Composite conductor, preparation method thereof and electric contact element

By covering the carbide layer and graphene layer on the copper alloy conductor, combined with ball milling and vapor deposition, the hardness and conductivity of the composite conductor are improved, and the oxidation resistance and conductivity of the existing copper alloy conductors are solved. insufficient.

CN119028626APending Publication Date: 2024-11-26ZHEJIANG CHINT ELECTRIC CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310601798.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing copper alloy conductors have shortcomings in oxidation resistance and conductivity, especially at high temperatures, which are prone to oxidation and reduced conductivity, and graphene is difficult to distribute uniformly, so it is impossible to effectively improve conductivity and hardness.

Method used

A composite conductor structure is adopted, including metal particles, carbide layer and graphene layer. The carbide layer covers metal particles to improve hardness and oxidation resistance, and the graphene layer covers metal particles and carbide layer to improve conductivity. And the preparation method is carried out by specific ball milling and vapor deposition methods to ensure uniform distribution of graphene.

Benefits of technology

It significantly improves the hardness and conductivity of composite conductors, solves the problem of simultaneous improvement of conductivity and hardness, and has a simple process and low cost, making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028626A_ABST
    Figure CN119028626A_ABST
Patent Text Reader

Abstract

The invention discloses a composite conductor, a preparation method thereof and an electric contact element, and relates to the technical field of conductors. The composite conductor provided by the present application comprises: metal particles; the carbide layer coats the metal particles; and a graphene layer coating the carbide layer and the metal particles. According to the composite conductor provided by the invention, the metal particles are coated with the carbide layer, so that the combination of the carbide and the metal particles is facilitated, and the carbide can remarkably improve the hardness and oxidation resistance of the metal particles; the metal particles and the carbide layer are coated with the graphene layer, so that uniform distribution of graphene is facilitated, and the conductivity of the metal particles is improved; according to the composite conductor provided by the invention, the hardness and the conductivity of the composite conductor are improved at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of conductor technology, and in particular to a composite conductor and a preparation method thereof, and an electrical contact element. Background Art

[0002] Copper is widely used as an electrical contact conductor, but copper and most copper alloys have poor resistance to welding and breaking, and are very easy to oxidize, which increases the contact resistance of the contact element, resulting in a significant reduction in the reliability and service life of the copper contact material. In the prior art, the hardness and oxidation resistance of copper are usually improved by adding nickel, chromium, carbide, etc., and the loss of copper conductivity caused by adding conductivity-reducing elements is compensated by adding highly conductive materials such as graphene and silver. Limited by the existing processing technology, when chromium is added, chromium is easily precipitated on the copper surface at high temperatures. Although the addition of carbides, such as chromium carbide, tungsten carbide and other substances, can greatly increase the hardness of copper, carbides are difficult to fuse with metals, resulting in uneven distribution of carbides in copper, complex processing technology, high cost, and a large increase in resistance after the alloy is formed, and a more serious reduction in conductivity.

[0003] In the prior art, copper is usually prepared into copper powder, and then a graphene layer is formed on the surface of the copper powder. The copper powder containing the graphene coating layer is mixed with other metals and / or non-metals for further processing to prepare the desired product, so as to give full play to the excellent performance of graphene, improve the strength of copper, improve the breaking ability and anti-oxidation ability, and ensure the conductivity of copper. Although graphene has many excellent properties, it is easy to agglomerate, has poor wettability, and is easily disordered in the metal-graphene mixed material. The existing process cannot well compensate for the loss of conductivity of copper alloy by adding graphene.

[0004] How to simultaneously improve the conductivity and hardness of metals needs further improvement. Summary of the invention

[0005] In view of this, the present application provides a composite conductor and a preparation method thereof, and an electrical contact element, aiming to simultaneously improve the electrical conductivity and hardness of metal.

[0006] The embodiment of the present application is implemented as follows: a composite conductor includes:

[0007] Metal particles;

[0008] a carbide layer covering the metal particles; and

[0009] A graphene layer covers the carbide layer and the metal particles.

[0010] Optionally, in some embodiments of the present application, the coverage rate of the carbide layer on the metal particles is 50% to 80%; and / or

[0011] The coverage rate of the graphene layer on the carbide layer and the metal particles is 90% to 100%.

[0012] Optionally, in some embodiments of the present application, the average particle size of the metal particles is 10 μm to 100 μm; and / or

[0013] The metal particles are copper alone or a copper alloy.

[0014] Optionally, in some embodiments of the present application, the copper alloy includes one or more of a copper-chromium alloy, a copper-nickel alloy, and a copper-antimony alloy.

[0015] Optionally, in some embodiments of the present application, the material of the carbide layer includes one or more of chromium carbide, vanadium carbide, and zirconium carbide; and / or

[0016] The thickness of the carbide layer is 0.5 μm to 10 μm.

[0017] Optionally, in some embodiments of the present application, the number of graphene layers is 5 to 10 layers.

[0018] Optionally, in some embodiments of the present application, the surface of the metal particles is also coated with a metal mixed layer.

[0019] Optionally, in some embodiments of the present application, there is a depression on the surface of the metal particle, and the depth of the metal mixed layer embedded in the depression is 0.01 to 0.5 μm; and / or

[0020] The metal mixed layer is a mixture of copper element and carbide precursor.

[0021] Optionally, in some embodiments of the present application, the carbide precursor includes one or more of chromium, vanadium pentoxide, vanadium trioxide, and zirconium dioxide; and / or

[0022] The metal mixed layer also includes one or more of nickel and antimony.

[0023] Accordingly, an embodiment of the present application further provides a method for preparing a composite conductor, comprising:

[0024] Providing metal particles, and mixing the metal particles with a carbide precursor by ball milling to obtain a metal mixture, wherein the metal mixture is metal particles coated with a metal mixing layer;

[0025] heating the metal mixture and introducing methane to obtain a first intermediate;

[0026] Graphene is deposited on the surface of the first intermediate to obtain a composite conductor.

[0027] Optionally, in some embodiments of the present application, the thickness of the metal mixed layer is 0.5 μm to 10 μm; and / or

[0028] The coverage rate of the metal mixed layer on the metal particles is 50% to 80%; and / or

[0029] There are depressions on the surface of the metal particles, and the depth of the metal mixed layer embedded in the depressions is 0.01 to 0.5 μm.

[0030] Optionally, in some embodiments of the present application, before heating the metal mixture, an anti-sintering agent is provided and mixed with the metal mixture.

[0031] Optionally, in some embodiments of the present application, the anti-sintering agent includes one or more of magnesium oxide, aluminum oxide, graphite, chromium, and silver; and / or

[0032] The average particle size of the anti-sintering agent is 0.1 μm to 15 μm; and / or

[0033] The mass ratio of the metal mixture to the anti-sintering agent is (5-10):4.

[0034] Optionally, in some embodiments of the present application, the temperature of heating the metal mixture is 700° C. to 1070° C.; and / or

[0035] The heating time of the metal mixture is 50 min to 110 min; and / or

[0036] The volume flow rate of the methane is 5 sccm to 20 sccm.

[0037] Accordingly, an embodiment of the present application further provides an electrical contact element, and a method for preparing the electrical contact element includes:

[0038] Providing the composite conductor and pressing it into an embryonic body;

[0039] The green body is sintered to obtain an electrical contact element.

[0040] Optionally, in some embodiments of the present application, sintering the green body includes a first sintering and a second sintering;

[0041] The temperature of the first sintering is 400° C. to 500° C., the pressure of the first sintering is 50KN to 200KN, and the time of the first sintering is 2min to 20min;

[0042] The temperature of the second sintering is 800° C. to 950° C., the pressure of the second sintering is 200 KN to 1200 KN, and the time of the second sintering is 5 min to 20 min.

[0043] In the composite conductor provided by the present application, the carbide layer coats the metal particles, which is beneficial to the combination of the carbide and the metal particles. The carbide can significantly improve the hardness and oxidation resistance of the metal particles. The graphene layer coats the metal particles and the carbide layer, which is beneficial to the uniform distribution of the graphene and improves the conductivity of the metal particles. The composite conductor provided by the present application simultaneously improves the hardness and conductivity of the composite conductor. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0045] Figure 1 is a schematic diagram of the structure of a composite conductor provided in an embodiment of the present application;

[0046] Figure 2 is a flow chart of a method for preparing a composite conductor provided in an embodiment of the present application;

[0047] Reference numerals:

[0048] 10 - metal particle; 20 - carbide layer; 30 - graphene layer. DETAILED DESCRIPTION

[0049] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0050] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0051] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0052] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0053] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0054] The technical solution of this application is as follows:

[0055] First, see Figure 1 , an embodiment of the present application provides a composite conductor, comprising:

[0056] Metal particles 10;

[0057] a carbide layer 20 covering the metal particles 10; and

[0058] The graphene layer 30 covers the carbide layer 20 and the metal particles 10 .

[0059] In the composite conductor provided by the present application, the carbide layer 20 coats the metal particles 10, which is beneficial to the combination of the carbide and the metal particles 10. The carbide can significantly improve the hardness and oxidation resistance of the metal particles 10. The graphene layer 30 coats the metal particles 10 and the carbide layer 20, which is beneficial to the uniform distribution of the graphene and improves the conductivity of the metal particles 10. The composite conductor provided by the present application simultaneously improves the hardness and conductivity of the composite conductor.

[0060] In some embodiments, the average particle size of the metal particles 10 may be 10 μm to 100 μm, for example, 15 μm to 90 μm, 20 μm to 80 μm, 25 μm to 70 μm, 30 μm to 60 μm, 40 μm to 50 μm, etc.

[0061] In some embodiments, the metal particles 10 may be copper or copper alloys. Further, the copper alloy may include one or more of copper-chromium alloy, copper-nickel alloy, and copper-antimony alloy. It is understood that the copper alloy may also be copper-chromium-nickel alloy, or copper-chromium-nickel-antimony alloy.

[0062] Further, when the copper alloy is a copper-chromium-nickel-antimony alloy, the mass fraction of chromium is 0.05% to 3%, for example, 0.06% to 2.8%, 0.07% to 2.5%, 0.08% to 2.2%, 0.09% to 2%, 1% to 1.5%, etc. Within this range, chromium can improve the hardness and resistance to welding of copper. The mass fraction of nickel is 0.1%. Within this range, nickel can improve the corrosion resistance and ductility of copper. In the copper alloy, the mass fraction of antimony is 0.2%. Within this range, chromium can improve the corrosion resistance and resistance to welding of copper.

[0063] In some embodiments, the material of the carbide layer 20 includes one or more of chromium carbide, vanadium carbide, and zirconium carbide.

[0064] In some embodiments, the thickness of the carbide layer 20 is 0.5 μm to 10 μm, for example, 1 μm to 9 μm, 2 μm to 8 μm, 3 μm to 7 μm, 4 μm to 6 μm, 5 μm to 5.5 μm, etc.

[0065] In some embodiments, the coverage rate of the carbide layer 20 on the metal particles 10 is 50% to 80%, for example, 52% to 78%, 55% to 75%, 58% to 72%, 60% to 70%, 62% to 65%, etc.

[0066] In some embodiments, the number of graphene layers 30 is 5 to 10, for example, 6, 7, 8, 9, etc. Further, the thickness of a single graphene layer 30 may be 0.335 nm, in other words, the thickness of the graphene layer 30 may be 1.675 nm to 3.35 nm.

[0067] In some embodiments, the coverage of the graphene layer 30 on the metal particles 10 and the carbide layer 20 is 90% to 100%, for example, 91% to 99%, 92% to 98%, 93% to 97%, 94% to 96%, 95%, etc.

[0068] It should be noted that the metal particles 10 may not be completely covered by the carbide layer 20 , and the surfaces of some of the uncovered metal particles 10 are exposed. The graphene layer 30 partially or completely covers the exposed metal particles 10 and the carbide layer 20 .

[0069] In some embodiments, the surface of the metal particle 10 is further coated with a metal mixed layer.

[0070] In some embodiments, there are depressions on the surface of the metal particles 10 , and the depth of the metal mixed layer embedded in the depressions is 0.01-0.5 μm.

[0071] In some embodiments, the metal mixed layer is a mixture of copper element and a carbide precursor.

[0072] In some embodiments, the carbide precursor includes one or more of chromium, vanadium pentoxide, vanadium trioxide, and zirconium dioxide.

[0073] In some embodiments, the metal mixed layer further includes one or more of nickel and antimony. It is understood that nickel can increase the corrosion resistance and ductility of the composite conductor, and antimony can improve the corrosion resistance and anti-welding property of the composite conductor.

[0074] In some embodiments, there are depressions on the surface of the metal particles 10, and the depth of the metal mixed layer embedded in the depression is 0.01-0.5 μm, for example, 0.05-0.45 μm, 0.1-0.4 μm, 0.15-0.35 μm, 0.2-0.3 μm, 0.25-0.28 μm, etc. It can be understood that ball milling is the high-speed collision and extrusion of metal balls on powders, etc. Under the action of force, the metal layer will be pressed into a sheet and cover the surface of the metal powder, and part of it will be embedded into the surface of the metal powder for a certain distance.

[0075] Second, see Figure 2 The present application also provides a method for preparing the composite conductor, comprising:

[0076] Step S11: providing metal particles 10, and mixing the metal particles 10 with a carbide precursor by ball milling to obtain a metal mixture, wherein the metal mixture is the metal particles 10 coated with a metal mixing layer;

[0077] Step S12: heating the metal mixture and introducing methane to obtain a first intermediate;

[0078] Step S13: depositing graphene on the surface of the first intermediate to obtain a composite conductor.

[0079] The preparation method of the composite conductor provided in the present application makes the carbide precursor on the surface of the metal particle 10 carbonized to form a carbide layer 20, and the carbide layer 20 covers the metal particle 10, which is conducive to the combination of the carbide and the metal particle 10. The carbide can significantly improve the hardness and oxidation resistance of the metal particle 10; and further depositing the graphene layer 30, the graphene layer 30 covers the metal particle 10 and the carbide layer 20, which is conducive to the uniform distribution of graphene and improves the conductivity of the metal particle 10. The preparation method is simple to operate, low in cost, and is conducive to large-scale application.

[0080] In step S11:

[0081] In some embodiments, the thickness of the metal mixed layer is 0.5 μm to 10 μm. It is understood that after carbonization, most of the metal mixed layer is carbonized to form a carbide layer 20 , and a very small part is not completely carbonized and remains between the metal particles 10 and the carbide layer 20 .

[0082] In some embodiments, the coverage rate of the metal mixed layer on the metal particles 10 is 50% to 80%.

[0083] In some embodiments, the carbide precursor includes one or more of chromium, vanadium pentoxide, vanadium trioxide, and zirconium dioxide.

[0084] It can be understood that when the carbide precursor is chromium, under heating conditions, chromium will precipitate, so that most of the chromium is on the outer surface of the metal particle 10, which is conducive to the carburization reaction with methane to form chromium carbide. When the carbide precursor includes vanadium pentoxide and vanadium trioxide, methane can react with them to form vanadium carbide. When the carbide precursor is zirconium dioxide, methane can react with it to form zirconium carbide.

[0085] In some embodiments, the metal mixed layer further includes one or more of nickel and antimony.

[0086] In some embodiments, the rotation speed of the ball milling treatment is 100 r / min to 300 r / min, for example, 120 r / min to 280 r / min, 140 r / min to 260 r / min, 150 r / min to 240 r / min, 160 r / min to 220 r / min, 180 r / min to 200 r / min, etc. The time of the ball milling treatment is 30 min to 300 min, for example, 50 min to 280 min, 80 min to 250 min, 100 min to 220 min, 120 min to 200 min, 150 min to 180 min, etc. In this way, the metal particles 10 are fully mixed with the carbonized precursor.

[0087] In step S12:

[0088] In some embodiments, before heating the metal mixture, a sintering prevention agent is provided and mixed with the metal mixture.

[0089] In some embodiments, the particle size of the sintering inhibitor may be 0.1 μm to 15 μm, for example, 1 μm to 14 μm, 2 μm to 13 μm, 3 μm to 12 μm, 4 μm to 11 μm, 5 μm to 10 μm, etc.

[0090] In some embodiments, the anti-sintering agent includes one or more of magnesium oxide, aluminum oxide, graphite, chromium, and silver. For example, the anti-sintering agent can be magnesium oxide, or a mixture of magnesium oxide and aluminum oxide, or a mixture of magnesium oxide, aluminum oxide, and graphite.

[0091] In some embodiments, the mass ratio of the metal mixture to the anti-sintering agent is (5-10):4, for example, 6:4, 7:4, 8:4, 9:4, etc. It can be understood that the anti-sintering agent can improve the corrosion resistance and thermal shock resistance of the metal mixture at high temperatures, so that the metal mixture still maintains excellent corrosion resistance and other properties after the carbonization reaction.

[0092] In some embodiments, before heating the metal mixture and introducing methane, vacuuming and introducing an inert gas are also performed, and heating is performed under an inert gas atmosphere. The rate of introducing the inert gas can be 200 sccm to 500 sccm, for example, 220 sccm to 480 sccm, 250 sccm to 450 sccm, 280 sccm to 420 sccm, 300 sccm to 400 sccm, 420 sccm to 450 sccm, etc. Further, the inert gas can be one or more of argon, helium, neon, krypton, xenon, and radon.

[0093] It should be noted that under heating conditions, metal particles 10 such as copper will react with oxygen in the air to generate metal oxides, thereby affecting the performance of the metal particles 10. Therefore, before the heating reaction, an inert gas is introduced to prevent the metal particles 10 from contacting and reacting with oxygen.

[0094] In some embodiments, after the inert gas is introduced, hydrogen is also introduced to perform heat treatment.

[0095] In some embodiments, the temperature of the heat treatment is 400°C to 700°C, for example, 420°C to 680°C, 450°C to 650°C, 480°C to 600°C, 500°C to 580°C, 520°C to 560°C, etc. The time of the heat treatment is 30min to 90min, for example, 35min to 80min, 40min to 75min, 45min to 70min, 50min to 65min, 55min to 60min, etc. In this way, hydrogen can reduce the metal particles 10, such as reducing the copper oxide or cuprous oxide in the copper to copper, ensuring that the hydrogen in the CVD vapor deposition process is used for the cracking of methane, rather than participating in the reduction of copper oxide or cuprous oxide.

[0096] In some embodiments, the volume flow rate of methane may be 5 sccm to 20 sccm, for example, 6 sccm to 18 sccm, 8 sccm to 16 sccm, 9 sccm to 15 sccm, 10 sccm to 13 sccm, 11 sccm to 12 sccm, etc. Within this rate range, methane is conducive to full contact with the metal particles 10 for carbonization reaction.

[0097] In some embodiments, the temperature of heating the metal mixture is 700°C to 1070°C, for example, 720°C to 1050°C, 750°C to 1000°C, 780°C to 950°C, 800°C to 900°C, 820°C to 880°C, etc. The time of heating the metal mixture is 50min to 110min, for example, 10min to 120min, 60min to 100min, 65min to 95min, 70min to 90min, 75min to 80min, etc. In this way, the methane and metal mixture can be fully carbonized to form the carbide layer 20.

[0098] It should be noted that, in some embodiments, the metal mixture may be heated first and then methane gas may be introduced; in other embodiments, methane may be introduced before heating; in yet another embodiment, methane gas may be introduced while the metal mixture is heated.

[0099] In some embodiments, the first intermediate body includes a metal mixture and a carbide layer 20 encapsulating the metal mixture.

[0100] In step S13:

[0101] It is understood that the graphene can be deposited using methods commonly used in the art. In at least one embodiment, the graphene is deposited using a CVD vapor deposition method to obtain the graphene layer 30 .

[0102] In some embodiments, after graphene is deposited on the surface of the first intermediate, cleaning and ultrasonic dispersion are also included. Cleaning is beneficial to remove the anti-sintering agent and ensure the purity of the powder, and ultrasonic dispersion is beneficial to the uniform distribution of graphene. The duration of cleaning and ultrasonic dispersion can be 30s to 120s, for example, 35s to 115s, 40s to 110s, 50s to 100s, 60s to 90s, 70s to 80s, etc.

[0103] In some embodiments, after washing and ultrasonic dispersion, filtering is further included. The filtering may be suction filtration. The filtering time may be 5 min to 20 min, for example, 6 min to 18 min, 7 min to 16 min, 8 min to 15 min, 9 min to 14 min, 10 min to 12 min, etc. By filtering, the composite conductor and the solvent used for washing can be separated.

[0104] Furthermore, drying is also included after filtering. The drying temperature can be 60°C to 150°C, for example, 65°C to 140°C, 70°C to 130°C, 75°C to 120°C, 80°C to 110°C, 90°C to 100°C, etc. The drying time can be 5min to 30min, for example, 6min to 28min, 7min to 25min, 8min to 22min, 9min to 20min, 10min to 15min, etc. The solvent on the composite conductor can be effectively removed by drying.

[0105] In a third aspect, an embodiment of the present application further provides an electrical contact element, which includes the above-mentioned composite conductor.

[0106] The electrical contact element provided in the present application contains a graphene layer 30. The uniform distribution of graphene can significantly improve the conductivity of the electrical contact element.

[0107] In some embodiments, a method for preparing an electrical contact element includes:

[0108] Step S21, providing the above-mentioned composite conductor and pressing it into an embryonic body;

[0109] Step S22: sintering the green body to obtain an electrical contact element.

[0110] The method for preparing the electrical contact element provided in the present application is simple and convenient to operate and has high conductivity.

[0111] In step S22:

[0112] In some embodiments, sintering the green body includes a first sintering and a second sintering.

[0113] In some embodiments, the temperature of the first sintering may be 400°C to 500°C, for example, 410°C to 490°C, 420°C to 480°C, 430°C to 470°C, 440°C to 460°C, 450°C to 455°C, etc. The pressure of the first sintering is 50KN to 200KN, for example, 60KN to 180KN, 70KN to 160KN, 80KN to 150KN, 90KN to 140KN, 100KN to 120KN, etc. The time of the first sintering may be 2min to 20min, for example, 3min to 18min, 5min to 16min, 6min to 15min, 8min to 14min, 10min to 12min, etc.

[0114] In some embodiments, the heating rate to the temperature of the first sintering can be 10℃ / min to 100℃ / min, for example, 20℃ / min to 90℃ / min, 30℃ / min to 80℃ / min, 40℃ / min to 70℃ / min, 50℃ / min to 60℃ / min, 52℃ / min to 55℃ / min, etc.

[0115] In some embodiments, the temperature of the second sintering may be 800°C to 950°C, for example, 810°C to 940°C, 820°C to 920°C, 830°C to 900°C, 840°C to 880°C, 850°C to 860°C, etc. The pressure of the second sintering is 200KN to 1200KN, for example, 300KN to 1100KN, 400KN to 1000KN, 500KN to 900KN, 600KN to 800KN, 700KN to 750KN, etc. The time of the second sintering may be 5min to 20min, for example, 6min to 18min, 7min to 16min, 8min to 15min, 9min to 14min, 10min to 12min, etc.

[0116] In some embodiments, the heating rate from the temperature of the first sintering to the temperature of the second sintering can be 10℃ / min to 100℃ / min, for example, 20℃ / min to 90℃ / min, 30℃ / min to 80℃ / min, 40℃ / min to 70℃ / min, 50℃ / min to 60℃ / min, 52℃ / min to 55℃ / min, etc.

[0117] It can be understood that when sintering the green body, the temperature is first raised to the temperature of the first sintering, and the first sintering is performed. After the first sintering is performed for a certain period of time, the temperature is further raised to the temperature of the second sintering, and the second sintering is performed. After the second sintering is performed for a certain period of time, the green body is cooled to obtain an electrical contact element. The first sintering temperature is low, which can prevent the rapid growth of grains and cause holes or bubbles in the green body. The second sintering is performed at a higher temperature, which can make the green body sintered densely and improve the conductivity, wear resistance and other performance properties.

[0118] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0119] Example 1

[0120] The present embodiment provides a composite conductor, which includes a copper alloy, a chromium carbide layer covering the copper alloy, and a graphene layer that completely covers the copper alloy and the chromium carbide layer; wherein the copper alloy includes copper and 2% chromium, 0.1% nickel, and 0.2% antimony; the coverage rate of the chromium carbide layer on the copper alloy is 50%, the thickness of the chromium carbide layer is 0.5 μm, the coverage rate of the graphene layer on the copper alloy and the chromium carbide layer is 100%, and the number of graphene layers is 5. The preparation method of the composite conductor is as follows:

[0121] 70 g of copper alloy powder and chromium were put into a ball mill for ball milling at a speed of 100 r / min in a clockwise direction for 30 min to obtain a metal mixture;

[0122] The metal mixture is uniformly mixed with 40 g of sintering-preventing agent magnesium oxide having an average particle size of 3 μm to obtain a mixed powder;

[0123] The mixed powder was heated under the protection of inert gas, and methane was introduced at a rate of 6 sccm. The carbonization reaction was carried out at 900°C for 40 minutes to coat the surface with a carbide layer.

[0124] Five graphene layers were deposited on the surface of the carbide-coated metal mixture by vapor deposition, and the mixture was repeatedly washed with deionized water and ultrasonically dispersed for 30 seconds. The mixture was then filtered and dried at 60°C for 5 minutes to obtain a composite conductor.

[0125] Accordingly, this embodiment further provides an electrical contact element, and the preparation method of the electrical contact element is as follows:

[0126] Putting the composite conductor into a mold and pressing it into an embryonic body;

[0127] The embryo body is sintered by first heating to 450°C, keeping the temperature for 10 minutes, and applying a pressure of 80 KN for the first sintering; then heating to 800°C, keeping the temperature for 15 minutes, and applying a pressure of 700 KN for the second sintering to obtain an electrical contact element.

[0128] Example 2

[0129] The present embodiment provides a composite conductor, which includes a copper alloy, a chromium carbide layer covering the copper alloy, and a graphene layer covering the copper alloy and the chromium carbide layer; wherein the copper alloy includes copper, 2.8% chromium, and 0.1% nickel; the coverage of the chromium carbide layer on the copper alloy is 50%, the thickness of the chromium carbide layer is 0.5 μm, the coverage of the graphene layer on the copper alloy core and the chromium carbide layer is 100%, and the number of graphene layers is 5. The preparation method of the composite conductor is as follows:

[0130] 70 g of copper alloy powder and chromium were put into a ball mill for ball milling, wherein the ball mill rotated at 300 r / min and ball milled clockwise for 300 min to obtain a metal mixture, wherein the thickness of chromium on the surface of the copper alloy was 0.8 μm;

[0131] The metal mixture is uniformly mixed with 40 g of sintering-preventing agent magnesium oxide having an average particle size of 3 μm to obtain a mixed powder;

[0132] The mixed powder was heated under the protection of inert gas, and methane was introduced at a rate of 6 sccm. The carbonization reaction was carried out at 900°C for 30 minutes to coat the surface with a carbide layer.

[0133] Five graphene layers were deposited on the surface of the carbide-coated metal powder by vapor deposition, and the powder was repeatedly washed with deionized water and ultrasonically dispersed for 30 seconds. The powder was then filtered and dried at 60°C for 5 minutes to obtain a composite conductor.

[0134] Accordingly, this embodiment further provides an electrical contact element, and the preparation method of the electrical contact element is as follows:

[0135] Putting the composite conductor into a mold and pressing it into an embryonic body;

[0136] The embryo body is sintered by first heating to 450°C, keeping the temperature for 10 minutes, and applying a pressure of 80 KN for the first sintering; then heating to 800°C, keeping the temperature for 15 minutes, and applying a pressure of 700 KN for the second sintering to obtain an electrical contact element.

[0137] Example 3

[0138] This embodiment is basically the same as Embodiment 2, except that, in this embodiment, the coverage rate of the chromium carbide layer on the copper alloy is 65%.

[0139] Example 4

[0140] This embodiment is basically the same as Embodiment 1, except that, in this embodiment, the coverage rate of the chromium carbide layer on the copper alloy is 80%.

[0141] Example 5

[0142] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the coverage rate of the graphene layer on the copper alloy and the chromium carbide layer is 90%.

[0143] Example 6

[0144] This embodiment is basically the same as Embodiment 1, except that, in this embodiment, the coverage rate of the graphene layer on the copper alloy and the chromium carbide layer is 95%.

[0145] Example 7

[0146] This embodiment is substantially the same as Embodiment 1, except that the thickness of the chromium carbide layer in this embodiment is 5 μm.

[0147] Example 8

[0148] This embodiment is substantially the same as Embodiment 1, except that the thickness of the chromium carbide layer in this embodiment is 10 μm.

[0149] Example 9

[0150] This embodiment is substantially the same as Embodiment 1, except that the number of graphene layers in this embodiment is 8.

[0151] Example 10

[0152] This embodiment is substantially the same as Embodiment 1, except that the number of graphene layers in this embodiment is 10.

[0153] Embodiment 11

[0154] This embodiment is substantially the same as Embodiment 1, except that the temperature of the carbonization reaction in this embodiment is 700°C.

[0155] Example 12

[0156] This embodiment is substantially the same as embodiment 1, except that the temperature of the carbonization reaction in this embodiment is 1040°C.

[0157] Example 13

[0158] This embodiment is substantially the same as embodiment 1, except that the carbonization reaction time in this embodiment is 10 minutes.

[0159] Embodiment 14

[0160] This embodiment is substantially the same as embodiment 1, except that the carbonization reaction time in this embodiment is 120 min.

[0161] Comparative Example

[0162] In this comparative example, copper alloy, chromium carbide and graphene are directly mixed to obtain a composite conductor.

[0163] The density of the composite conductors of Examples 1 to 14 and the comparative example was calculated by ρ=m / V; the hardness of the composite conductors of Examples 1 to 14 and the comparative example was measured by a Vickers hardness tester; the conductivity of the composite conductors of Examples 1 to 14 and the comparative example was tested by an AC bridge method. The results of the density, hardness and conductivity of the composite conductors of Examples 1 to 14 and the comparative example are shown in Table 1.

[0164] Table 1

[0165]

[0166]

[0167] As can be seen from Table 1, the density of the composite conductors of Examples 1 to 14 is slightly higher than that of the composite conductors of the comparative example. Generally, the denser the conductor, the better its electrical conductivity and thermal conductivity. Wear resistance is jointly restricted by multiple factors such as the thickness of the carbide layer, the coverage rate and the density of the conductor. The thicker the carbide layer and the wider the coverage, the lower the density of the conductor and the higher the wear resistance. The hardness of the composite conductor of the comparative example is less than 50HV, while the hardness of the composite conductors of Examples 1 to 14 is significantly higher than 50HV, indicating that the composite conductors prepared by the methods of Examples 1 to 14 solve the problem of easy precipitation of chromium during heating. In this scheme, part of the precipitated chromium reacts with methane to form a chromium carbide layer, which further improves the hardness of the composite conductor; the conductivity of the composite conductor of the comparative example is 68.94% IACS, and the conductivity of the composite conductor of Examples 1 to 14 is higher than 70% IACS. This is because the present scheme deposits graphene on the surface of the metal particles and the carbide layer, which is conducive to the uniform distribution of graphene and improves the conductivity of the composite conductor. In summary, the hardness and electrical conductivity of the composite conductors of Examples 1 to 14 are significantly higher than those of the composite conductor of the comparative example. The composite conductor provided by this solution fully utilizes the properties of carbide and graphene, and can simultaneously improve the hardness and electrical conductivity of the composite conductor.

[0168] The composite conductor and its preparation method and electrical contact element provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of ​​the present application. At the same time, for technicians in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite conductor, characterized in that: include: Metal particles; a carbide layer covering the metal particles; as well as A graphene layer covers the carbide layer and the metal particles.

2. The composite conductor according to claim 1, characterized in that: The coverage rate of the carbide layer on the metal particles is 50% to 80%; and / or The coverage rate of the graphene layer on the carbide layer and the metal particles is 90% to 100%.

3. The composite conductor according to claim 1, characterized in that: The average particle size of the metal particles is 10 μm to 100 μm; and / or The metal particles are copper alone or a copper alloy.

4. The composite conductor according to claim 3, characterized in that: The copper alloy includes one or more of copper-chromium alloy, copper-nickel alloy and copper-antimony alloy.

5. The composite conductor according to claim 1, characterized in that The material of the carbide layer includes one or more of chromium carbide, vanadium carbide and zirconium carbide; and / or The thickness of the carbide layer is 0.5 μm to 10 μm.

6. The composite conductor according to claim 1, characterized in that: The number of graphene layers is 5 to 10.

7. The composite conductor according to claim 1, characterized in that: The surface of the metal particles is also coated with a metal mixed layer.

8. The composite conductor according to claim 7, characterized in that: There are depressions on the surface of the metal particles, and the depth of the metal mixed layer embedded in the depression is 0.01 to 0.5 μm; and / or The metal mixed layer is a mixture of copper element and carbide precursor.

9. The composite conductor according to claim 8, characterized in that The carbide precursor includes one or more of chromium, vanadium pentoxide, vanadium trioxide, and zirconium dioxide; and / or The metal mixed layer also includes one or more of nickel and antimony.

10. A method for preparing a composite conductor, characterized in that: include: Providing metal particles, and mixing the metal particles with a carbide precursor by ball milling to obtain a metal mixture, wherein the metal mixture is metal particles coated with a metal mixing layer; heating the metal mixture and introducing methane to obtain a first intermediate; Graphene is deposited on the surface of the first intermediate to obtain a composite conductor.

11. The preparation method according to claim 10, characterized in that: The thickness of the metal mixed layer is 0.5 μm to 10 μm; and / or The coverage rate of the metal mixed layer on the metal particles is 50% to 80%; and / or There are depressions on the surface of the metal particles, and the depth of the metal mixed layer embedded in the depressions is 0.01 to 0.5 μm.

12. The preparation method according to claim 10, characterized in that: Before heating the metal mixture, the method further includes providing an anti-sintering agent to mix with the metal mixture.

13. The preparation method according to claim 12, characterized in that: The anti-sintering agent includes one or more of magnesium oxide, aluminum oxide, graphite, chromium, and silver; and / or The average particle size of the anti-sintering agent is 0.1 μm to 15 μm; and / or The mass ratio of the metal mixture to the anti-sintering agent is (5-10):

4.

14. The preparation method according to claim 10, characterized in that: The temperature of heating the metal mixture is 700° C. to 1070° C.; and / or The heating time of the metal mixture is 50 min to 110 min; and / or The volume flow rate of the methane is 5 sccm to 20 sccm.

15. An electrical contact element, characterized in that: The method for preparing the electrical contact element comprises: Providing the composite conductor according to any one of claims 1 to 9, pressed into an embryonic body; The green body is sintered to obtain an electrical contact element.

16. The electrical contact element according to claim 15, characterized in that The sintering of the embryonic body includes a first sintering and a second sintering; The temperature of the first sintering is 400° C. to 500° C., the pressure of the first sintering is 50KN to 200KN, and the time of the first sintering is 2min to 20min; The temperature of the second sintering is 800° C. to 950° C., the pressure of the second sintering is 200 KN to 1200 KN, and the time of the second sintering is 5 min to 20 min.