Nanofiber material as well as preparation method and application thereof
By adding a viscous polymer during the spray drying process and combining it with electro-spray drying and post-treatment technology, the problem of traditional spray drying methods being unable to prepare fiber materials with good continuity and stability has been solved, and the industrial production of high-quality nanofiber materials has been realized.
Patent Information
- Application Number
- CN202310601454.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional spray drying methods are difficult to use to prepare fiber materials with good continuity and stability, and cannot meet the needs of large-scale industrial production.
A viscous polymer is added during the spray drying process to prepare nanofiber materials via electro-spray drying. The viscous polymer forms fibrous products during spraying, and post-treatment methods such as solvent extraction, carbonization, impregnation, and calcination are combined to improve the performance of the fiber materials.
High-quality, continuous, and stable nanofiber materials were prepared, exhibiting excellent continuity and stability, and are suitable for industrial production in multiple fields, especially showing significant effects in nanofiber materials.
Smart Images

Figure HDA0004256038920000011 
Figure HDA0004256038920000012 
Figure HDA0004256038920000013
Abstract
Description
Technical Field
[0001] The present application relates to a nanofiber material and a preparation method and application thereof, belonging to the technical field of nanomaterial preparation. Background Art
[0002] Nanofiber materials have been widely used in many fields, including filtration, separation, medical treatment, electronics, energy, environment, etc. There are many traditional methods for preparing nanofibers, such as electrospinning, solution adsorption, phase separation, etc. Although these methods can produce nanofibers with small sizes, the continuity and stability of the fibers are poor, making them difficult to apply to large-scale industrial production. Spray drying is an emerging method for preparing nanomaterials. This method sprays the solution into fine droplets and instantly dries them into powder materials in a hot air flow. However, the products prepared by spray drying are currently mainly in powder form. Summary of the invention
[0003] In order to solve the problem that the spray drying method in the prior art cannot prepare fiber materials, the present application provides a method for preparing fiber materials by adding a viscous polymer during the spray drying process. The viscous polymer solution has high viscosity and can obtain fine droplets with a certain viscosity during the spraying process, so that high-quality, continuous and stable fiber materials can be prepared during the hot air flow drying process.
[0004] Specifically, the present invention adds a viscous polymer to the solution used in the conventional spray drying method, and forms the viscous polymer into a fibrous product through instant drying. The fiber material prepared by adding the viscous polymer has excellent continuity and stability, can meet the needs of fiber materials in multiple fields, and is particularly effective in preparing nanofibers.
[0005] According to one aspect of the present application, a method for preparing a nanofiber material is provided, comprising the following steps:
[0006] 1) dissolving a viscous polymer in a solvent to form a precursor solution;
[0007] 2) The precursor solution is sprayed by electrospray drying to obtain the nanofiber material.
[0008] The electrospray drying method is that a viscous polymer solution is sheared into tiny droplets under the action of an electric field, and a solid product with a nanofiber structure is prepared through a drying process. In this application, fibers of different components can be obtained according to different polymer solution components.
[0009] Optionally, the viscous high molecular polymer is selected from at least one of polyacrylonitrile, polymethyl methacrylate, polyvinyl pyrrolidone and polystyrene.
[0010] Optionally, the solvent is selected from at least one of water, alcohol solution, acetone, N,N-dimethylformamide, dimethyl sulfoxide, and tetrahydrofuran.
[0011] Optionally, the alcohol solution is selected from methanol and / or ethanol.
[0012] Optionally, the mass fraction of the viscous high molecular polymer in the precursor solution is 0.1-50%.
[0013] Optionally, the mass fraction of the viscous high molecular polymer in the precursor solution is any value of 0.1%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, or a range between two values.
[0014] In the present application, when the viscous high molecular polymer is polyacrylonitrile, the solvent is selected from N,N-dimethylformamide;
[0015] When the viscous high molecular polymer is polymethyl methacrylate, the solvent is selected from at least one of N,N-dimethylformamide, tetrahydrofuran, acetone, and dimethyl sulfoxide;
[0016] When the viscous high molecular polymer is polyvinyl pyrrolidone, the solvent is selected from at least one of an alcohol solution, water, and N,N-dimethylformamide;
[0017] When the viscous high molecular polymer is polystyrene, the solvent is selected from at least one of N,N-dimethylformamide, tetrahydrofuran and acetone.
[0018] Optionally, the conditions of the electrospray drying method are:
[0019] The voltage of the electric field is 1 to 30 kV;
[0020] The inlet temperature of the electrospray drying device is 10-300°C, and the outlet temperature is 50-500°C.
[0021] Optionally, the ambient temperature of electrospray is 60-300°C.
[0022] Optionally, the injection speed of the precursor solution is 0.1 to 1000 mL / min.
[0023] Optionally, the precursor solution further contains an additive, which is a metal salt or a metal nanomaterial.
[0024] The metal element of the metal salt is selected from noble metal elements and / or non-noble metal elements.
[0025] Optionally, the precious metal element is selected from at least one of platinum, gold and silver.
[0026] Optionally, the non-precious metal element is selected from at least one of iron, cobalt, nickel, zinc and manganese.
[0027] Optionally, the metal salt is selected from at least one of nitrates, carbonates and chlorates corresponding to the metal element.
[0028] Optionally, the mass ratio of the metal salt to the viscous high molecular polymer is 1:0.5-5.
[0029] In this application, the specific preparation method for preparing nanofiber materials when the precursor solution contains metal salts is:
[0030] (a) dissolving a viscous high molecular polymer in a solvent to prepare a polymer solution with a certain viscosity, and adding different metal salts or metal nanomaterials according to the specific use of the fiber material to obtain a uniform solution;
[0031] (b) Using a spray drying device, the solution is sprayed into mist particles; the mist particles are dried in an air flow to form a fibrous material.
[0032] The metal nanomaterial is a nanoparticle powder containing metal, alloy, metal oxide, etc., which is prepared in advance and has a specific nanostructure and size;
[0033] Specific metal nanomaterials may be metals, alloys, metal oxides, etc. that can be composited in graphene, MXene, carbon nanotubes, and organic metal frameworks.
[0034] Optionally, the method for preparing the nanofiber material further comprises post-processing:
[0035] The post-treatment includes at least one of a solvent method, a carbonization method, an impregnation method, and a calcination method.
[0036] Optionally, the solvent method is: immersing the nanofiber material in solvent I to dissolve;
[0037] The solvent I is a solvent that does not dissolve at least one of the viscous high molecular polymers;
[0038] When the post-treatment method is a solvent method, the viscous polymer used in preparing the nanofiber material needs to be selected from at least two of polyacrylonitrile, polymethyl methacrylate, polyvinyl pyrrolidone, and polystyrene. In the process of dissolving and making holes by the solvent method, the solvent is selected to dissolve one of the viscous polymers but not the other, as shown in Example 3.
[0039] Optionally, the carbonization method is: carbonizing the nanofiber material under a flowing atmosphere;
[0040] The carbonization temperature is 100-2000°C.
[0041] Optionally, the impregnation method is: impregnating the nanofiber material in a metal salt solution and freeze-drying;
[0042] The immersion temperature is 20 to 50° C., and the immersion time is 8 to 12 hours;
[0043] The freeze drying temperature is -20 to -16°C, and the freeze drying time is 25 to 40 hours;
[0044] The concentration of the metal salt solution is 0.01-1 g / mL.
[0045] The metal salt solution selected during the impregnation process is a salt solution containing precious metal elements and / or non-precious metal elements;
[0046] The precious metal element is selected from at least one of platinum, gold and silver; the non-precious metal element is selected from at least one of iron, cobalt, nickel, zinc and manganese.
[0047] The salt solution is selected from at least one of nitrate, carbonate and chlorate.
[0048] Optionally, the calcination method is: calcining the nanofiber material in an oxygen-containing atmosphere;
[0049] The calcination temperature is 600-800° C., and the calcination time is 3-7 hours.
[0050] In the present application, when the selected post-treatment method is the calcination method, the precursor solution needs to contain additives.
[0051] According to another aspect of the present application, a nanofiber material is provided, wherein the diameter of the nanofiber material is 10 nm to 5 μm.
[0052] Optionally, the nanofiber material has a pore structure inside.
[0053] Optionally, the surface and interior of the nanofiber material have a porous structure.
[0054] Optionally, the nanofiber material contains metal oxide particles inside.
[0055] Optionally, metal oxide particles are loaded on the surface of the nanofiber material.
[0056] According to another aspect of the present application, there is provided an application of a nanofiber material in nanomaterial preparation, sensors, catalysts, liquid phase hydrogenation, photocatalysis, and drug sustained release.
[0057] The beneficial effects of this application include:
[0058] 1) The preparation method provided in this application can obtain high-quality, well-controllable nanofiber materials by adjusting different polymer types and concentration conditions; the preparation process is simple, low-cost, does not require complex equipment such as high temperature and high pressure, and can realize industrial production.
[0059] 2) The preparation method provided in this application prepares a fibrous material having excellent properties such as large specific surface area, high porosity, and strong adsorption capacity.
[0060] 3) The nanofiber material provided in this application has a relatively small diameter. The nanofiber material prepared in this application is generally between tens of nanometers and several microns, so it has good mechanical properties and softness, and can be used to prepare high-performance composite materials, nanosensors, electrode materials, etc.
[0061] 4) The preparation method provided in the present application can prepare fibrous materials with different functions according to different combinations of polymer materials, and has high application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 Characterization diagram of the nanofiber material prepared in Example 1 of the present application, wherein Figure a is an electron photograph of the fiber material, Figure b is a scanning electron microscope image of the fiber material, and Figure c is a transmission electron microscope image of the fiber material;
[0063] Figure 2 Characterization diagrams of the nanofiber materials prepared in Examples 2 and 3 of the present application, wherein Figure a is an electronic photograph of the fiber material prepared in Example 2, Figure b is a scanning electron microscope image of the fiber material prepared in Example 3, and Figure c is a transmission electron microscope image of the fiber material prepared in Example 3;
[0064] Figure 3 Characterization diagram of the porous carbon fiber material prepared in Example 4 of the present application; wherein Figure a is a transmission electron microscope image of the porous carbon fiber material, Figure b is a scanning electron microscope image of the surface of the porous carbon fiber material, and Figure c is a scanning electron microscope image of the cross section of the porous carbon fiber material;
[0065] Figure 4 These are characterization diagrams of the fiber materials of Examples 5 and 6 of the present application, wherein Figure a is a transmission electron microscope image of the fiber material prepared in Example 5 at a magnification of 200nm, Figure b is a scanning electron microscope image of the fiber material prepared in Example 5 at a magnification of 1μm, Figure c is a transmission electron microscope image of the fiber material prepared in Example 6 at a magnification of 200nm, and Figure d is an X-ray diffraction analysis spectrum of the fiber materials in Examples 5 and 6. DETAILED DESCRIPTION
[0066] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0067] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0068] The analysis method in the examples of this application is as follows:
[0069] Scanning electron microscopy (SEM) was performed using Quanta 200F from FEI, USA; transmission electron microscopy (TEM) was performed using HT7700 from Hitachi, Japan; and X-ray diffraction analysis was performed using D / Max 2500 / PC from Rigaku Corporation, Japan.
[0070] As an embodiment, the method for preparing the fiber material by spray drying comprises the following steps:
[0071] (1) After dissolving polymers of different viscosities, metal salts or metal nanomaterials are added to obtain a uniform solution;
[0072] (2) The solution is atomized using a spray drying device and dried to obtain a fibrous material.
[0073] Example 1
[0074] Polymethyl methacrylate particles (1 g) and polyvinyl pyrrolidone (1 g) were dissolved in 10 ml of N,N-dimethylformamide and stirred at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method was 20 kV, the inlet temperature in the spray dryer was 175 degrees Celsius, the outlet temperature was 115 degrees Celsius, the solution injection speed was 5 ml / min, and the drying gas flow rate was 5 liters / min to obtain a fiber material.
[0075] Figure 1 The electronic photography image and the scanning electron microscope image of the fiber material in this embodiment 1 show that the material is a thin film-like integral material formed by fiber accumulation.
[0076] Example 2
[0077] Ferrous chloride (2 g) and polyacrylonitrile (1 g) were dissolved in 10 ml of N,N-dimethylformamide and stirred at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method was 20 kV, the inlet temperature in the spray dryer was 175 degrees Celsius, the outlet temperature was 115 degrees Celsius, the solution injection speed was 8 ml / min, and the drying gas flow rate was 5 liters / min to obtain a fiber material.
[0078] Figure 2 a is the fiber material obtained by spray drying in Example 2, and the fibers are piled up into a whole material. Due to the presence of ferrous chloride, the color of the fiber is light green.
[0079] Example 3
[0080] Polymethyl methacrylate particles (1 gram) and polyvinyl pyrrolidone (1 gram) were dissolved in 10 ml of N,N-dimethylformamide and stirred at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method was 20 kV, the inlet temperature in the spray dryer was 175 degrees Celsius, the outlet temperature was 115 degrees Celsius, the solution injection rate was 5 ml / min, and the drying gas flow rate was 5 liters / min. After obtaining the fiber material, it was soaked in anhydrous ethanol solution for 12 hours and transferred to a forced air drying oven at 60 degrees Celsius for 24 hours.
[0081] Figure 2 b is a scanning electron microscope image of the fiber prepared under the conditions of Example 3, Figure 2 c is the transmission electron microscope image of the material. Since polyvinyl pyrrolidone can be dissolved in anhydrous ethanol, while polymethyl methacrylate cannot be dissolved in ethanol, it can be seen from the scanning electron microscope image that the fiber surface has wrinkles. Through transmission electron microscopy, it can be observed that the fiber has channels inside.
[0082] Example 4
[0083] Polyacrylonitrile (0.5 g) and polymethyl methacrylate (1.5 g) were dissolved in 10 ml of N,N-dimethylformamide and stirred at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method was 20 kV, the inlet temperature in the spray dryer was 175 degrees Celsius, the outlet temperature was 115 degrees Celsius, the solution injection speed was 8 ml / min, and the drying gas flow rate was 5 liters / min to obtain a fiber material. The obtained fiber material was heated from room temperature to 500 degrees Celsius at a rate of 5 degrees / min in a nitrogen atmosphere and maintained for 3 hours to obtain a fiber material with a porous structure.
[0084] Figure 3 a is a transmission electron microscope image of the porous carbon fiber material prepared under the conditions of Example 4, Figure 3 3b and 3c are scanning electron microscope images of the porous carbon fiber material prepared under the conditions of this Example 4. The images show the porous structure on the fiber surface and inside.
[0085] Example 5
[0086] Polyacrylonitrile (1 g) was dissolved in 10 ml of N,N-dimethylformamide and stirred at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method was 20 kV, the inlet temperature in the spray dryer was 175 degrees Celsius, the outlet temperature was 115 degrees Celsius, the solution injection rate was 8 ml / min, and the drying gas flow rate was 5 liters / min to obtain a fiber material.
[0087] Ferric nitrate (2 g) was dissolved in 50 ml of deionized water, and the polyacrylonitrile fibers obtained by spray drying were immersed in the ferric nitrate aqueous solution at 35 degrees Celsius for 10 hours. The fibers were taken out of the solution, rinsed with deionized water 5 times, pre-dried at -18 degrees Celsius for 10 hours, and transferred to a freeze dryer for 20 hours.
[0088] The completely dried fibers were heated from room temperature to 700 degrees Celsius at a rate of 5 degrees per minute in a nitrogen atmosphere, maintained for 5 hours, and then naturally cooled to room temperature to obtain a nanocarbon fiber material containing iron oxide particles on the surface.
[0089] Figure 4 4a and 4b are respectively the transmission electron microscopy and scanning electron microscopy images of the fiber material containing iron oxide on the surface prepared under the conditions of Example 5 of the present application. The images show that the metal iron oxide is distributed on the surface of the fiber.
[0090] Figure 4 d is the X-ray diffraction spectrum of the carbon fiber material containing iron oxide, which proves that the iron oxide on the fiber surface is Fe3O4.
[0091] Example 6
[0092] Dissolve ferric nitrate (2 g) and polyacrylonitrile (1 g) in N,N-dimethylformamide and stir at room temperature for 24 hours until uniform; the electric field voltage of the electrospray drying method is 20 kV, the inlet temperature in the spray dryer is 175 degrees Celsius, the outlet temperature is 115 degrees Celsius, the solution injection rate is 8 ml / min, and the drying gas flow rate is 5 liters / min to obtain the fiber material. Raise the temperature to 700°C at 2°C / min in an air atmosphere, bake in an air atmosphere for 2 hours, and finally cool naturally to room temperature to obtain a nano-carbon fiber material containing iron oxide particles.
[0093] Figure 4 c is a transmission electron micrograph of a nano-carbon fiber material containing iron oxide particles prepared under the conditions of Example 6, showing a fiber structure composed of a large amount of iron oxide.
[0094] Figure 4 The X-ray diffraction pattern of the carbon fiber material containing iron oxide in d proves that the particles on the fiber surface are composed of Fe3O4 and Fe2O3.
[0095] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a nanofiber material, characterized in that: The following steps are involved: 1) dissolving a viscous polymer in a solvent to form a precursor solution; 2) The precursor solution is sprayed by electrospray drying to obtain the nanofiber material.
2. The preparation method according to claim 1, characterized in that: The viscous high molecular polymer is selected from at least one of polyacrylonitrile, polymethyl methacrylate, polyvinyl pyrrolidone and polystyrene; Preferably, the mass fraction of the viscous high molecular polymer in the precursor solution is 0.1-50%.
3. The preparation method according to claim 1, characterized in that: The solvent is selected from at least one of water, alcohol solution, acetone, N,N-dimethylformamide, dimethyl sulfoxide, and tetrahydrofuran; Preferably, the alcohol solution is selected from methanol and / or ethanol.
4. The preparation method according to claim 1, characterized in that: The conditions of the electrospray drying method are: The voltage of the electric field is 1 to 30 kV; The inlet temperature of the electrospray drying device is 10-300°C, and the outlet temperature is 50-500°C; The ambient temperature of electrospray is 60-300°C; Preferably, the injection speed of the precursor solution is 0.1-1000 mL / min.
5. The preparation method according to claim 1, characterized in that: The precursor solution also contains an additive, which is a metal salt or a metal nanomaterial. The metal element of the metal salt is selected from noble metal elements and / or non-noble metal elements; Preferably, the mass ratio of the metal salt to the viscous high molecular polymer is 1:0.5-5.
6. The preparation method according to claim 5, characterized in that: The noble metal element is selected from at least one of platinum, gold and silver; Preferably, the non-precious metal element is selected from at least one of iron, cobalt, nickel, zinc and manganese; Preferably, the metal salt is selected from at least one of nitrates, carbonates and chlorates corresponding to the metal element.
7. The preparation method according to claim 1, characterized in that: It also includes post-processing of nanofiber materials; The post-treatment includes at least one of a solvent method, a carbonization method, an impregnation method, and a calcination method.
8. A nanofiber material obtained according to the preparation method according to any one of claims 1 to 7, characterized in that: The diameter of the nanofiber material is 10 nm to 5 μm.
9. The nanofiber material according to claim 8, characterized in that The nanofiber material has a pore structure inside; Preferably, the surface and interior of the nanofiber material have a porous structure; Preferably, the nanofiber material contains metal oxide particles inside; Preferably, the surface of the nanofiber material is loaded with metal oxide particles.
10. Use of the nanofiber material according to claim 8 or claim 9 in nanomaterial preparation, sensors, catalysts, liquid phase hydrogenation, photocatalysis, and drug sustained release.