Split type nanocrystalline alloy steel casting tank and preparation method thereof

Through the split structure, the graphite runner groove and corundum cast steel head are combined to solve the problems of short life and liquid steel adhesion at high temperatures, achieving long life, low cost and easy cleaning.

CN119022664AActive Publication Date: 2024-11-26GUANGDONG ENERGY ENG POWER EQUIP PLANT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411417917.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-26
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

The existing nanocrystal alloy cast steel trough has a short life at high temperature and the liquid steel is prone to stick to it, resulting in short service life and difficulty in cleaning.

Method used

The split structure design is adopted, and the graphite runner groove and the corundum steel head are combined through a detachable connection. The graphite runner groove is responsible for high temperature resistance and the corundum steel head is responsible for flow diversion to avoid local damage and liquid steel adhesion.

Benefits of technology

It achieves the effect of long service life, low cost and not easy to adhere to the steel, avoids the disadvantages of the integrated cast steel trough and reduces the replacement cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119022664A_ABST
    Figure CN119022664A_ABST
Patent Text Reader

Abstract

The invention discloses a split type nanocrystalline alloy steel casting groove and a preparation method thereof.The split type nanocrystalline alloy steel casting groove is formed by splicing a graphite runner groove located in the rear section and a corundum steel casting head located in the front section, the graphite runner groove is made of graphite, and the corundum steel casting head is made of tabular corundum; the graphite runner groove and the corundum steel pouring head are detachably connected through a lap joint structure. The detachable and replaceable split type structural design is adopted, the nanocrystalline alloy steel pouring groove is divided into two parts, the graphite runner groove and the corundum steel pouring head which are made of different materials are spliced, the two-section structure can be independently replaced, and overall replacement caused by local damage is avoided; besides, the advantages of the corundum material and the graphite material are fully utilized, the cost is controlled, molten steel is prevented from adhering to the runner groove, and the defects that an existing integral graphite nanocrystalline alloy steel casting groove is short in service life and the molten steel is prone to adhering to the integral corundum nanocrystalline alloy steel casting groove are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel casting troughs, and in particular to a split nanocrystalline alloy steel casting trough used for producing and preparing nanocrystalline alloy strips and a preparation method thereof. Background Art

[0002] Nanocrystalline alloy soft magnetic materials have been rapidly developed in production and application in recent years due to their excellent electromagnetic properties, high saturation magnetic induction intensity, high squareness ratio, high magnetic permeability, low loss, stable performance and other advantages, especially various high-quality iron core materials used in switching power supplies and ISDN. At present, nanocrystalline alloy strips are mainly produced by single-roller rapid quenching method. The preparation process is: the nanocrystalline master alloy is put into a vacuum medium frequency furnace for remelting, and the melted alloy steel liquid is poured into the nozzle package through the nanocrystalline master alloy pouring trough and heated. After heating to 1400℃, the alloy steel liquid flows out of the nozzle package, passes through the water nozzle and nozzle cup, and finally sprays onto the high-speed rotating cooling copper roller through the nozzle to condense, and finally forms a nanocrystalline alloy strip with a thickness of 16 to 30μm and a width of 10 to 75mm. The nanocrystalline master alloy pouring trough is one of the key components of the nanocrystalline alloy strip production line. It is installed at the tail of the vacuum melting furnace. Its main function is to pour the nanocrystalline master alloy steel liquid of the vacuum melting furnace into the nozzle package, and it is a bridge between the vacuum melting furnace and the nozzle package.

[0003] The existing nanocrystalline master alloy casting trough is an integral type. According to the different materials, there are mainly two types:

[0004] The first type is an integral corundum casting trough, all of which are made of plate-shaped corundum. The advantages are simple structure and low cost. However, there are the following disadvantages: ① The corundum casting head has a short life. Under the continuous erosion of high-temperature molten steel, its life is very short and it will crack and become scrapped in about one month; ② The surface of the corundum runner trough is rough, and the molten steel is easy to adhere to both sides of the runner trough, which is troublesome to clean; ③ After the residual molten steel in the runner trough cools down, the steel block will firmly adhere to the bottom wall of the corundum runner trough, making it easy to scrape the bottom wall of the runner trough when the steel block is subsequently picked, resulting in pits on the bottom wall, slag, and pollution of the molten steel.

[0005] The second type is the integral graphite casting trough, which is made entirely of graphite. It has two advantages: ① The graphite surface is smooth, and the molten steel is not easy to adhere to the sides of the graphite casting trough; ② After the molten steel remaining in the graphite flow channel trough cools, it will automatically separate from the bottom wall of the graphite flow channel trough and will not adhere to the bottom of the graphite trough, making it easy to clean. However, there are also two disadvantages: ① The graphite casting steel head is relatively fragile, and under the continuous erosion of high-temperature molten steel, its life is very short, and it will crack and become scrapped in one month; ② The manufacturing cost of the graphite casting trough is high, which is 5 to 6 times that of the corundum casting trough.

[0006] Therefore, there is an urgent need for a new type of steel casting trough which is relatively low in cost, has a long service life and is not easy for molten steel to adhere to the runner groove. Summary of the invention

[0007] The purpose of the present invention is to provide a split nanocrystalline alloy casting trough and a preparation method thereof. A detachable and replaceable split structural design is adopted to splice a graphite flow channel trough and a corundum casting steel head made of different materials, thereby forming a split nanocrystalline alloy casting trough. The advantages of the two materials are perfectly combined, so that the split nanocrystalline alloy casting trough has the advantages of long service life, low cost and the steel liquid is not easy to adhere to the flow channel. It solves the shortcomings of the existing integral graphite nanocrystalline alloy casting trough mentioned in the above background technology, that is, the service life is short and the integral corundum nanocrystalline alloy casting trough is easy to adhere to the steel liquid.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] In the first aspect, the present invention provides a split nanocrystalline alloy casting trough, which is formed by splicing a graphite flow channel groove located in the rear section and a corundum casting head located in the front section, wherein the graphite flow channel groove is made of graphite, and the corundum casting head is made of plate-shaped corundum, and the graphite flow channel groove and the corundum casting head are detachably connected via a lap structure.

[0010] Furthermore, the graphite flow channel groove includes a horizontally distributed groove bottom, and both sides of the groove bottom and the side away from the corundum casting head are provided with groove walls extending upward, and the end of the groove bottom away from the corundum casting head is provided with a downward opening feed pipe; the corundum casting head includes a casting head body, and the upper surface of the casting head body has a guide arc surface distributed upward away from the graphite flow channel groove, and both sides of the casting head body are respectively provided with upward extending ribs.

[0011] Furthermore, the central axis of the feed pipe is perpendicular to the bottom of the trough, and the feed pipe as a whole is in a cone shape that is larger at the top and smaller at the bottom, with a taper of (1:10) to (1:20).

[0012] Furthermore, there are arc transitions between the groove wall and the groove bottom, and between the retaining edge and the casting head body.

[0013] Furthermore, the curvature of the guide cambered surface is R500mm to R1000mm.

[0014] Furthermore, the overlap structure includes an upper overlap joint and a lower overlap joint which are seamlessly overlapped.

[0015] Furthermore, the upper lap joint and the lower lap joint are distributed along the width direction of the split nanocrystalline alloy casting steel trough.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned split nanocrystalline alloy casting trough, comprising the following steps:

[0017] S1. Preparation of graphite flow channel:

[0018] S11, crushing, screening and batching: first, the raw materials for preparing the graphite flow channel groove are crushed and screened into 1# material with a particle size of 5 mesh, 2# material with a particle size of 20 mesh, 3# material with a particle size of 100 mesh, 4# material with a particle size of 200 mesh and 5# material with a particle size of 300 mesh; then, the crushed materials of different particle sizes are mixed uniformly according to the weight ratio of 1# material: 2# material: 3# material: 4# material: 5# material = (8-14): (12-18): (12-18): (12-18): (40-50) to obtain the first intermediate raw material;

[0019] S12, dry mixing: dry mixing the prepared first intermediate raw material, the dry mixing time is 30min to 60min, and the dry mixing temperature is 60°C to 80°C;

[0020] S13, kneading: adding a binder and kneading at a kneading temperature of 80° C. to 95° C. for a kneading time of 50 min to 70 min to obtain a second intermediate raw material;

[0021] S14, molding: drying the second intermediate raw material obtained by kneading at a temperature of 90° C. to 115° C. for 25 min to 40 min to obtain a clay material for isostatic pressing; then, the clay material is loaded into a mold of a predetermined shape, and is pressed and molded using an isostatic press, with a molding pressure of 20 MPa to 31 MPa and a holding time of 30 min to 60 min to obtain an intermediate product;

[0022] S15, curing and sintering: the intermediate product is loaded into a tunnel kiln, filled with argon gas for protection and anti-oxidation roasting, the purity of argon gas is ≥99%, the pressure of argon gas is 0.55MPa~0.7MPa, the roasting temperature is 1000℃~1250℃, the roasting time is 48h~72h, and then naturally cooled to room temperature;

[0023] S16, graphitization: the solidified and sintered product is then placed in a high-temperature graphitization furnace for graphitization treatment, the graphitization time is 60h to 80h, and the maximum graphitization temperature is 2300°C to 2600°C;

[0024] S17, machining: machining the outer dimensions to obtain the graphite flow channel groove;

[0025] S2. Preparation of corundum cast steel head:

[0026] S21. Weigh the raw materials for preparing the corundum cast steel head. The corundum cast steel head is composed of the following raw materials by mass percentage: 30% to 43% of 2-6 mm plate-shaped corundum aggregate, 10% to 24% of 0.5-2 mm plate-shaped corundum aggregate, 20% to 32% of 0-0.5 mm plate-shaped corundum powder, 5% to 10% of metal silicon powder, 2% to 4% of metal aluminum powder, and α-Al 2 O 3 Micro powder 5% to 10%, binder 4% to 7% and water 3% to 6%;

[0027] S22, prepare the co-grinding powder: 0 ~ 0.5mm particle plate-shaped corundum powder, metal silicon powder, metal aluminum powder and α-Al 2 O 3 The micro powders are premixed and co-milled for 30 to 40 minutes to form co-milled powders;

[0028] S23, preparing mud material: mixing 2-6 mm plate-shaped corundum aggregate and 0.5-2 mm plate-shaped corundum aggregate for 3-5 min, then adding the co-ground powder obtained in step S22, adding water and a binder, mixing and stirring evenly to obtain a corundum cast steel head embryo wet material;

[0029] S24, molding: putting the embryo wet material into the mold, placing it in the top-mounted vibration pressure molding machine for vibration, pressure and ramming molding;

[0030] S25, drying: drying the formed steel head embryo after demoulding, the drying temperature is 120°C to 135°C, the heating time is 1h, and the temperature is kept at 120°C to 135°C for 9h to 12h;

[0031] S26, sintering: put the dried steel head embryo into the nitriding furnace for sintering, the nitriding sintering temperature is 1400℃~1550℃, the heating time is 11 hours, and the temperature is kept at 1400℃~1550℃ for 11h~13h, and the nitrogen flow rate is 11m 3 / h~12m 3 / h; after sintering, take it out and cool it to obtain a corundum cast steel head;

[0032] S3. Splice the graphite flow channel trough and the corundum casting steel head to obtain a split nanocrystalline alloy casting steel trough.

[0033] Furthermore, in step S11, the raw material for preparing the graphite flow channel groove is a non-graphitized carbon material with a carbon content of ≥99%, an ash content of ≤0.35%, a volatile matter of ≤0.4%, and a sulfur content of ≤0.16%.

[0034] Further, in step S13, the binder used to prepare the graphite flow channel groove is any one of polyurethane resin, silicone resin, and polyimide, and the amount of the binder accounts for 6% to 13% of the total amount of the first intermediate raw material.

[0035] Further, in step S21, the raw material index requirements for preparing the corundum casting steel head are as follows: Al in the plate-shaped corundum aggregate 2 O 3 Content ≥99%, Fe 2 O 3 Content ≤0.2%, Na 2 O content ≤ 0.37%; Si content in metal silicon powder ≥ 98%; α-Al 2 O 3 α-Al in micro powder 2 O 3 The content is ≥98%, the particle size is ≤1 micron; the Al content in the metal aluminum powder is ≥99%.

[0036] Further, in step S21, the binder used to prepare the corundum cast steel head is any one of polyvinyl alcohol (ie PVA), ethylene-vinyl alcohol copolymer (ie PVOH), and clay.

[0037] Compared with the prior art, the present invention provides a split nanocrystalline alloy steel casting trough and a preparation method thereof, which has the following beneficial effects:

[0038] The present invention adopts a detachable and replaceable split structure design, which divides the nanocrystalline alloy casting steel trough into two parts, and splices the graphite flow channel trough and the corundum casting steel head made of different materials. The corundum casting steel head located at the front section and the graphite flow channel trough located at the rear section can be replaced independently, avoiding the overall replacement due to local damage.

[0039] Since the front-end casting steel head has a short life, it is made of cheap corundum material, which can reduce the cost of frequent replacement; while the back-end flow channel groove has a long life and is made of relatively expensive graphite material, which can reduce the cost of low-frequency replacement. The present invention fully utilizes the advantages of corundum material and graphite material, successfully avoids the disadvantages of the two materials, and achieves the optimal combination, which not only controls the cost but also avoids the adhesion of molten steel to the flow channel groove. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0041] Figure 1 It is a schematic diagram of the main cross-sectional structure of the present invention;

[0042] Figure 2 It is a schematic diagram of the top view structure of the present invention;

[0043] Figure 3 for Figure 1 The cross-section along the AA direction;

[0044] Figure 4 for Figure 2 Cross-section along the BB direction.

[0045] Figure numerals: 1, graphite flow channel groove; 11, groove bottom; 12, groove wall; 13, feed pipe; 14, lower lap joint; 2, corundum casting steel head; 21, casting steel head body; 22, guide arc surface; 23, retaining edge; 24, upper lap joint. DETAILED DESCRIPTION

[0046] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] refer to Figure 1 to Figure 4 The present invention provides a split nanocrystalline alloy casting trough, which is formed by splicing a graphite flow channel trough 1 located at the rear section and a corundum casting head 2 located at the front section. The graphite flow channel trough 1 and the corundum casting head 2 are detachably connected through an overlap structure.

[0049] Among them, the graphite flow channel groove 1 is made of graphite. Specifically, the graphite flow channel groove 1 includes a horizontally distributed groove bottom 11, and both sides of the groove bottom 11 and the side away from the corundum casting head 2 are provided with groove walls 12 extending upward, and the end of the groove bottom 11 away from the corundum casting head is provided with a downwardly opening feed pipe 13. The central axis of the feed pipe 13 is perpendicular to the groove bottom 11, and the whole feed pipe 13 is a cone with a larger top and a smaller bottom, and the taper is (1:10) ~ (1:20), so as to facilitate the connection with the nozzle casting steel mouth. There is an arc surface transition between the groove wall 12 and the groove bottom 11 to avoid stress concentration. As an example, the purity of graphite used to prepare the graphite flow channel groove is above 99%.

[0050] The corundum casting head 2 is made of plate-shaped corundum. Specifically, the corundum casting head 2 includes a casting head body 21, the upper surface of which has a guide arc surface 22 that is distributed upward away from the graphite flow channel groove 1, and the two sides of the casting head body 21 are respectively provided with ribs 23 extending upward. There is an arc transition between the rib 23 and the casting head body 21 to avoid stress concentration. The curvature of the guide arc surface 22 is R500mm~R1000mm, and the specific specifications and dimensions can be set according to the needs of use.

[0051] In some specific embodiments, the lap joint structure includes an upper lap joint 24 and a lower lap joint 14 that are seamlessly lapped. Specifically, the upper lap joint 24 and the lower lap joint 14 are both distributed along the width direction of the split nanocrystalline alloy casting trough. As an example, in this embodiment, the upper lap joint 24 is arranged at one end of the corundum casting head 2 close to the graphite flow channel 1, and the lower lap joint 14 is arranged at one end of the graphite flow channel 1 close to the corundum casting head 2, and the cross-sectional shapes of the upper lap joint 24 and the lower lap joint 14 are both rectangular.

[0052] In this way, by adopting a split structural design, the advantages of the two materials are combined, which effectively solves the shortcomings of the existing integral graphite nanocrystalline alloy casting trough, which has a short life, and the integral corundum nanocrystalline alloy casting trough, which is easy to adhere to the molten steel.

[0053] The present invention is further described in detail below through detailed preparation examples in conjunction with the accompanying drawings.

[0054] Unless otherwise specified, the experimental and testing methods used in the preparation examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial channels unless otherwise specified.

[0055] Preparation Example 1

[0056] A split type nanocrystalline alloy casting trough is formed by splicing a graphite flow channel trough 1 at the rear section and a corundum casting head 2 at the front section. The structure is as follows Figure 1 to Figure 4 As shown, it is the same as Example 1, so it will not be repeated here. The specific preparation method is as follows:

[0057] S1. Preparation of graphite flow channel 1:

[0058] S11, crushing, screening and batching: First, crush the raw materials for preparing the graphite flow channel groove 1, wherein the raw materials for preparing the graphite flow channel groove 1 are ungraphitized petroleum coke, with a carbon content of 99.12%, an ash content of 0.12%, a volatile matter of 0.22%, and a sulfur content of 0.11%. Then screen them into 1# material with a particle size of 5 mesh, 2# material with a particle size of 20 mesh, 3# material with a particle size of 100 mesh, 4# material with a particle size of 200, and 5# material with a particle size of 300 mesh. Afterwards, the crushed materials of different particle sizes are evenly mixed according to the weight ratio of 1# material: 2# material: 3# material: 4# material: 5# material = 12:14:15:16:43 to obtain the first intermediate raw material.

[0059] S12, dry mixing: put the prepared first intermediate raw material into a kneader for dry mixing, the dry mixing time is 45 minutes, and the dry mixing temperature is 70°C.

[0060] S13, kneading: Put the first intermediate raw material and the binder after dry mixing into a kneading machine at the same time and knead them at a kneading temperature of 90° C. for 60 minutes to obtain a second intermediate raw material. The binder used to prepare the graphite flow channel groove 1 is polyurethane resin, and its amount accounts for 8.5% of the total amount of the first intermediate raw material.

[0061] S14, molding: The second intermediate raw material obtained by kneading is dried at 103°C for 33 minutes using a drum drying equipment to obtain a mud material for isostatic pressing, wherein the volatile matter is 2.97%; then, the mixed mud material is directly loaded into an epoxy resin mold of a predetermined shape, and is pressed and molded using an isostatic press with a molding pressure of 28 MPa and a holding time of 50 minutes to obtain an intermediate product.

[0062] S15, solidification and sintering: the intermediate product after isostatic pressing is loaded into a tunnel kiln, filled with argon gas for protection and anti-oxidation roasting, the purity of argon gas is 99.32%, the argon gas pressure is 0.65MPa, the roasting temperature is 1130℃, the heating time is 52h, and it is kept at 1130℃ for 5h, and then naturally cooled to room temperature.

[0063] S16. Graphitization: The solidified and sintered product is then placed in a high-temperature graphitization furnace for graphitization treatment. The graphitization time is 72 hours and the maximum graphitization temperature is 2450°C.

[0064] S17, machining: Use CNC machine tools to process into the external dimensions required by the user, and use X-ray flaw detection on the product to obtain the graphite flow channel groove 1.

[0065] S2. Preparation of corundum cast steel head 2:

[0066] S21, weigh the raw materials for preparing the corundum cast steel head 2, and the corundum cast steel head 2 is composed of the following raw materials by mass percentage: 36% of 2-6mm plate-shaped corundum aggregate, 15% of 0.5-2mm plate-shaped corundum aggregate, 24% of 0-0.5mm plate-shaped corundum powder, 6% of metal silicon powder, 3% of metal aluminum powder, and α-Al 2 O 3 7% micro powder, 5% binder and 4% water. Among them, the raw materials used to prepare corundum cast steel head have the following index requirements: Al in plate-shaped corundum aggregate 2 O 3 Content ≥99%, Fe 2 O 3 Content ≤0.2%, Na 2 O content ≤ 0.37%; Si content in metal silicon powder ≥ 98%; α-Al 2 O 3 α-Al in micro powder 2 O 3The content is ≥98%, the particle size is ≤1 micron; the Al content in the metal aluminum powder is ≥99%. The binder used to prepare the corundum cast steel head 2 is polyvinyl alcohol (ie PVA).

[0067] S22, prepare the co-grinding powder: 0 ~ 0.5mm particle plate-shaped corundum powder, metal silicon powder, metal aluminum powder and α-Al 2 O 3 The micro powders are pre-mixed and ground in a ball mill for 33 minutes to form co-ground powder. Five magnets are hung under the ball mill, and the iron filings on the magnets are cleaned every time abrasive material is discharged.

[0068] S23, preparing mud material: 2-6mm plate-shaped corundum aggregate and 0.5-2mm plate-shaped corundum aggregate are mixed for 3-5 minutes until they are uniform, and then the co-ground powder obtained in step S22 is added, and water and a binder are added. After mixing and stirring in a wet mill, the wet material of the corundum cast steel head is obtained. At least 5 magnets are hung under the wet mill, and the iron filings on the magnets must be cleaned every time the material is ground.

[0069] S24, molding: putting the embryo wet material into the mold, placing it in the top-mounted vibration pressure molding machine for vibration, pressure and ramming to form.

[0070] S25, drying: after demoulding, the molded cast steel head embryo is placed in an electric drying furnace, heated from room temperature to 125°C, the heating time is 1 hour, and kept at 125°C for 10 hours to dry the moisture of the cast steel head embryo.

[0071] S26, sintering: put the dried steel head embryo into the nitriding furnace for sintering, raise the temperature from room temperature to 1450℃, the heating time is 11 hours, and then keep sintering at 1450℃ for 12 hours, the nitrogen flow rate is 12m 3 / h; after sintering, take it out and cool it to obtain the corundum cast steel head 2.

[0072] S3. Finally, the prepared graphite flow channel trough 1 and the corundum casting steel head 2 are spliced ​​to obtain a split nanocrystalline alloy casting steel trough.

[0073] Preparation Example 2

[0074] A split type nanocrystalline alloy casting trough is formed by splicing a graphite flow channel trough 1 at the rear section and a corundum casting head 2 at the front section. The structure is as follows Figure 1 to Figure 4 As shown, it is the same as Example 1, so it will not be repeated here. The specific preparation method is as follows:

[0075] S1. Preparation of graphite flow channel 1:

[0076] S11, crushing, screening and batching: First, crush the raw materials for preparing the graphite flow channel groove 1, wherein the raw materials for preparing the graphite flow channel groove 1 are ungraphitized petroleum coke, with a carbon content of 99.05%, an ash content of 0.15%, a volatile matter of 0.27%, and a sulfur content of 0.12%. Then screen them into 1# material with a particle size of 5 mesh, 2# material with a particle size of 20 mesh, 3# material with a particle size of 100 mesh, 4# material with a particle size of 200, and 5# material with a particle size of 300 mesh. Afterwards, the crushed materials of different particle sizes are evenly mixed according to the weight ratio of 1# material: 2# material: 3# material: 4# material: 5# material = 10:15:15:15:45 to obtain the first intermediate raw material.

[0077] S12, dry mixing: put the prepared first intermediate raw material into a kneader for dry mixing, the dry mixing time is 50 minutes, and the dry mixing temperature is 75°C.

[0078] S13, kneading: the first intermediate raw material and the binder after dry mixing are put into a kneading machine for kneading at the same time, the kneading temperature is 87° C., the kneading time is 65 minutes, and the second intermediate raw material is obtained. Among them, the binder used for preparing the graphite flow channel groove is silicone resin, and its amount accounts for 9.2% of the total amount of the first intermediate raw material.

[0079] S14, molding: The second intermediate raw material obtained by kneading is dried at 96°C for 28 minutes using a drum drying equipment to obtain a mud material for isostatic pressing, wherein the volatile matter is 4.1%; then, the mixed mud material is directly loaded into an epoxy resin mold of a predetermined shape, and is pressed and molded using an isostatic press with a molding pressure of 26 MPa and a holding time of 55 minutes to obtain an intermediate product.

[0080] S15, solidification and sintering: the intermediate product after isostatic pressing is loaded into a tunnel kiln, filled with argon gas for protection and anti-oxidation roasting, the purity of argon gas is 99.48%, the argon gas pressure is 0.64MPa, the roasting temperature is 1220℃, the heating time is 55h, and it is kept at 1220℃ for 7h, and then naturally cooled to room temperature.

[0081] S16. Graphitization: The solidified and sintered product is then placed in a high-temperature graphitization furnace for graphitization treatment. The graphitization time is 69 hours and the highest graphitization temperature is 2530°C.

[0082] S17, machining: Use CNC machine tools to process into the external dimensions required by the user, and use X-ray flaw detection on the product to obtain the graphite flow channel groove 1.

[0083] S2. Preparation of corundum cast steel head 2:

[0084] S21, weigh the raw materials for preparing the corundum cast steel head 2, and the corundum cast steel head 2 is composed of the following raw materials by mass percentage: 32% of 2-6mm plate-shaped corundum aggregate, 12% of 0.5-2mm plate-shaped corundum aggregate, 26% of 0-0.5mm plate-shaped corundum powder, 7% of metal silicon powder, 4% of metal aluminum powder, and α-Al 2 O 3 8% micro powder, 6% binder and 5% water. Among them, the raw materials used to prepare corundum cast steel head have the following index requirements: Al in plate-shaped corundum aggregate 2 O 3 Content ≥99%, Fe 2 O 3 Content ≤0.2%, Na 2 O content ≤ 0.37%; Si content in metal silicon powder ≥ 98%; α-Al 2 O 3 α-Al in micro powder 2 O 3 The content is ≥98%, the particle size is ≤1 micron; the Al content in the metal aluminum powder is ≥99%. The binder used to prepare the corundum cast steel head is ethylene-vinyl alcohol copolymer (PVOH).

[0085] S22, prepare the co-grinding powder: 0 ~ 0.5mm particle plate-shaped corundum powder, metal silicon powder, metal aluminum powder and α-Al 2 O 3 The micro powders are pre-mixed and ground in a ball mill for 33 minutes to form co-ground powder. Five magnets are hung under the ball mill, and the iron filings on the magnets are cleaned every time abrasive material is discharged.

[0086] S23, preparing mud material: 2-6mm plate-shaped corundum aggregate and 0.5-2mm plate-shaped corundum aggregate are mixed for 3-5 minutes until they are uniform, and then the co-ground powder obtained in step S22 is added, and water and a binder are added. After mixing and stirring in a wet mill, the wet material of the corundum cast steel head is obtained. At least 5 magnets are hung under the wet mill, and the iron filings on the magnets must be cleaned every time the material is ground.

[0087] S24, molding: putting the embryo wet material into the mold, placing it in the top-mounted vibration pressure molding machine for vibration, pressure and ramming to form.

[0088] S25, drying: after demoulding, the molded cast steel head embryo is placed in an electric drying furnace, heated from room temperature to 130°C, the heating time is 1 hour, and kept at 130°C for 11 hours to dry the moisture of the cast steel head embryo.

[0089] S26, sintering: put the dried steel head embryo into the nitriding furnace for sintering, heating from room temperature to 1500℃, heating time 11 hours, then sintering at 1450℃ for 11 hours, nitrogen flow rate 11m 3 / h; after sintering, take it out and cool it to obtain the corundum cast steel head 2.

[0090] S3. Finally, the prepared graphite flow channel trough 1 and the corundum casting steel head 2 are spliced ​​to obtain a split nanocrystalline alloy casting steel trough.

[0091] Preparation Example 3

[0092] A split type nanocrystalline alloy casting trough is formed by splicing a graphite flow channel trough 1 at the rear section and a corundum casting head 2 at the front section. The structure is as follows Figure 1 to Figure 4 As shown, it is the same as Example 1, so it will not be repeated here. The specific preparation method is as follows:

[0093] S1. Preparation of graphite flow channel 1:

[0094] S11, crushing, screening and batching: First, crush the raw materials for preparing the graphite flow channel groove 1, wherein the raw materials for preparing the graphite flow channel groove 1 are ungraphitized petroleum coke, with a carbon content of 99.38%, an ash content of 0.32%, a volatile matter of 0.33%, and a sulfur content of 0.14%. Then screen them into 1# material with a particle size of 5 mesh, 2# material with a particle size of 20 mesh, 3# material with a particle size of 100 mesh, 4# material with a particle size of 200, and 5# material with a particle size of 300 mesh. Afterwards, the crushed materials of different particle sizes are evenly mixed according to the weight ratio of 1# material: 2# material: 3# material: 4# material: 5# material = 13:13:13:15:46 to obtain the first intermediate raw material.

[0095] S12, dry mixing: put the prepared first intermediate raw material into a kneader for dry mixing, the dry mixing time is 57 minutes, and the dry mixing temperature is 78°C.

[0096] S13, kneading: the first intermediate raw material and the binder after dry mixing are put into a kneading machine for kneading at the same time, the kneading temperature is 93° C., the kneading time is 68 minutes, and the second intermediate raw material is obtained. Among them, the binder used for preparing the graphite flow channel groove is a polyimide resin, and its amount accounts for 10.4% of the total amount of the first intermediate raw material.

[0097] S14, molding: The second intermediate raw material obtained by kneading is dried at 112°C for 36 minutes using a drum drying equipment to obtain a mud material for isostatic pressing, wherein the volatile matter is 3.7%; then, the mixed mud material is directly loaded into an epoxy resin mold of a predetermined shape, and is pressed and molded using an isostatic press with a molding pressure of 30 MPa and a holding time of 48 minutes to obtain an intermediate product.

[0098] S15, solidification and sintering: the intermediate product after isostatic pressing is loaded into a tunnel kiln, filled with argon gas for protection and anti-oxidation roasting, the purity of argon gas is 99.39%, the argon gas pressure is 0.59MPa, the roasting temperature is 1190℃, the heating time is 48h, and it is kept at 1190℃ for 9h, and then naturally cooled to room temperature.

[0099] S16, graphitization: the solidified and sintered product is then placed in a high-temperature graphitization furnace for graphitization treatment. The graphitization time is 69 hours and the highest graphitization temperature is 2390°C.

[0100] S17, machining: Use CNC machine tools to process into the external dimensions required by the user, and use X-ray flaw detection on the product to obtain the graphite flow channel groove 1.

[0101] S2. Preparation of corundum cast steel head 2:

[0102] S21, weigh the raw materials for preparing the corundum cast steel head 2, and the corundum cast steel head 2 is composed of the following raw materials by mass percentage: 35% of 2-6mm plate-shaped corundum aggregate, 12% of 0.5-2mm plate-shaped corundum aggregate, 28% of 0-0.5mm plate-shaped corundum powder, 5% of metal silicon powder, 3% of metal aluminum powder, and α-Al 2 O 3 6% micro powder, 7% binder and 4% water. Among them, the raw materials used to prepare corundum cast steel head have the following index requirements: Al in plate-shaped corundum aggregate 2 O 3 Content ≥99%, Fe 2 O 3 Content ≤0.2%, Na 2 O content ≤ 0.37%; Si content in metal silicon powder ≥ 98%; α-Al 2 O 3 α-Al in micro powder 2 O 3 The content is ≥98%, the particle size is ≤1 micron; the Al content in the metal aluminum powder is ≥99%. The binder used to prepare the corundum cast steel head is clay.

[0103] S22, prepare the co-grinding powder: 0 ~ 0.5mm particle plate-shaped corundum powder, metal silicon powder, metal aluminum powder and α-Al 2 O 3 The micro powders are pre-mixed and ground in a ball mill for 33 minutes to form co-ground powder. Five magnets are hung under the ball mill, and the iron filings on the magnets are cleaned every time abrasive material is discharged.

[0104] S23, preparing mud material: 2-6mm plate-shaped corundum aggregate and 0.5-2mm plate-shaped corundum aggregate are mixed for 3-5 minutes until they are uniform, and then the co-ground powder obtained in step S22 is added, and water and a binder are added. After mixing and stirring in a wet mill, the wet material of the corundum cast steel head is obtained. At least 5 magnets are hung under the wet mill, and the iron filings on the magnets must be cleaned every time the material is ground.

[0105] S24, molding: putting the embryo wet material into the mold, placing it in the top-mounted vibration pressure molding machine for vibration, pressure and ramming to form.

[0106] S25, drying: after demoulding, the molded cast steel head embryo is placed in an electric drying furnace, heated from room temperature to 133°C, the heating time is 1 hour, and kept at 130°C for 12 hours to dry the moisture of the cast steel head embryo.

[0107] S26, sintering: put the dried steel head embryo into the nitriding furnace for sintering, heating from room temperature to 1530℃, heating time 11 hours, then sintering at 1520℃ for 13 hours, nitrogen flow rate 12m 3 / h; after sintering, take it out and cool it to obtain the corundum cast steel head 2.

[0108] S3. Finally, the prepared graphite flow channel trough 1 and the corundum casting steel head 2 are spliced ​​to obtain a split nanocrystalline alloy casting steel trough.

[0109] The graphite flow channel grooves and corundum casting steel heads prepared in Preparation Examples 1 to 3 were tested for performance, and the data are shown in Tables 1 and 2 below.

[0110] Table 1 Properties of graphite flow channel grooves prepared in Preparation Examples 1 to 3

[0111]

[0112] Table 2 Properties of the corundum cast steel heads obtained in Preparation Examples 1 to 3

[0113]

[0114] The above embodiments are merely illustrative of the concept and technical solution of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.

[0115] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A split nanocrystalline alloy casting trough, characterized in that: It is formed by splicing a graphite flow channel groove located at the rear section and a corundum casting steel head located at the front section. The graphite flow channel groove is made of graphite, and the corundum casting steel head is made of plate-shaped corundum. The graphite flow channel groove and the corundum casting steel head are detachably connected through an overlap structure.

2. The split type nanocrystalline alloy casting trough according to claim 1, characterized in that: The graphite flow channel groove includes a horizontally distributed groove bottom, and both sides of the groove bottom and the side away from the corundum casting head are provided with groove walls extending upward, and the end of the groove bottom away from the corundum casting head is provided with a downward opening feed pipe; the corundum casting head includes a casting head body, and the upper surface of the casting head body has a guide arc surface distributed upward away from the graphite flow channel groove, and both sides of the casting head body are respectively provided with upward extending ribs.

3. The split type nanocrystalline alloy casting trough according to claim 2, characterized in that: The central axis of the feed pipe is perpendicular to the bottom of the trough, and the feed pipe as a whole is in a cone shape that is larger at the top and smaller at the bottom, with a taper of (1:10) to (1:20).

4. The split type nanocrystalline alloy casting trough according to claim 2, characterized in that: There are arc transitions between the groove wall and the groove bottom, and between the retaining edge and the casting head body.

5. The split type nanocrystalline alloy casting trough according to claim 2, characterized in that: The curvature of the guide cambered surface is R500mm-R1000mm.

6. The split type nanocrystalline alloy casting trough according to claim 1, characterized in that: The overlapping structure comprises an upper overlapping joint and a lower overlapping joint which are seamlessly overlapped.

7. The split type nanocrystalline alloy casting trough according to claim 6, characterized in that: The upper lap joint and the lower lap joint are distributed along the width direction of the split nanocrystalline alloy casting steel trough.

8. A method for preparing a split nanocrystalline alloy steel casting trough as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Preparation of graphite flow channel: S11, crushing, screening and batching: first, the raw materials for preparing the graphite flow channel groove are crushed and screened into 1# material with a particle size of 5 mesh, 2# material with a particle size of 20 mesh, 3# material with a particle size of 100 mesh, 4# material with a particle size of 200 mesh and 5# material with a particle size of 300 mesh; then, the crushed materials of different particle sizes are mixed uniformly according to the weight ratio of 1# material: 2# material: 3# material: 4# material: 5# material = (8-14): (12-18): (12-18): (12-18): (40-50) to obtain the first intermediate raw material; S12, dry mixing: dry mixing the prepared first intermediate raw material, the dry mixing time is 30min to 60min, and the dry mixing temperature is 60°C to 80°C; S13, kneading: adding a binder and kneading at a kneading temperature of 80° C. to 95° C. for a kneading time of 50 min to 70 min to obtain a second intermediate raw material; S14, molding: drying the second intermediate raw material obtained by kneading at a temperature of 90° C. to 115° C. for 25 min to 40 min to obtain a clay material for isostatic pressing; then, the clay material is loaded into a mold of a predetermined shape, and is pressed and molded using an isostatic press, with a molding pressure of 20 MPa to 31 MPa and a holding time of 30 min to 60 min to obtain an intermediate product; S15, curing and sintering: the intermediate product is loaded into a tunnel kiln, filled with argon gas for protection and anti-oxidation roasting, the purity of argon gas is ≥99%, the pressure of argon gas is 0.55MPa~0.7MPa, the roasting temperature is 1000℃~1250℃, the roasting time is 48h~72h, and then naturally cooled to room temperature; S16, graphitization: the solidified and sintered product is then placed in a high-temperature graphitization furnace for graphitization treatment, the graphitization time is 60h to 80h, and the maximum graphitization temperature is 2300°C to 2600°C; S17, machining: machining the outer dimensions to obtain the graphite flow channel groove; S2. Preparation of corundum cast steel head: S21. Weigh the raw materials for preparing the corundum cast steel head. The corundum cast steel head is composed of the following raw materials by mass percentage: 30% to 43% of 2-6 mm plate-shaped corundum aggregate, 10% to 24% of 0.5-2 mm plate-shaped corundum aggregate, 20% to 32% of 0-0.5 mm plate-shaped corundum powder, 5% to 10% of metallic silicon powder, 2% to 4% of metallic aluminum powder, 5% to 10% of α-Al2O3 powder, 4% to 7% of binder and 3% to 6% of water; S22, preparing co-grinding powder: premixing 0-0.5 mm plate-shaped corundum powder, metal silicon powder, metal aluminum powder and α-Al2O3 micropowder, and co-grinding for 30-40 minutes to form co-grinding powder; S23, preparing mud material: mixing 2-6 mm plate-shaped corundum aggregate and 0.5-2 mm plate-shaped corundum aggregate for 3-5 min, then adding the co-ground powder obtained in step S22, adding water and a binder, mixing and stirring evenly to obtain a corundum cast steel head embryo wet material; S24, molding: putting the embryo wet material into the mold, placing it in the top-mounted vibration pressure molding machine for vibration, pressure and ramming molding; S25, drying: drying the formed steel head embryo after demoulding, the drying temperature is 120°C to 135°C, the heating time is 1h, and the temperature is kept at 120°C to 135°C for 9h to 12h; S26, sintering: put the dried steel head embryo into the nitriding furnace for sintering, the nitriding sintering temperature is 1400℃~1550℃, the heating time is 11 hours, and the temperature is kept at 1400℃~1550℃ for 11h~13h, and the nitrogen flow rate is 11m 3 / h~12m 3 / h; after sintering, take it out and cool it to obtain a corundum cast steel head; S3. Splice the graphite flow channel trough and the corundum casting steel head to obtain a split nanocrystalline alloy casting steel trough.

9. The method for preparing a split nanocrystalline alloy steel casting trough according to claim 8, characterized in that: In step S11, the raw material used to prepare the graphite flow channel groove is an ungraphitized carbon material with a carbon content of ≥99%, an ash content of ≤0.35%, a volatile matter of ≤0.4%, and a sulfur content of ≤0.16%; in step S21, the index requirements of the raw material used to prepare the corundum cast steel head are as follows: the Al2O3 content in the plate-like corundum aggregate is ≥99%, the Fe2O3 content is ≤0.2%, and the Na2O content is ≤0.37%; the Si content in the metal silicon powder is ≥98%; the α-Al2O3 content in the α-Al2O3 micropowder is ≥98%, and the particle size is ≤1 micron; the Al content in the metal aluminum powder is ≥99%.

10. The method for preparing a split type nanocrystalline alloy casting trough according to claim 8, characterized in that: In step S13, the binder used to prepare the graphite flow channel groove is any one of polyurethane resin, silicone resin, and polyimide, and the amount of the binder accounts for 6% to 13% of the total amount of the first intermediate raw material; in step S21, the binder used to prepare the corundum cast steel head is any one of polyvinyl alcohol, ethylene-vinyl alcohol copolymer, and clay.

Citation Information

Patent Citations

  • Molten steel runner made of aluminium-carbon composition with low cement content

    CN1053601A

  • Refractory material as well as preparation method and application thereof

    CN118290133A

  • Split type nanocrystalline alloy steel pouring tank

    CN223179303U

  • Dispersion-type corundum-spinel air-permeable brick and preparation method therefor

    WO2018126937A1