Monocrystal III-group oxide nano-alloy material and preparation and application thereof

Through chemical vapor deposition technology under multi-stage growth treatment, the metal layer and nitride film substrate are used to solve the problem of uncontrollable growth of Group III oxide nano alloy materials in the prior art, and the high-quality single-crystal nanomaterials are achieved. Preparation and application of high-performance electronic devices.

CN119020864APending Publication Date: 2024-11-26FUDAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310585708.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

It is difficult to prepare high-quality controlled-grown single-crystal Group III oxide nano alloy materials in the prior art. It is mainly because the metal catalyst is amorphous at high temperatures and cannot provide a specific lattice structure, resulting in the crystal phase of the nanomaterial being uncontrollable.

Method used

Using chemical vapor deposition technology, multi-stage growth treatment under specific atmosphere conditions, including annealing, growth and structural shaping, a heterostructure substrate composed of metal layer and nitride film, to adjust carrier gas flow, cavity pressure and oxygen Content, control the growth temperature by gradually or rapidly cooling to ensure high-quality growth of the material.

Benefits of technology

It realizes a high-quality single-crystal Group III oxide nano alloy material that can be controlled, simplifies equipment requirements and operating steps, and can be used to prepare electronic devices with high electron mobility and high gas-sensitive characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020864A_ABST
    Figure CN119020864A_ABST
Patent Text Reader

Abstract

The invention relates to a single-crystal III-group oxide nano alloy material and preparation and application thereof, and the process specifically comprises the following steps: placing a substrate in chemical vapor deposition equipment, and carrying out annealing treatment for 15-40 minutes under a first growth condition with the growth temperature of 50-700 DEG C; and then, growing for 30 to 240 minutes under a second growth condition at the growth temperature of 800 to 1400 DEG C, so as to obtain the nano material, and finally, carrying out structural shaping under a third growth condition to obtain a target product, namely the single crystal III-group oxide nano-alloy material. Compared with the prior art, the method can be used for preparing high-quality (-201) and (010) crystalline phase single crystal III-group oxide alloy nano materials, and can be applied to preparation of transistors and transparent electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor material preparation, and relates to a single crystal III group oxide nano alloy material and its preparation and application. Background Art

[0002] As a new type of ultra-wide bandgap semiconductor material system, group III oxides have material properties such as adjustable band gap of 3.5eV to 8.8eV, high Baliga figure of merit, high thermal / chemical stability, high visible light transmittance, room-temperature excitons, and high-density two-dimensional electron gas. Their potential applications in ultraviolet transparent electrodes, optoelectronic and electronic devices, memory, and gas sensors have aroused strong research interest in recent years [Y.Liu et al., J.Mater.Chem.A, 2014, 2, 9919-9943; H.Peelaers et al., Physi.Rev.B, 2015, 92, 085206; Z.Galazka, Semicond.Sci.Tech., 2018, 33, 113001; SJPearton et al., Appl.Phys.Rev., 2018, 5, 011301; HCZhai et al., Ceram. Int., 2022, 48, 24213-24233.].

[0003] Nanomaterial growth has special properties such as large surface area, quantum size confinement effect, quantum tunneling effect, etc. In recent years, many research works have begun to focus on the research of III-group oxide nanomaterials and new devices. The methods currently used to prepare III-group oxide nanomaterials include thermal evaporation, chemical vapor deposition, arc discharge, pulsed laser deposition, chemical reaction, magnetron sputtering, etc. [I. López et al., J. Phys. Chem. C, 2012, 116, 3935; HJ Chun et al., Appl. Phys. Lett., 2004, 85, 461; ZY Zhou et al., Nano Res., 2018, 11, 5935; B. Jin et al., Appl. Phys. Lett., 2014, 104, 103510; SJ Zelewski et al., ACS Appl. Mater. Interfaces, 2019, 11, 19260.]. The above growth methods usually use metals such as gold, silver, and platinum as catalysts to grow nanomaterials. Since metal materials are usually amorphous and flexible droplets under high temperature conditions, they cannot provide a specific lattice structure for the growth of materials, making the grown nanomaterials uncontrollable in crystal phase and different in structure; and there are huge miscibility gaps in ternary and quaternary alloys of group III oxides, making it difficult to prepare high-quality single-crystal group III oxide alloy nanomaterials; therefore, it is urgent to design and provide a method for controllably growing single-crystal group III oxide alloy nanomaterials. Summary of the invention

[0004] The purpose of the present invention is to provide a single crystal III group oxide nano alloy material and its preparation and application, so as to achieve controllable high-quality production and preparation.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] One of the technical solutions of the present invention provides a method for preparing a single crystal III group oxide nano alloy material, characterized in that the process is specifically as follows:

[0007] The substrate is placed in a chemical vapor deposition device, the atmosphere of the device is adjusted, and an annealing treatment is first performed for 15 to 40 minutes under a first growth condition of a growth temperature of 50 to 700° C.;

[0008] Next, the nanomaterial is grown under a second growth condition at a growth temperature of 800 to 1400° C. for 30 to 240 minutes to obtain the nanomaterial;

[0009] Finally, the structure is finalized under the third growth condition to obtain the target product, a single crystal III group oxide nano alloy material.

[0010] Furthermore, the substrate is a metal layer / nitride film heterostructure substrate composed of a metal layer and a nitride film.

[0011] Furthermore, the thickness of the metal layer is 1-20 nm, and the material thereof is any one of indium, gallium, platinum, gold, silver, palladium, and iron.

[0012] Furthermore, the material of the nitride film is any one of indium nitride, indium gallium nitride, aluminum gallium nitride, and aluminum indium gallium nitride.

[0013] Furthermore, the atmosphere condition specifically includes introducing a carrier gas and adjusting the cavity pressure to reach the first growth condition, and the carrier gas is any one of nitrogen, argon, hydrogen or other inert gases or a mixture of several of them.

[0014] Furthermore, the first growth conditions are as follows: carrier gas flow rate 50-400 sccm, chamber pressure 100-770 Torr, chamber oxygen content 1.0×10 -12 ~5.0×10 -6 mol / L.

[0015] Furthermore, the second growth conditions are: carrier gas flow rate 50-400 sccm, chamber pressure 10-770 Torr, chamber oxygen content 1.0×10 -12 ~5.0×10 -6 mol / L.

[0016] Furthermore, the third growth condition is: carrier gas flow rate 50-400 sccm, chamber pressure 700-770 Torr. During the structural shaping process, the growth temperature is cooled to room temperature. Optionally, the cooling method can be gradual cooling or rapid cooling.

[0017] Furthermore, in the second growth condition, in order to ensure that the material can continue to grow, raw materials for depositing the final product can also be introduced. For example, trimethylgallium or triethylgallium can be introduced as an additional gallium source with a flow rate of 1 to 30 sccm; trimethylindium can be introduced as an additional indium source with a flow rate of 1 to 30 sccm; trimethylaluminum or triethylaluminum can be introduced as an additional aluminum source with a flow rate of 1 to 30 sccm.

[0018] Furthermore, the molecular formula of the prepared single crystal III group oxide alloy nanomaterial is (In x Ga 1-x )2O3、(Al x Ga 1-x )2O3 or (Al x In y Ga 1-x-y )2O3.

[0019] The second technical solution of the present invention provides a single crystal III group oxide nano alloy material, which is prepared by any of the preparation methods described above, and the nano alloy material is one of a nano wire in (-201) crystal phase, a nano belt in (010) crystal phase or a nano sheet in (010) crystal phase, wherein the diameter of the nano wire is 20 to 500 nm; the side length of the nano belt is 200 to 4000 nm, and the thickness is 20 to 500 nm; the side length of the nano sheet is 4 to 20 μm, and the thickness is 20 to 500 nm.

[0020] A third technical solution of the present invention provides an application of a single crystal III group oxide nano alloy material in transistors and transparent electrodes.

[0021] In the present invention, the first growth condition forms a high-density initial nanostructure on the substrate surface for nucleation growth of group III oxide nano alloy materials; then the second growth condition grows regular nano materials; the second growth stage and the third growth stage are combined to control the final grown nano material morphology to be a line, a strip or a sheet. If any parameter in the growth conditions of the present invention exceeds the range, it is usually difficult to grow nano materials.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] 1) The present invention can controllably prepare high-quality single-crystal III-group oxide alloy nanomaterials.

[0024] 2) The present invention has low requirements on equipment and simple experimental operation steps.

[0025] 3) The single crystal III group oxide alloy nanomaterial prepared by the preparation method of the present invention can be further used to make electronic devices with high electron mobility, high light absorption and high gas sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The scanning electron microscope image (SEM), X-ray diffraction pattern (XRD) and selected area electron diffraction pattern (SAED) of the single crystal (010) InGaO nanoribbon prepared in Example 1 are shown.

[0027] Figure 2 This is the X-ray photoelectron spectrum (XPS) of the single crystal (010) InGaO nanoribbon prepared in Example 1.

[0028] Figure 3 The scanning electron microscope image (SEM) and X-ray diffraction pattern (XRD) of the single crystal (-201) indium gallium oxygen nanowires prepared in Example 2 are shown.

[0029] Figure 4This is the X-ray photoelectron spectrum (XPS) of the single crystal (-201) InGaO nanowires prepared in Example 2.

[0030] Figure 5 The scanning electron microscope image (SEM) and X-ray diffraction pattern (XRD) of the single crystal (-201) aluminum gallium oxygen nanowires prepared in Example 3 are shown.

[0031] Figure 6 This is the X-ray photoelectron spectrum (XPS) of the single crystal (-201) aluminum gallium oxygen nanowire prepared in Example 3.

[0032] Figure 7 This is a scanning electron microscope (SEM) image of the InGaO nanostructure prepared in Comparative Example 1.

[0033] Figure 8 This is a scanning electron microscope (SEM) image of the InGaO nanostructure prepared in Comparative Example 2.

[0034] Fig. 9 This is the time-current curve of (010) β-InGaO nanoribbon. DETAILED DESCRIPTION

[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0036] In the following embodiments,

[0037] If there is no special description of the raw materials or processing technology, it means that they are all conventional commercially available raw materials or conventional processing technologies in the field. For example, the nitride film in the metal layer / nitride film heterostructure substrate can be obtained by any epitaxial equipment, and the metal layer can be obtained by any coating equipment.

[0038] Embodiment 1:

[0039] Preparation of single-crystalline (010) InGaO nanoribbons.

[0040] Step 1: Prepare 5nm platinum metal layer / 2μm aluminum indium gallium nitride film (Al 0.2 Ga 0.6 In 0.2 N) heterostructure substrate;

[0041] Step 2: Place the substrate into the chemical vapor deposition equipment, introduce carrier gas (nitrogen is used in this embodiment), adjust the chamber pressure to 700 Torr, and then, at a growth temperature of 500°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 700 Torr, and a chamber oxygen content of 1.0×10 -9Annealing was performed for 30 min under the condition of mol / L;

[0042] Step 3: The chamber was adjusted to a growth temperature of 1145°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 700 Torr, and a chamber oxygen content of 1.0×10 -11 mol / L for 120 min of growth to prepare nanomaterials;

[0043] Step 4: Rapidly cool down the chamber at a carrier gas flow rate of 100 sccm and a chamber pressure of 700 Torr at a rate of 18° C. / min to finalize the structure and obtain a single crystal (010) indium gallium oxygen nanobelt material. Figure 1 The crystal structure and morphology were characterized. Figure 2 The results of component characterization show that a single-crystal (010) β-InGaO nanoribbon with an indium component of 10% was obtained, and its molecular formula is β-(In 0.1 Ga 0.9 )2O3.

[0044] Embodiment 2:

[0045] Preparation of single crystal (-201) InGaO nanowires

[0046] Step 1: Prepare 5nm platinum metal layer / 2μm aluminum indium gallium nitride film (Al 0.2 Ga 0.6 In 0.2 N) heterostructure substrate;

[0047] Step 2: Place the substrate into the chemical vapor deposition equipment, introduce the carrier gas, adjust the chamber pressure to 700 Torr, and then at a growth temperature of 500°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 700 Torr, and a chamber oxygen content of 1.0×10 - 9 Annealing was performed at mol / L for 30 min;

[0048] Step 3: The chamber was adjusted to a growth temperature of 1140°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 700 Torr, and a chamber oxygen content of 1.0×10 -10 mol / L for 50 min of growth to prepare nanomaterials;

[0049] Step 4: Rapidly cool down the chamber at a carrier gas flow rate of 100 sccm and a chamber pressure of 700 Torr at a rate of 18° C. / min to finalize the structure and obtain a single crystal (-201) indium gallium oxygen nanowire material. Figure 3 The crystal structure and morphology were characterized. Figure 4The component characterization results show that single crystal (-201) β-indium gallium oxygen nanowires with an indium component of 10% were obtained.

[0050] Embodiment 3:

[0051] Preparation of single crystal (-201) aluminum gallium oxide nanowires

[0052] Step 1: Prepare 8nm platinum metal layer / 1.5μm aluminum gallium nitride film (Al 0.7 Ga 0.3 N) heterostructure substrate;

[0053] Step 2: Place the substrate into the chemical vapor deposition equipment, introduce carrier gas, adjust the chamber pressure to 300 Torr, and then, at a growth temperature of 500°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 300 Torr, and a chamber oxygen content of 1.0×10 - 8 Annealing was performed at mol / L for 30 min;

[0054] Step 3: The chamber was adjusted to a growth temperature of 1160°C, a carrier gas flow rate of 100 sccm, a chamber pressure of 300 Torr, and a chamber oxygen content of 1.0×10 -9 mol / L for 240 min of growth to prepare nanomaterials;

[0055] Step 4: Rapidly cool down the chamber at a carrier gas flow rate of 100 sccm and a chamber pressure of 300 Torr at a rate of 18° C. / min to finalize the structure and obtain a single crystal (-201) aluminum gallium oxygen nanowire material. Figure 5 The crystal structure and morphology were characterized. Figure 6 The results of component characterization show that the single crystal (-201) β-aluminum gallium oxide nanowires with an aluminum component of 67% were obtained, and its molecular formula is β-(Al 0.67 Ga 0.33 )2O3.

[0056] By conventional device processes such as extreme ultraviolet lithography, parallel electrodes were plated on the indium gallium oxygen nanoribbons prepared in Example 1 to obtain a deep ultraviolet light detection device, and then the photoelectric performance of the device was tested using a photoelectric testing system. Fig. 9 The obtained time-current curve is shown, and the results show that the indium gallium oxygen nanoribbon optoelectronic device has an extremely fast deep ultraviolet light response speed and light response intensity, and has excellent deep ultraviolet detection capabilities.

[0057] Comparative Example 1:

[0058] Compared with Example 1, most of the aspects are the same, except that the annealing step under the first growth condition is omitted, that is, the growth is directly performed for 150 minutes under the growth condition of the original step 3. Figure 7 The morphological characterization results show that only a small amount of irregular nanostructures can be prepared.

[0059] Comparative Example 2:

[0060] Compared with Example 1, most of them are the same, except that the growth process under the second growth condition is omitted, that is, the annealing process is directly completed under the growth condition of the original step 2 and then the growth condition of the original step 4 is entered. Figure 8 The morphological characterization results showed that high-density nanoparticles could only grow on the sample surface.

[0061] Embodiment 4:

[0062] Compared with Example 1, most of the conditions are the same, except that the growth temperature in step 2 is adjusted to 700°C, the annealing time is 15 min, and the growth conditions are adjusted to: carrier gas flow rate 50 sccm, chamber pressure 770 Torr, chamber oxygen content 5.0×10 - 6 mol / L.

[0063] Embodiment 5:

[0064] Compared with Example 1, most of the conditions are the same, except that the growth temperature in step 3 is adjusted to 800°C, the annealing time is 240 min, and the growth conditions are adjusted to: carrier gas flow rate 50 sccm, chamber pressure 770 Torr, chamber oxygen content 1.0×10 -12 mol / L.

[0065] Embodiment 6:

[0066] Compared with Example 1, most of the conditions are the same, except that the growth temperature in step 3 is adjusted to 1400°C, the annealing time is 30 min, and the growth conditions are adjusted to: carrier gas flow rate 400 sccm, chamber pressure 10 Torr, chamber oxygen content 5.0×10 - 6 mol / L.

[0067] Embodiment 7:

[0068] Compared with Example 1, most of the conditions are the same, except that the growth conditions in step 4 are adjusted to: carrier gas flow rate 50 sccm, chamber pressure 720 Torr.

[0069] Embodiment 8:

[0070] Compared with Example 1, most of the conditions are the same, except that the growth conditions in step 4 are adjusted to: carrier gas flow rate 400 sccm, chamber pressure 770 Torr.

[0071] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a single crystal group III oxide nano alloy material, characterized in that: The specific process is: The substrate is placed in a chemical vapor deposition device, and an annealing treatment is first performed for 15 to 40 minutes under a first growth condition of a growth temperature of 50 to 700° C.; Next, the nanomaterial is grown under a second growth condition at a growth temperature of 800 to 1400° C. for 30 to 240 minutes to obtain the nanomaterial; Finally, the structure is finalized under the third growth condition to obtain the target product, a single crystal III group oxide nano alloy material.

2. The method for preparing a single crystal III group oxide nano alloy material according to claim 1, characterized in that: The substrate is a metal layer / nitride film heterostructure substrate composed of a metal layer and a nitride film.

3. The method for preparing a single crystal III group oxide nano alloy material according to claim 2, characterized in that: The thickness of the metal layer is 1-20 nm, and the material thereof is any one of indium, gallium, platinum, gold, silver, palladium, and iron.

4. The method for preparing a single crystal III group oxide nano alloy material according to claim 2, characterized in that: The material of the nitride film is any one of indium nitride, indium gallium nitride, aluminum gallium nitride, and aluminum indium gallium nitride.

5. The method for preparing a single crystal III group oxide nano alloy material according to claim 1, characterized in that: A carrier gas is also introduced into the chemical vapor deposition equipment to adjust the inside of the chemical vapor deposition equipment to achieve the first growth condition, the second growth condition and the third growth condition respectively. The carrier gas is any one or a mixture of nitrogen, argon, hydrogen or other inert gases.

6. The method for preparing a single crystal III group oxide nano alloy material according to claim 1, characterized in that: The first growth conditions are as follows: carrier gas flow rate 50-400 sccm, chamber pressure 100-770 Torr, chamber oxygen content 1.0×10 -12 ~5.0×10 -6 mol / L.

7. The method for preparing a single crystal III group oxide nano alloy material according to claim 1, characterized in that: The second growth conditions are: carrier gas flow rate 50-400 sccm, chamber pressure 10-770 Torr, chamber oxygen content 1.0×10 -12 ~5.0×10 -6 mol / L.

8. The method for preparing a single crystal III group oxide nano alloy material according to claim 1, characterized in that: The third growth condition is: carrier gas flow rate 50-400 sccm, chamber pressure 700-770 Torr.

9. A single crystal III group oxide nano alloy material, prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The nano alloy material is one of a nano wire in (-201) crystal phase, a nano belt in (010) crystal phase or a nano sheet in (010) crystal phase, wherein the diameter of the nano wire is 20 to 500 nm; the side length of the nano belt is 200 to 4000 nm, and the thickness is 20 to 500 nm; the side length of the nano sheet is 4 to 20 μm, and the thickness is 20 to 500 nm.

10. Application of the single crystal III group oxide nano alloy material as claimed in claim 9 in transistors and transparent electrodes.