaxy equipment, and the vacuum environment in the chamber is 5×10 -10 Torr, then the Si wafer substrate is heated to 500°C at a heating rate of 15°C / min;
[0128] The source furnace equipped with Ga source was heated for the first time: the tip area on the source furnace was heated (heating rate 15℃ / min) to 700℃, and the base area on the source furnace was heated (heating rate 10℃ / min) to 500℃; after keeping warm for 10 minutes, the source furnace equipped with Ga source was heated for the second time: the tip area on the source furnace was heated (heating rate 10℃ / min) to 900℃, and the base area on the source furnace was heated (heating rate 8℃ / min) to 680℃; during the heating process, the current and voltage values of the tip area and base area of the Ga source were observed by TDK, and the power ratio of the tip area and base area of the Ga source was kept at 9 to 9.2;
[0129] 1-3) Turn on the Ga source and As source switches at the same time, open the As source valve position to 100mil, and maintain the degassing time for 45min. Then, turn off the Ga source and As source switches at the same time, set the As source valve position to 0mil, and maintain the time for 5min to complete the first step of degassing;
[0130] 1-4) The source furnace equipped with Ga source is heated for the third time: the tip area on the source furnace is heated (heating rate 15℃ / min) to 1120℃, and the base area on the source furnace is heated (heating rate 10℃ / min) to 860℃; during the heating process, the current and voltage values of the Ga source tip area and base area are observed by TDK, and the power ratio of the Ga source tip area and base area is kept at 9 to 9.2;
[0131] Then, turn on the Ga source and As source switches at the same time, open the As source valve position to 150mil, maintain the degassing time for 35min, then turn off the Ga source and As source switches at the same time, set the As source valve position to 0mil, maintain the time for 5min, and complete the second step of degassing; repeat steps 1-4 twice);
[0132] 1-5) The source furnace equipped with Ga source is heated for the fourth time: the tip area on the source furnace is heated (heating rate 10℃ / min) to 1240℃, and the base area on the source furnace is heated (heating rate 8℃ / min) to 975℃; during the heating process, the current and voltage values of the Ga source tip area and base area are observed by TDK, and the power ratio of the Ga source tip area and base area is kept at 9 to 9.2;
[0133] Then, open the switches of Ga source and As source at the same time, open the valve position of As source to 200mil, maintain the degassing time for 25min, and then close the switches of Ga source and As source at the same time, maintain the time for 5min, and complete the third step of degassing; repeat steps 1-5) for 3 times;
[0134] 1-6) Cool down the tip area on the source furnace (cooling rate 3℃ / min) to 1120℃, and cool down the base area on the source furnace (cooling rate 5℃ / min) to 860℃; turn on the Ga source and As source switches at the same time, and open the As source valve position to 150mil, and maintain the degassing time for 35min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0135] 1-7) Cool down the tip area on the source furnace (cooling rate 3℃ / min) to 900℃, and cool down the base area on the source furnace (cooling rate 5℃ / min) to 680℃; turn on the Ga source and As source switches at the same time, and open the As source valve position to 100mil, and maintain the degassing time for 25min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil;
[0136] 1-8) Cool the tip area on the source furnace (cooling rate 3°C / min) to 600°C, and cool the base area on the source furnace (cooling rate 5°C / min) to 500°C to complete the degassing of the Ga source;
[0137] 2) Growth of GaAs epitaxial layer:
[0138] 2-1) Deoxidizing the GaAs substrate, including:
[0139] 2-1-1) Place a 4-inch GaAs non-doped substrate on a molybdenum tray, move it to the injection chamber and the buffer chamber in sequence, and perform preliminary low-temperature degassing in the injection chamber and the buffer chamber; the degassing temperature in the injection chamber is 200°C and the time is 2h; the degassing temperature in the buffer chamber is 300°C and the time is 30min;
[0140] 2-1-2) The GaAs substrate processed in step 2-1-1) is transferred to the growth chamber of the epitaxial equipment, and the vacuum environment in the chamber is 5×10 -10 Torr, rotate the GaAs substrate and heat it up to 300°C (heating rate 15°C / min); then, turn on the As source switch and set the valve position to 30mil;
[0141] 2-1-3) heating the GaAs substrate treated in step 2-1-2) to 400°C (heating rate 15°C / min), and then raising the valve position to 50mil;
[0142] 2-1-4) heating the GaAs substrate treated in step 2-1-3) to 550°C (heating rate 10°C / min), and then raising the valve position to 70mil;
[0143] 2-1-5) Heat the GaAs substrate treated in step 2-1-4) to 600°C (heating rate 5°C / min), then increase the valve position to 100 mil, and complete the deoxidation of the GaAs substrate at 610°C.
[0144] 2-2) After the deoxidation of the GaAs substrate is completed, the Ga and As source furnace switches are turned on at the same time, the growth rate is 1 ML / s, and a GaAs epitaxial layer with a thickness of 500 nm is grown;
[0145] After the growth of the GaAs epitaxial layer is completed, the Ga source furnace switch is turned off and the furnace is cooled to 200°C at 20°C / min in an As atmosphere.
[0146] Verify the defect density change of GaAs epitaxial layer before and after degassing:
[0147] Surfscan and electron microscope tests and analysis were performed on the GaAs epitaxial layer grown before and after gallium source degassing. The results are as follows: Figure 1 shown. Figure 1 The Surfscan image and defect count image of GaAs material before and after gallium source degassing. Figure 1 It can be seen that before the gallium source is degassed, there are many small defects of size >0.3μm in the grown GaAs epitaxial layer. After two steps of degassing (second step degassing), in the GaAs epitaxial layer, it can be observed that the number of defects of size >2μm is significantly reduced, while the number of defects of size >5μm is not much different. After the third step of degassing, the number of defects of size >5μm in the grown GaAs epitaxial layer is 3, and the number of defects is greatly reduced, indicating that the third step of degassing can effectively inhibit Ga source sputtering and reduce the formation of large-size defects.
[0148] Figure 2 Electron microscope images of GaAs material before and after degassing of gallium source. Figure 2 It can be seen that before degassing of the gallium source, the defect size in the GaAs epitaxial layer is about 7.54μm, while the defect size of the GaAs epitaxial layer after degassing is reduced. After the third step of degassing, the defect size is reduced to 5.43μm.
[0149] It can be seen from the above test results that the number and size of defects in the GaAs epitaxial layer grown after the three-step degassing are significantly reduced compared to before degassing.
[0150] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A novel gallium source degassing method, The following steps are involved: A) Gallium source degassing: A1) placing a silicon wafer on a molybdenum tray and moving it to a sample injection chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sample injection chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.; A2) transferring the silicon wafer treated in step A1) to a growth chamber, and heating the silicon wafer to 450-550° C. under vacuum conditions; The source furnace equipped with Ga source is heated for the first time: the tip area on the source furnace is heated to 680-720°C, and the base area on the source furnace is heated to 480-520°C; and the heating rate of the tip area is greater than the heating rate of the base area; after keeping warm for a period of time, the source furnace equipped with Ga source is heated for the second time: the tip area on the source furnace is heated to 880-920°C, and the base area on the source furnace is heated to 660-700°C; A3) Turn on the Ga source and As source switches at the same time, open the As source valve position to 100mil, and maintain the degassing time for 40 to 50 minutes. Then, turn off the Ga source and As source switches at the same time, set the As source valve position to 0 to 5mil, and maintain the time for 4 to 6 minutes to complete the first step of degassing; A4) The source furnace equipped with Ga source is heated for the third time: the tip area on the source furnace is heated to 1100-1140°C, and the base area on the source furnace is heated to 840-880°C; then, the switches of Ga source and As source are turned on at the same time, the valve position of As source is opened to 150mil, and the degassing time is maintained for 30-40min, and then the switches of Ga source and As source are turned off at the same time, the valve position of As source is set to 0-5mil, and the time is maintained for 4-6min, and the second step of degassing is completed; A5) The source furnace equipped with Ga source is heated for the fourth time: the tip area on the source furnace is heated to 1220-1260°C, and the base area on the source furnace is heated to 955-995°C; then, the Ga source and As source switches are turned on at the same time, the As source valve position is opened to 200mil, and the degassing time is maintained for 20-30min, and then the Ga source and As source switches are turned off at the same time, and the time is maintained for 4-6min, completing the third step of degassing; A6) Cool the tip area on the source furnace to 1100-1140°C, and cool the base area on the source furnace to 840-880°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 150mil, and maintain the degassing time for 30-40min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil; A7) Cool the tip area on the source furnace to 880-920°C, and cool the base area on the source furnace to 660-700°C; turn on the Ga source and As source switches at the same time, and open the As source valve position to 100mil, and maintain the degassing time for 20-30min. After completion, turn off the Ga source and As source switches at the same time, and set the As source valve position to 0mil; A8) Cooling the tip area on the source furnace to 580-620°C, and cooling the base area on the source furnace to 480-520°C, to complete the degassing of the Ga source; B) Growth of GaAs epitaxial layer: After the GaAs substrate is deoxidized, the Ga and As source furnace switches are turned on at the same time to grow a GaAs epitaxial layer.
2. The method according to claim 1, It is characterized in that In step A1), the degassing time in the injection chamber is 1.5 to 2.5 hours, and the degassing time in the buffer chamber is 25 to 35 minutes.
3. The method according to claim 1, It is characterized in that In step A2), the vacuum condition is 3×10 -10 ~7×10 - 10 Torr; The silicon wafer temperature rise rate is 10-20°C / min.
4. The method according to claim 1, It is characterized in that In step A2), during the first heating, the heating rate of the tip region and the base region is 10-18°C / min; The insulation time is 8 to 12 minutes; In the second heating, the heating rate of the tip and base regions is 6-12°C / min; During the first heating process and the second heating process, the power ratio between the tip region and the base region of the Ga source is 9 to 9.
2.
5. The method according to claim 1, It is characterized in that In step A4), during the third heating, the heating rate of the tip region and the base region is 10-18°C / min; During the third heating process, the power ratio between the tip region and the base region of the Ga source was 9 to 9.
2.
6. The method according to claim 1, It is characterized in that In step A5), during the fourth heating, the heating rate of the tip region and the base region is 6-12°C / min; During the fourth heating process, the power ratio between the tip region and the base region of the Ga source was 9 to 9.
2.
7. The method according to claim 1, It is characterized in that In step A6), the tip region and the base region are cooled at a rate of 3 to 5°C / min; In step A7), the temperature of the tip region and the base region is reduced at a rate of 3 to 5°C / min; In step A8), the temperature of the tip region and the base region is reduced at a rate of 3-5°C / min.
8. The method according to claim 1, It is characterized in that In step B), the GaAs substrate is deoxidized, comprising: B1) placing a GaAs non-doped substrate on a molybdenum tray, and moving it to a sampling chamber and a buffer chamber in sequence for degassing; the degassing temperature of the sampling chamber is 150-200° C., and the degassing temperature of the buffer chamber is 300-350° C.; B2) transferring the GaAs substrate processed in step B1) to a growth chamber, heating the GaAs substrate to 250-350° C. under vacuum conditions; then, turning on the As source switch, and setting the valve position to 30 mil; B3) heating the GaAs substrate processed in step B2) to 350-450° C., and then raising the valve position to 50 mil; B4) heating the GaAs substrate treated in step B3) to 500-570° C., and then raising the valve position to 70 mil; B5) heating the GaAs substrate treated in step B4) to 580-630°C, raising the valve position to 100-180 mil, and completing the deoxidation of the GaAs substrate at 600-620°C.
9. The method according to claim 8, It is characterized in that In step B1), the degassing time in the injection chamber is 1.5 to 2.5 hours, and the degassing time in the buffer chamber is 25 to 35 minutes; In step B2), the vacuum condition is 3×10 -10 ~7×10 -10 Torr; The heating rate of GaAs substrate is 10-20℃ / min; Step B2) The temperature of the treated GaAs substrate is raised at a rate of 10-20° C. / min; Step B3) The temperature of the treated GaAs substrate is raised at a rate of 8-12°C / min; The heating rate of the GaAs substrate after step B4) is 3-7°C / min.
10. The method according to claim 1, It is characterized in that In step B), the growth rate of growing the GaAs epitaxial layer is 0.8 to 1.2 ML / s; After the growth of the GaAs epitaxial layer is completed, the method further includes: closing the Ga source furnace switch and cooling down in an As atmosphere; the temperature after cooling down is 130-170°C.