Preparation method and application of high-elastic polyester second-dry super-breathable fabric

By mixing polyester fiber with hydrophilic polymer and combining with breathable coatings, an ultra-breathable fabric is formed, which solves the problem of insufficient moisture absorption and sweating performance of traditional fabrics during high-strength exercises, and achieves high elasticity, instant drying and ultra-breathable performance. Improve and enhance the hydrophobic and antibacterial properties of the fabric.

CN119021002APending Publication Date: 2024-11-26JIANGSU DINGXIN PRINTING & DYEING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201162.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional fabrics lack moisture absorption and sweating performance during high-intensity exercise, resulting in the wearer being stuffy and uncomfortable, and lack of high elasticity, instant drying and super breathable fabrics.

Method used

Compound fibers are prepared by mixing polyester fibers with hydrophilic polymers and melt spinning, soaking breathable coatings to form breathable coatings, and super breathable fabrics are obtained after heat treatment. The silica composite acrylate emulsion and eugenol microcapsules are used to enhance hydrophobic, antibacterial and antibacterial and UV resistance.

Benefits of technology

It significantly improves the breathability, dryness and antibacterial properties of the fabric, enhances the hydrophobic properties and UV resistance of the fiber, and is suitable for sportswear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a high-elastic polyester second-dry super-breathable fabric. The preparation method comprises the following steps: S1, mixing polyester fibers with a hydrophilic polymer, and performing melt spinning to obtain composite fibers; s2, the composite fibers are soaked in the breathable coating, a breathable coating is formed on the surfaces of the composite fibers, and the treated composite fibers are obtained; s3, spinning the treated fibers to obtain a composite fabric; s4, the composite fabric is subjected to heat treatment, and the super-breathable fabric is obtained; the hydrophilic polymer comprises any one of polyvinyl alcohol and sodium polyacrylate, and the breathable coating comprises a silicon dioxide composite acrylate emulsion, a dispersing agent and a defoaming agent. The fabric has the effect of improving the air permeability of the fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of fabric preparation, and in particular to a preparation method and application of a highly elastic polyester instant-drying super-breathable fabric. Background Art

[0002] Fabric is the material used to make clothing. As one of the three elements of clothing, fabric can not only interpret the style and characteristics of clothing, but also directly influence the color and shape of clothing.

[0003] As people's health awareness increases, the performance requirements for sports equipment are also increasing. Traditional fabrics have certain limitations in terms of moisture absorption and perspiration and breathability. Especially during high-intensity exercise, sweat cannot evaporate quickly, causing the wearer to feel stuffy and uncomfortable. Therefore, the development of a fabric with high elasticity, fast drying and super breathable properties has become an urgent need in the industry. Summary of the invention

[0004] In order to improve the air permeability of fabrics, the present application provides a preparation method and application of a highly elastic polyester instant-drying super breathable fabric.

[0005] The present application provides a method for preparing a highly elastic polyester second-drying super breathable fabric and its application adopts the following technical solutions: In the first aspect, the present application provides a method for preparing a highly elastic polyester second-drying super breathable fabric, adopting the following technical solutions: S1, mixing polyester fiber with a hydrophilic polymer, and melt spinning to prepare a composite fiber; S2, impregnating the composite fiber into the breathable coating, forming a layer of breathable coating on the surface of the composite fiber, and obtaining a treated composite fiber; S3, weaving the treated fibers to obtain a composite fabric; S4, heat-treating the composite fabric to obtain a super breathable fabric; The hydrophilic polymer includes any one of polyvinyl alcohol and sodium polyacrylate, and the breathable coating includes silicon dioxide composite acrylate emulsion, dispersant and defoamer.

[0006] By adopting the above technical scheme, the composite fiber prepared by blending polyester fiber and hydrophilic polymer has better hydrophilicity and film-forming property, so that it can be better combined with the breathable coating to improve the stability of the obtained breathable coating. The breathable coating prepared by using silica composite acrylate emulsion, dispersant and defoaming agent has good air permeability and comfortable hydrophobicity, reduces the occurrence of water vapor wetting the fiber, and thus can keep the fabric dry.

[0007] Preferably, the silica composite acrylate emulsion comprises an acrylate matrix, a silica composite and dodecafluoroheptyl methacrylate, and the silica composite acrylate emulsion is prepared by the following method: The emulsifier is mixed with water to obtain an emulsifier solution; a part of the acrylate matrix, dodecafluoroheptyl methacrylate and vinyl trimethoxysilane are mixed, added to the emulsifier solution, ultrasonically treated, and then magnetically stirred to obtain a prefabricated emulsion; a silicon dioxide composite, the remaining part of the acrylate matrix, sodium bicarbonate and water are added to the prefabricated emulsion, the temperature is increased after ultrasonic treatment, potassium persulfate is added for reaction, and after the reaction, filtering is performed to obtain a silicon dioxide composite acrylate emulsion.

[0008] By adopting the above technical scheme, an acrylate matrix is ​​used as a polymerization monomer, and a silica complex, dodecafluoroheptyl methacrylate and vinyltrimethoxysilane are added to obtain a silica composite acrylate emulsion. The silica in the emulsion is evenly dispersed and has high stability. Dodecafluoroheptyl methacrylate contains fluorine. In the formed breathable coating, the fluorine- and silicon-containing chain segments will gather on the outer layer of the fabric, greatly reducing the surface tension of the fiber, so that the fabric has good hydrophobic properties, and under the protection of the CF bond, the strength of the composite fiber can be significantly improved.

[0009] Preferably, the acrylate matrix includes any one of butyl acrylate, methyl methacrylate and hydroxyethyl methacrylate, or a mixture of several of them.

[0010] Preferably, the mass ratio of the acrylate matrix, the silica composite and dodecafluoroheptyl methacrylate is 2.65:(0.32-0.36):1.

[0011] By adopting the above technical solution, preferably the mass ratio of the acrylate body, the silica composite and dodecafluoroheptyl methacrylate is within the above range, which can further improve the stability of the prepared silica composite acrylate emulsion.

[0012] Preferably, the silicon dioxide composite comprises silicon dioxide, eugenol and hexadecyltrimethylammonium bromide.

[0013] By adopting the above technical scheme, silicon dioxide and eugenol are compounded to obtain microcapsules, which are added to the coating system to improve the overall antibacterial properties of the coating. After being combined with the composite fiber, the overall antibacterial properties of the fabric are improved. At the same time, the prepared microcapsules can slowly release eugenol, thereby achieving long-lasting antibacterial properties.

[0014] Preferably, the silicon dioxide composite is prepared by the following method: Water and hexadecyltrimethylammonium bromide are mixed to obtain a surfactant solution, and eugenol is added to obtain a mixed solution; tetraethoxysilane, ethanol, and (3-aminopropyl)triethoxysilane are mixed, added to the mixed solution for reaction, and allowed to stand until stratification, centrifuged, washed, and dried to obtain a silicon dioxide composite.

[0015] By adopting the above technical scheme, eugenol is encapsulated with silicone to prepare microcapsules, and eugenol is loaded onto silica, thereby improving the stability of eugenol in the coating system, allowing eugenol to play a role for a long time and further improving the overall antibacterial properties of the coating system, thereby improving the antibacterial properties of breathable fabrics.

[0016] Preferably, the mass ratio of tetraethoxysilane, hexadecyltrimethylammonium bromide and eugenol is (2.1-2.3):0.2:1.

[0017] By adopting the above technical solution, preferably the mass ratio of tetraethoxysilane, hexadecyltrimethylammonium bromide and eugenol is within the above range, which can effectively improve the stability of the prepared silicon dioxide composite.

[0018] Preferably, the breathable coating also includes sunscreen nanoparticles.

[0019] By adopting the above technical solution and adding sunscreen particles, the anti-ultraviolet performance of the composite fiber can be improved, thereby improving the overall anti-ultraviolet performance of the fabric.

[0020] Preferably, in step S2, the soaking treatment time is 30-60 minutes, and the soaking temperature is 25-40° C.; in step S4, the heat treatment temperature is 120-150° C., and the treatment time is 5-10 min.

[0021] By adopting the above technical solution, preferably the immersion time and temperature in step S2 are within the above range, and preferably the heat treatment temperature and time in step S4 are within the above range, the breathable coating can be more stably covered on the surface of the composite fiber, thereby improving the stability of the obtained breathable layer.

[0022] In a second aspect, the present application also provides an application of the above-mentioned high-elastic polyester instant-drying super-breathable fabric in sportswear.

[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. The polyester fiber and the hydrophilic polymer are mixed and melt-spun to obtain composite fibers. The composite fibers have good hydrophilicity and film-forming properties, and can be more stably combined with the breathable coating, thereby further improving the stability of the paint coating. The breathable coating is added with silica composite acrylic emulsion, so that the formed breathable coating has good hydrophobic properties, which reduces the occurrence of sweat adhering to the surface of the fabric, and further improves the dryness of the fabric; 2. The silica composite acrylic emulsion is added with silica composite and dodecafluoroheptyl methacrylate, so that the coating system contains fluorine elements. The fluorine- and silicon-containing segments are aggregated on the outer layer of the fabric, reducing the surface tension of the fiber to further improve the hydrophobic performance of the breathable coating; 3. Microcapsules are prepared by loading eugenol in the silica complex. Eugenol has good antibacterial properties and can effectively improve the overall long-term antibacterial properties of the fabric. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments: Description of raw materials: All raw materials in the examples are commercially available; the emulsifier in the silica composite acrylate emulsion is prepared by a fatty alcohol polyoxyethylene ether and sodium dodecyl sulfate in a mass ratio of 1:1; the dispersant in the breathable coating is a polymer of 2-ethyl-2-(hydroxymethyl)-1,3-propanediol and bis(isocyanatomethyl)benzene (CAS No.: 51852-81-4), and the defoaming agent is BYK011.

[0025] Example 1 Preparation of silica composite: 20 g of deionized water was mixed with 0.91 g of hexadecyltrimethylammonium bromide (CAS No.: 57-09-0), and the solution was stirred for 30 min to obtain a surfactant solution. Subsequently, 4.55 g of eugenol (CAS No.: 97-53-0) was added, and stirring was continued for 30 min to obtain a mixed solution. 9.54 g of tetraethoxysilane, 50 g of ethanol, and 3 g of (3-aminopropyl)triethoxysilane (CAS No.: 919-30-2) were mixed and added to the mixed solution. When the mixed solution became clear, 1 ml of ammonia water was added to promote the reaction. After the reaction was completed, the mixture was allowed to stand until stratification, and then centrifuged. The mixture was washed alternately with anhydrous ethanol and deionized water three times, and then transferred to a vacuum drying oven and dried at 55°C for 12 h to obtain a silica composite.

[0026] Preparation of silica composite acrylate emulsion: 1.84 g of an emulsifier was mixed with 10 g of deionized water to obtain an emulsifier solution; butyl acrylate, methyl methacrylate and hydroxyethyl methacrylate were mixed in a mass ratio of 3:2:0.03 to obtain an acrylate matrix; 16.69 g of the acrylate matrix, 12.59 g of dodecafluoroheptyl methacrylate (CAS No.: 2261-99-6) and 1.34 g of vinyltrimethoxysilane were mixed and added to the emulsifier solution, ultrasonically dispersed for 30 min, and then magnetically stirred for 30 min to obtain Prefabricated emulsion; adding 4.03g of silica composite, 16.69g of acrylate matrix, 0.5g of sodium bicarbonate and 30g of deionized water to the prefabricated emulsion, ultrasonically dispersing for 30min, then heating to 50°C, and then heating to 80°C after 20min, adding 0.11g of potassium persulfate, keeping warm for 30min, and then adding 0.22g of potassium persulfate within 2h, keeping warm for reaction, cooling the system to 30°C after the reaction, and filtering with a 200-mesh sieve to obtain a silica composite acrylate emulsion.

[0027] Preparation of breathable coating: 15 g of silica composite acrylate emulsion, 80 g of polyurethane, 4 g of sunscreen nanoparticles, 2 g of dispersant and 2 g of defoamer were mixed and stirred for 10 minutes to obtain a breathable coating.

[0028] Among them, the sunscreen nanoparticles are nano titanium dioxide.

[0029] Prepare breathable fabrics: S1, mixing polyester fiber and hydrophilic polymer in a mass ratio of 7:1, and melt spinning to prepare composite fiber; S2, completely soaking the prepared composite fiber in the breathable coating for 30 min at a temperature of 40° C., so that the breathable coating is fully combined with the composite fiber, and a layer of breathable coating is formed on the surface of the composite fiber, thereby obtaining the treated composite fiber; S3, weaving the treated fibers to obtain a composite fabric; S4. The composite fabric is heat treated at a temperature of 150° C. for 5 min, so that the components in the composite fabric are more closely bonded to obtain a super breathable fabric.

[0030] Wherein, the hydrophilic polymer is polyvinyl alcohol (CAS No.: 9002-89-5).

[0031] Example 2 Preparation of silica composite: Mix 20 g of deionized water and 0.86 g of hexadecyltrimethylammonium bromide, stir for 30 min to obtain a surfactant solution, then add 4.29 g of eugenol, continue stirring for 30 min to obtain a mixed solution; mix 9.85 g of tetraethoxysilane, 50 g of ethanol, and 3 g of (3-aminopropyl)triethoxysilane, and add to the mixed solution. When the mixed solution becomes clear, add 1 ml of ammonia water to promote the reaction. After the reaction is completed, let it stand until stratification, then centrifuge, wash alternately with anhydrous ethanol and deionized water three times, transfer to a vacuum drying oven, and dry at 55°C for 12 h to obtain a silica composite.

[0032] Preparation of silica composite acrylate emulsion: 1.84 g of emulsifier was mixed with 10 g of deionized water to obtain an emulsifier solution; butyl acrylate, methyl methacrylate and hydroxyethyl methacrylate were mixed in a mass ratio of 3:2:0.03 to obtain an acrylate matrix; 16.52 g of the acrylate matrix, 12.47 g of dodecafluoroheptyl methacrylate and 1.34 g of vinyltrimethoxysilane were mixed and added to the emulsifier solution, ultrasonically dispersed for 30 min, and then magnetically stirred for 30 min to obtain a prefabricated emulsion; 4 .49g of silica composite, 16.52g of acrylate matrix, 0.5g of sodium bicarbonate and 30g of deionized water were added to the prefabricated emulsion, ultrasonically dispersed for 30 minutes, then heated to 50°C, and then continued to heat to 80°C after 20 minutes, added with 0.11g of potassium persulfate, kept warm for 30 minutes, and then added with 0.22g of potassium persulfate within 2 hours, kept warm for reaction, and after the reaction, the system was cooled to 30°C and filtered with a 200-mesh sieve to obtain a silica composite acrylate emulsion.

[0033] Preparation of breathable coating: 19 g of silica composite acrylate emulsion, 86 g of polyurethane, 7 g of sunscreen nanoparticles, 4 g of dispersant and 4 g of defoamer were mixed and stirred for 10 minutes to obtain a breathable coating.

[0034] Among them, the sunscreen nanoparticles are nano titanium dioxide.

[0035] Prepare breathable fabrics: S1, mixing polyester fiber and hydrophilic polymer in a mass ratio of 9:2, and melt spinning to prepare composite fiber; S2, completely soaking the prepared composite fiber in the breathable coating for 60 minutes at a temperature of 25° C., so that the breathable coating is fully combined with the composite fiber, and a layer of breathable coating is formed on the surface of the composite fiber, thereby obtaining the treated composite fiber; S3, weaving the treated fibers to obtain a composite fabric; S4. The composite fabric is heat treated at a temperature of 120° C. for 10 min, so that the components in the composite fabric are more closely bonded to obtain a super breathable fabric.

[0036] Wherein, the hydrophilic polymer is sodium polyacrylate (CAS No.: 9003-04-7).

[0037] Example 3 Preparation of silica composite: Mix 20 g of deionized water and 0.88 g of hexadecyltrimethylammonium bromide, stir for 30 min to obtain a surfactant solution, then add 4.41 g of eugenol, continue stirring for 30 min to obtain a mixed solution; mix 9.71 g of tetraethoxysilane, 50 g of ethanol, and 3 g of (3-aminopropyl)triethoxysilane, and add to the mixed solution. When the mixed solution becomes clear, add 1 ml of ammonia water to promote the reaction. After the reaction is completed, let it stand until stratification, then centrifuge, wash alternately with anhydrous ethanol and deionized water three times, transfer to a vacuum drying oven, and dry at 55°C for 12 h to obtain a silica composite.

[0038] Preparation of silica composite acrylate emulsion: 1.84 g of emulsifier was mixed with 10 g of deionized water to obtain an emulsifier solution; butyl acrylate, methyl methacrylate and hydroxyethyl methacrylate were mixed in a mass ratio of 3:2:0.03 to obtain an acrylate matrix; 16.61 g of the acrylate matrix, 12.53 g of dodecafluoroheptyl methacrylate and 1.34 g of vinyltrimethoxysilane were mixed and added to the emulsifier solution, ultrasonically dispersed for 30 min, and then magnetically stirred for 30 min to obtain a prefabricated emulsion; 4 .26g of silica composite, 16.61g of acrylate matrix, 0.5g of sodium bicarbonate and 30g of deionized water were added to the prefabricated emulsion, ultrasonically dispersed for 30 minutes, then heated to 50°C, and then continued to heat to 80°C after 20 minutes, added with 0.11g of potassium persulfate, kept warm for 30 minutes, and then added with 0.22g of potassium persulfate within 2 hours, kept warm for reaction, and after the reaction, the system was cooled to 30°C and filtered with a 200-mesh sieve to obtain a silica composite acrylate emulsion.

[0039] Preparation of breathable coating: 17 g of silica composite acrylate emulsion, 83 g of polyurethane, 5 g of sunscreen nanoparticles, 3 g of dispersant and 3 g of defoamer were mixed and stirred for 10 minutes to obtain a breathable coating.

[0040] Among them, the sunscreen nanoparticles are nano zinc oxide.

[0041] Prepare breathable fabrics: S1, mixing polyester fiber and hydrophilic polymer at a mass ratio of 8:1.5, and melt spinning to prepare composite fiber; S2, completely soaking the prepared composite fiber in the breathable coating for 45 min at a temperature of 33° C., so that the breathable coating is fully combined with the composite fiber, and a layer of breathable coating is formed on the surface of the composite fiber, thereby obtaining the treated composite fiber; S3, weaving the treated fibers to obtain a composite fabric; S4. The composite fabric is heat treated at a temperature of 135° C. for 8 minutes, so that the components in the composite fabric are more closely bonded to obtain a super breathable fabric.

[0042] Wherein, the hydrophilic polymer is polyvinyl alcohol.

[0043] Example 4 Example 4 is based on Example 3. The difference between Example 4 and Example 3 is that the mass ratio between the polyester fiber and the hydrophilic polymer in Example 4 is 8.5:1.5.

[0044] Example 5 Example 5 is based on Example 3. The difference between Example 5 and Example 3 is that in Example 4, when preparing the silicon dioxide composite, 9 g of tetraethoxysilane, 1 g of hexadecyltrimethylammonium bromide and 5 g of eugenol are used.

[0045] Example 6 Example 6 is based on Example 3. The difference between Example 6 and Example 3 is that in Example 6, when preparing the silicon dioxide composite, 10.26 g of tetraethoxysilane, 0.79 g of hexadecyltrimethylammonium bromide and 3.95 g of eugenol are used.

[0046] Example 7 Example 7 is based on Example 3. The difference between Example 7 and Example 3 is that when preparing the silica composite acrylate emulsion in Example 7, a total of 33.72 g of acrylate matrix, 12.72 g of dodecafluoroheptyl methacrylate and 3.56 g of silica composite are used.

[0047] Example 8 Example 8 is based on Example 3. The difference between Example 8 and Example 3 is that when Example 8 prepares the silica composite acrylate emulsion, a total of 32.72 g of acrylate matrix, 12.35 g of dodecafluoroheptyl methacrylate and 4.93 g of silica composite are used.

[0048] Example 9 Example 9 is based on Example 3. In Example 9, when preparing the silica composite acrylate emulsion, the silica composite is prepared by the following method: Mix 15 g of tetraethoxysilane with 50 g of anhydrous ethanol, add ammonia water to adjust the pH value of the system to 9, control the system temperature to 50°C, add 30 g of deionized water, stir and react for 4 hours, use glacial acetic acid to adjust the pH value of the system to neutral, add 0.2 g of KH-560 (CAS No.: 2530-83-8), continue to react at 50°C for 4 hours, wash three times by centrifugation with anhydrous ethanol, and obtain a silica composite after drying.

[0049] Example 10 Example 10 is based on Example 3. The silicon dioxide composite in Example 10 is prepared by mixing nano silicon dioxide and eugenol in a mass ratio of 7:4.

[0050] Embodiment 11 Example 11 is based on Example 3. In Example 11, when preparing the composite fiber, the mass ratio between the polyester fiber and the hydrophilic polymer is 6:4.

[0051] Example 12 Example 12 is based on Example 3. In Example 12, when preparing the composite fiber, the mass ratio between the polyester fiber and the hydrophilic polymer is 9.5:0.5.

[0052] Embodiment 13 Example 13 is based on Example 3, and the soaking treatment time in step S2 of Example 13 is 20 minutes.

[0053] Embodiment 14 Example 14 is based on Example 3, and the soaking treatment time in step S2 of Example 14 is 70 minutes.

[0054] Embodiment 15 Example 15 is based on Example 3, and the immersion treatment temperature in step S2 of Example 15 is 15°C.

[0055] Example 16 Example 16 is based on Example 3, and the immersion treatment temperature in step S2 of Example 16 is 50°C.

[0056] Embodiment 17 Example 17 is based on Example 3, and the heat treatment temperature in step S4 in Example 17 is 100°C.

[0057] Embodiment 18 Example 18 is based on Example 3, and the heat treatment temperature in step S4 in Example 18 is 170°C.

[0058] Embodiment 19 Example 19 is based on Example 3, and the heat treatment time in step S4 in Example 19 is 3 minutes.

[0059] Embodiment 20 Example 20 is based on Example 3, and the heat treatment time in step S4 in Example 20 is 15 minutes.

[0060] Comparative Example 1 Comparative Example 1 is based on Example 3, and no hydrophilic polymer is added in Comparative Example 1.

[0061] Comparative Example 2 Comparative Example 2 is based on Example 3. In Comparative Example 2, when preparing the silica composite acrylate emulsion, the silica composite is replaced with ordinary silica.

[0062] Example 3 Comparative Example 3 is based on Example 3. In Comparative Example 3, dodecafluoroheptyl methacrylate is not added when preparing the silica composite acrylate emulsion.

[0063] Comparative Example 4 Comparative Example 4 is based on Example 3. When preparing the breathable coating, no sunscreen nanoparticles are added in Comparative Example 4.

[0064] Performance testing The samples of Examples 1-20 and Comparative Examples 1-4 were sampled and the following performance tests were performed: (1) Hydrophobic properties The contact angle of the prepared sample surface was tested. Three points were randomly selected for each sample and tested three times. The average value was taken and the test results were filled in Table 1.

[0065] (2) Antibacterial properties Taking “GB / T 20944.1 Evaluation of antibacterial properties of textiles” as the testing standard, the antibacterial performance of the prepared fabrics was tested, and the antibacterial rate was tested after 7d and 120d respectively. Each sample was tested 3 times, and the average value was taken. The test results were filled in Table 1.

[0066] (3) Anti-ultraviolet performance The anti-ultraviolet performance of the prepared fabrics was tested according to GB / T 18830-2009 Evaluation of the anti-ultraviolet performance of textiles. Each sample was tested 3 times, and the average value was taken. The test results were filled in Table 1.

[0067] Table 1 Performance test results of samples of Examples 1-20 and Comparative Examples 1-4 Combined with Table 1, it can be seen that the hydrophobic angles of Examples 1-4 are all 141° and above, indicating that the super-breathable fabric prepared by this application has good hydrophobic properties; the antibacterial rates of Escherichia coli in Examples 1-4 are all 99.55% and above at 7d, and 97.22% and above at 14d, and the antibacterial rates of Staphylococcus aureus are all above 99.67% at 7d, and 97.25% and above at 14d, indicating that the super-breathable fabric prepared by this application has good antibacterial properties and can play a long-term antibacterial role; the ultraviolet blocking rates of Examples 1-4 are all 97.24% and above, indicating that the super-breathable fabric prepared by this application has good anti-ultraviolet properties.

[0068] In Example 5 and Example 6, when preparing the silica composite, the mass ratios of tetraethoxysilane, hexadecyltrimethylammonium bromide and eugenol are not within the range specified in the present application. When the content of tetraethoxysilane is too little, it is difficult to completely coat the eugenol in the system, so that part of the eugenol is free in the system, and the eugenol is rapidly oxidized in the early stage, affecting the long-term antibacterial performance; when the content of tetraethoxysilane is too much, the content of eugenol is too little, affecting the overall antibacterial performance of the system. At the same time, the excessive amount of nano-silica generated agglomerates in the system, affecting the overall stability of the coating system.

[0069] The mass ratios of the acrylate matrix, dodecafluoroheptyl methacrylate and the silica composite in Examples 7 and 8 are not within the range defined in the present application. When the content of the silica composite is too much, the silica composite agglomerates in the system, affecting the stability of the system; when the content of the silica composite is too little, the conversion rate of the emulsion system is affected, thereby also affecting the overall stability and comprehensive performance of the emulsion system.

[0070] In Example 9, when preparing the silica composite, only KH-560 was used to modify the surface of silica, and eugenol was not added, so the antibacterial performance of the system was reduced.

[0071] In Example 10, when preparing the silica composite, only the nano-silica and eugenol were physically mixed. At this time, the eugenol can only play a good antibacterial performance in the initial stage, and then it is quickly oxidized, and the antibacterial performance is greatly reduced.

[0072] In Example 11 and Example 12, when preparing the composite fiber, the mass ratio between the polyester fiber and the hydrophilic polymer is not within the range specified in the present application. When the mass ratio between the polyester fiber and the hydrophilic polymer is too large or too small, it will affect the comprehensive performance between the breathable coating and the composite fiber.

[0073] When the composite fiber is immersed in water for treatment, if the immersion time is too long or too short, it will affect the comprehensive performance of the prepared super breathable fabric; if the immersion temperature is too high or too low, it will affect the comprehensive performance of the prepared super breathable fabric. Therefore, the various performances of Examples 13-16 are all reduced.

[0074] When the composite fabric is heat-treated, if the treatment temperature is too high or too low, the comprehensive performance of the prepared super breathable fabric will be affected; if the heat treatment time is too long or too short, the comprehensive performance of the super breathable fabric will be affected. Therefore, the comprehensive performance of Examples 17-20 is reduced.

[0075] In Comparative Example 1, no hydrophilic polymer is added, the hydrophilic effect of the fiber is difficult to improve, and the bonding performance between the fiber and the breathable coating is reduced.

[0076] In Comparative Example 2, the silica composite was replaced with ordinary silica. Ordinary silica agglomerated in the system, affecting the overall stability of the coating system. At the same time, the antibacterial performance of the coating system without adding eugenol also decreased.

[0077] In Comparative Example 3, dodecafluoroheptyl methacrylate was not added, so that there was no fluorine element in the prepared silica composite acrylate emulsion, and the overall hydrophobic performance of the coating was difficult to further improve. At the same time, it was difficult to form CF bonds, which reduced the bonding strength between the breathable coating and the composite fiber, further affecting the overall stability of the system.

[0078] In Comparative Example 4, since no sunscreen nanoparticles were added, the anti-ultraviolet performance of the super breathable fabric was reduced.

[0079] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a highly elastic polyester instant-drying super breathable fabric, characterized in that: The steps include: S1, mixing polyester fiber and hydrophilic polymer, and melt spinning to prepare composite fiber; S2, impregnating the composite fiber into the breathable coating, forming a breathable coating layer on the surface of the composite fiber, and obtaining a treated composite fiber; S3, weaving the treated fibers to obtain composite fabrics; S4, heat-treating the composite fabric to obtain a super breathable fabric; The hydrophilic polymer includes any one of polyvinyl alcohol and sodium polyacrylate, and the breathable coating includes silicon dioxide composite acrylate emulsion, dispersant and defoamer.

2. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 1, characterized in that: The silicon dioxide composite acrylate emulsion comprises an acrylate matrix, a silicon dioxide composite and dodecafluoroheptyl methacrylate, and the silicon dioxide composite acrylate emulsion is prepared by the following method: The emulsifier is mixed with water to obtain an emulsifier solution; a part of the acrylate matrix, dodecafluoroheptyl methacrylate and vinyl trimethoxysilane are mixed, added to the emulsifier solution, ultrasonically treated, and then magnetically stirred to obtain a prefabricated emulsion; a silicon dioxide composite, the remaining part of the acrylate matrix, sodium bicarbonate and water are added to the prefabricated emulsion, the temperature is increased after ultrasonic treatment, potassium persulfate is added for reaction, and after the reaction, filtering is performed to obtain a silicon dioxide composite acrylate emulsion.

3. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 2, characterized in that: The acrylic ester matrix includes any one of butyl acrylate, methyl methacrylate and hydroxyethyl methacrylate or a mixture of several of them.

4. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 3, characterized in that: The mass ratio of the acrylate matrix, the silica composite and dodecafluoroheptyl methacrylate is 2.65:(0.32-0.36):

1.

5. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 2, characterized in that: The silicon dioxide composite comprises silicon dioxide, eugenol and hexadecyltrimethylammonium bromide.

6. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 5, characterized in that: The silicon dioxide composite is prepared by the following method: Water and hexadecyltrimethylammonium bromide are mixed to obtain a surfactant solution, and eugenol is added to obtain a mixed solution; tetraethoxysilane, ethanol, and (3-aminopropyl)triethoxysilane are mixed, added to the mixed solution for reaction, and allowed to stand until stratification, centrifuged, washed, and dried to obtain a silicon dioxide composite.

7. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 5, characterized in that: The mass ratio of the tetraethoxysilane, hexadecyltrimethylammonium bromide and eugenol is (2.1-2.3):0.2:

1.

8. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 1, characterized in that: The breathable coating also includes sunscreen nanoparticles.

9. The method for preparing a highly elastic polyester instant-drying super breathable fabric according to claim 1, characterized in that: In the step S2, the soaking treatment time is 30-60 minutes, and the soaking temperature is 25-40° C.; in the step S4, the heat treatment temperature is 120-150° C., and the treatment time is 5-10 minutes.

10. Use of the high-elastic polyester instant-drying super-breathable fabric according to any one of claims 1 to 9 in sportswear.