Preparation method and application of CTAB (Cetyltrimethyl Ammonium Bromide) regulated and controlled CuO / Cu2O nanoelectrode loaded with rGO layer

CuO/Cu2O nanoelectrode was prepared through the CTAB-regulated loaded rGO layer, which solved the problems of copper oxide electrode materials in the cycle stability and charge and discharge process, achieved high rate performance and good electrochemical performance, and significantly improved the ultracapacitor energy density.

CN119028739APending Publication Date: 2024-11-26NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310603780.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing copper oxide electrode materials have crystal defects, volume deformation and fracture problems during cycle stability and charge and discharge, resulting in a decrease in energy density and making it difficult to establish stable interactions on graphene support to improve ultraelectric performance.

Method used

The loaded rGO layer regulated by CTAB is used to prepare CuO/Cu2O nanoelectrodes by electrochemical deposition and hydrothermal method to form a new petal structure, which enhances the uniformity and dispersion of the material and improves conductivity and toughness.

Benefits of technology

The cycling stability and charge and discharge efficiency of the nanoelectrode are significantly improved, the specific capacitance is increased, and the high rate performance and good electrochemical performance are ensured, and the capacity attenuation is only 3.8% after 4,000 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028739A_ABST
    Figure CN119028739A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of an rGO layer loaded CuO / Cu2O nanoelectrode regulated and controlled by CTAB (cetyltrimethyl ammonium bromide), and can effectively solve the problems that the cycling stability is generally low, and a copper oxide material has crystal defects and is deformed in volume in the long-term cycling charge-discharge use process in the prior art. The rGO-CuO / Cu2O nano composite material with a novel structure is prepared by taking the rGO as a carrier and controlling the amount of a copper source under the regulation and control of a surfactant CTAB (Cetyltrimethyl Ammonium Bromide), the preparation method is simple, the cost is low, the operation is easy, and the rGO-CuO / Cu2O nano composite material with a relatively high surface area and volume ratio is constructed. The rGO-CuO / Cu2O nano-composite electrode material has the characteristics of high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance, high-temperature resistance and high
Need to check novelty before this filing date? Find Prior Art

Description

1. Technical Field

[0001] The invention relates to the technical field of electrocatalytic nanocomposite materials, in particular to a preparation method of a CuO / Cu2O nanoelectrode loaded with an rGO layer regulated by CTAB and an application thereof. 2. Background Technology

[0002] Supercapacitors (abbreviated as "supercapacitors") are currently the main energy storage and conversion devices. They have attracted much attention due to their high power density, long cycle life, high reliability and low maintenance costs, and are widely used in electronic devices, power supplies, electric vehicles and various microelectronic devices. In order to further improve the energy density of supercapacitors, researchers have developed and applied asymmetric flexible supercapacitors (FASCs), which have higher peak power density and have therefore received widespread attention.

[0003] As we all know, specific capacitance is an important parameter that affects superelectric performance. In order to improve the superelectric specific capacity, the electrode material must have a large activity and a large specific surface area, which can accommodate a large amount of electroactive substances to participate in the Faraday reaction. At present, transition metal oxides are the most widely studied superelectric electrode materials. Among transition metal oxides, copper oxide has become an ideal and practical material due to its excellent characteristics such as low price and high catalytic activity. Although copper oxide materials can show good capacitance performance in experimental studies, their inherent low conductivity reduces their charge and discharge cycle ability, and the cycle stability is generally low. In addition, during long-term cyclic charge and discharge use, copper oxide materials will have crystal defects and volume deformation, resulting in the breakage of copper oxide electrode materials and a rapid decrease in capacity. If you want to obtain an electrode material with good capacitance performance, good cycle stability and strong stability, you must improve the conductivity of the electrode material itself, increase the specific surface area and strengthen the toughness of the material.

[0004] Studies have shown that graphene-based nanoparticles exhibit better material properties in the overall medium. However, when copper oxide is used as a superelectric material, the addition of reduced graphene oxide (rGO) does not establish a stable interaction between the two and effectively improve the overall performance of the electrode. In order to increase the energy density of the superelectric, CuO and Cu2O are introduced together to the surface of the conductive carrier graphene to increase the area of ​​the active material. However, in most experiments, it was found that CuO-based composites often agglomerate during the preparation process. In summary, it is imperative to develop a high-performance electrode material for asymmetric flexible supercapacitors. III. Summary of the invention

[0005] In view of the above situation, in order to solve the defects of the prior art, the purpose of the present invention is to provide a preparation method and application of a CuO / Cu2O nanoelectrode loaded with an rGO layer regulated by CTAB, which can effectively solve the defects of the prior art, such as the generally low cycle stability, the occurrence of crystal defects and volume deformation of the copper oxide material during long-term cyclic charge and discharge use, resulting in the breakage of the copper oxide electrode material and the rapid decrease in capacity.

[0006] The technical solution provided by the present invention comprises the following steps:

[0007] 1) Weigh 30-32 mg of single-layer graphene into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 5-8 minutes, and then put it into an ultrasonic instrument at 50° C. for 2 hours to make it evenly dispersed to obtain solution A;

[0008] 2) Weigh 0.10g-0.30g of copper acetate into a small beaker, add 10ml of deionized water, dissolve under ultrasonic for 0.5h, then transfer to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, then slowly add surfactant CTAB to obtain solution B;

[0009] 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1), and continue stirring for 0.5-1h. After the stirring is completed, use a pipette to take 2.5mL of 2mol / L NaOH solution, add it to the above mixed solution, and continue stirring for 0.5h to obtain solution C;

[0010] 4) The C solution obtained in step 3) is transferred to a high-pressure reactor and maintained at 180° C. for hydrothermal reaction for 20 hours. After the reaction is completed, the precipitate is separated and repeatedly washed with anhydrous ethanol, deionized water, and anhydrous ethanol, and then placed in a vacuum drying oven at 60-80° C. for 24 hours to obtain the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB, which is labeled as rGO / Cu'-CTAB.

[0011] The invention discloses an application of the CTAB-regulated rGO-loaded CuO / Cu2O nanoelectrode in a flexible asymmetric supercapacitor.

[0012] The method for preparing the flexible asymmetric supercapacitor of the present invention comprises the following steps:

[0013] 1) Preparation of gel electrolyte: First, 2.0 g PVA was dissolved in 20 ml deionized water and stirred at 80 °C for 2 h. Then, 8.4 g KOH was dissolved in 20 ml deionized water and slowly dripped into the PVA solution. Stirring was continued until the colloidal solution became clear. Finally, the colloidal solution was placed at room temperature for 10 h to obtain a PVA / KOH gel.

[0014] 2) Assembling asymmetric flexible supercapacitor (rGO / Cu'-CTAB / / AC)@FASC: First, 0.04g of active material rGO / Cu'-CTAB, 0.04g of activated carbon (AC), 0.005g of polytetrafluoroethylene, and 0.005g of acetylene black were put into an agate mortar, and anhydrous ethanol was added to make it uniform and viscous. After grinding, a uniform slurry was obtained, and the slurry was evenly coated on the flexible carbon cloth to obtain the positive and negative electrodes (the coating area was controlled within 1cm 2 , the coating mass is controlled at 0.8-1.2 mg), the electrode is placed in a vacuum drying oven and dried at 80 ° C for 24 h, and then the PVA / KOH gel obtained in step 1) is evenly applied on the electrode, and the positive and negative electrodes are separated by a cellulose separator to avoid short circuit, thus obtaining an asymmetric flexible supercapacitor (rGO / Cu'-CTAB / / AC)@FASC.

[0015] The CTAB-regulated CuO / Cu2O nanoelectrode loaded with rGO layer prepared by the present invention exhibits a new hollow petal structure, has good uniformity and dispersibility, has good rate performance, good charge and discharge efficiency and more stable cyclability. In the process of preparing electrode materials, the addition of surfactant-cetyltrimethylammonium bromide (CTAB) plays a very important role in regulating the microstructure and surface morphology of the (CuO / Cu2O)@rGO nanocomposite material, which is an innovation in nanoelectrodes. IV. Description of the drawings

[0016] Figure 1 The present invention discloses the synthesis process and formation mechanism of the rGO-CuO / Cu2O nanoelectrode.

[0017] Figure 2 (a) XRD spectra of samples CuO, rGO / Cu' and rGO / Cu'-CTAB of the present invention, (b) FT-IR spectra of rGO-CuO / Cu2O and CuO at wavenumbers of 400-1800 / cm.

[0018] Figure 3 (a) XPS spectra of CuO and rGO-CuO / Cu2O of the present invention, (b and c) high-resolution spectra of C1s and Cu2p.

[0019] Figure 4TEM images of rGO-CuO / Cu2O of the present invention: (a, b and c) high magnification images at different positions, (d, e, f, g, h) are high magnification images of Figure b, and (i) X-ray energy spectrum.

[0020] Figure 5 (a) TG curve of the present invention - the inset is the phase composition calculated by the k-value method, (b) BET of rGO-CuO / Cu2O, the inset is the BJH pore size distribution.

[0021] Figure 6 The present invention shows (a) cyclic voltammetry (CV) curve at a scan rate of 0.3 mV / s, (b) CV of the sample rGO / Cu'-CTAB at different scan rates, (c) curves of the specific capacitance and capacitance retention of the sample rGO / Cu'-CTAB at different scan rates, and (d) cycle performance.

[0022] Figure 7 (a) The constant current charge-discharge curve of the rGO-CuO / Cu2O nanoelectrode at different current densities of the present invention, and (b) the rate curve of the electrode material.

[0023] Figure 8 The current density of the present invention is 2.5 mA / cm 2 Constant current charge and discharge curve during the cycle.

[0024] Fig. 9 (a) Electrode impedance characteristics of the present invention, the inset is the electrode equivalent circuit, (b) logi-logv curve, (c) CV curve of energy storage process and diffusion-controlled electrochemical process contribution diagram at a scanning rate of 0.5 mV / s, (d) surface-controlled capacitance process contribution diagram at different scanning rates.

[0025] Fig.10 (a) Schematic diagram of FASC assembly, (b) CV values ​​of AC and rGO / Cu'-CTAB, (c) CV and GCD curves of FASC under different voltages at a constant scan rate of 1.5 mV / s and different current densities, (e) CV value, (f) specific capacitance value, (g) 4000 cycle stability test of FASC device, (h) Nyquist impedance curve of FASC device. V. Specific implementation methods

[0026] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0027] Example 1

[0028] The present invention, when implemented, comprises the following steps:

[0029] 1) Weigh 30 mg of single-layer graphene and put it into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 5 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A;

[0030] 2) Weigh 0.10 g of copper acetate into a small beaker, add 10 ml of deionized water, and dissolve under ultrasonication for 0.5 h. Then transfer the solution to a magnetic stirrer, drop 4 ml of concentrated ammonia water, continue stirring for 1.5 h, and then slowly add the surfactant CTAB into the solution to obtain solution B;

[0031] 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1), and continue stirring for 0.5 h. After the stirring is completed, use a pipette to take 2.5 mL of a 2 mol / L NaOH solution, add it to the above mixed solution, and continue stirring for 0.5 h to obtain a solution C;

[0032] 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180° C. for reaction for 20 h, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 60° C. for 24 h, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

[0033] Example 2

[0034] The present invention, when implemented, comprises the following steps:

[0035] 1) Weigh 31 mg of single-layer graphene and put it into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 6 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A;

[0036] 2) Weigh 0.20g of copper acetate into a small beaker, add 10ml of deionized water, and dissolve under ultrasonication for 0.75h. Then transfer the solution to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, and then slowly add the surfactant CTAB into the solution to obtain solution B;

[0037] 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1), and continue stirring for 0.5 h. After the stirring is completed, use a pipette to take 2.5 mL of a 2 mol / L NaOH solution, add it to the above mixed solution, and continue stirring for 0.5 h to obtain a solution C;

[0038] 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180° C. for reaction for 20 h, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 70° C. for 24 h, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

[0039] Example 3

[0040] The present invention, when implemented, comprises the following steps:

[0041] 1) Weigh 32 mg of single-layer graphene and put it into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 8 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A;

[0042] 2) Weigh 0.30g of copper acetate into a small beaker, add 10ml of deionized water, and dissolve by ultrasonic for 0.5h. Then transfer the solution to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, and then slowly add the surfactant CTAB into the solution to obtain solution B;

[0043] 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1), and continue stirring for 1 hour. After the stirring is completed, use a pipette to take 2.5 mL of a 2 mol / L NaOH solution, add it to the above mixed solution, and continue stirring for 0.5 hour to obtain a solution C;

[0044] 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180° C. for reaction for 20 h, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 80° C. for 24 h, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

[0045] The present invention prepares rGO-CuO / Cu2O nanoelectrode material by electrochemical deposition combined with hydrothermal synthesis, and the process flow and mechanism are as follows: Figure 1 As shown. Among them, CTAB converts the positively charged CTA in the solution + Ionization, CTA + Adsorbed on the GO surface, interacting with GO anions and OH - At the same time, adding excess NaOH solution can replace a large amount of Cu 2+ ions, oxygen-containing groups in graphene oxide react with reducing [Cu(NH3)4] 2+The ions react in situ to form CuO nanocrystals, and then under heating reaction conditions, graphene oxide is converted into [Cu(NH3)4] 2+ ions and NaOH reduction to remove a large number of oxygen-containing groups on its surface to form redox graphene (rGO), and finally obtain rGO-CuO / Cu2O nanocomposite materials.

[0046] Subsequently, the nanoelectrode material was subjected to morphological analysis, cyclic voltammetry test, constant current charge-discharge test and AC impedance test. The results showed that the rGO-CuO / Cu2O nanoelectrode material exhibited a new type of composite structure, namely, flaky Cu2O and single crystal stacked hollow petal-shaped CuO, with good uniformity and dispersion. Electrochemical tests showed that at a current density of 2.5 mA / cm 2 It has a specific capacitance of up to 852F / g. The composite electrode was then subjected to 4000 cycles of charge and discharge tests, and it was found that the specific capacitance only decayed by 3.8%, with good rate performance, good charge and discharge efficiency, and more stable cyclability. Finally, the effect of the amount of copper acetate added on the capacitance performance of the composite material was also explored. The final comparison found that the copper oxide prepared by still using 0.20g of copper acetate loaded on graphene has more outstanding capacitance performance and can show better electrochemical performance in superelectric. The relevant experimental data are as follows:

[0047] 1. Experimental materials and procedures

[0048] Graphene, copper acetate, concentrated ammonia (25-28%), acetone, concentrated hydrochloric acid, sodium hydroxide, potassium hydroxide, anhydrous ethanol, deionized water (self-made in the laboratory), all reagents are analytically pure. The electrochemical experiment uses a three-electrode system, that is, a platinum sheet electrode, a saturated calomel electrode, and a nickel foam coated with electrode materials as the reference electrode, auxiliary electrode, and working electrode, respectively. Connect the alligator clip and fix it in a 50ml beaker. Then select the electrochemical test technology and set the parameters.

[0049] 2. Experimental Methods

[0050] Before the electrochemical experiment, the working electrode was prepared. Then it was placed in a 1mol / LKOH alkaline electrolyte solution and activated at a scan rate of 10mV / s at -1 to 1V to determine the specific potential window; then the nickel foam electrode was subjected to a cyclic voltammetry scan to analyze the effect of the scan rate on the entire medium. Finally, a constant current charge and discharge test was performed to obtain the capacitance at different scan rates. The water used in the experiment was homemade by the laboratory water purification system, and the entire experiment was carried out at room temperature.

[0051] 1. Characterization of rGO-CuO / Cu2O Electrode

[0052] (1) XRD. The crystal structure of the sample was characterized by X-ray diffractometer. Figure 2 (a) is the XRD spectrum of nanostructured samples CuO, rGO / Cu' and rGO / Cu'-CTAB composite materials. The diffraction peaks of the experimentally prepared CuO material are easily matched with the standard XRD pattern of CuO with monoclinic structure (JCPDS No.48-1548). The diffraction peaks of the sample at 2θ=32.5°, 35.5°, 38.7°, 48.7°, 53.5°, 58.3°, 61.5°, 66.4°, 68.1°, 72.4°, and 75.2° correspond to the characteristic peaks of the (110) (11-1) (111) (20-2) (020) (202) (11-3) (310) (220) (311) (22-2) crystal planes, and the diffraction peaks are thin and long, indicating that the CuO material has a high degree of crystallinity. And there is a peak at the angle 2θ = 26.6°, corresponding to the characteristic peak (002) of the C crystal plane, which belongs to rGO. In addition, based on the reflection of the (110) crystal plane of CuO, the crystallinity of the sample rGO / Cu'-CTAB is greater than that of rGO / Cu'; the trace Cu2O peak is blocked behind the CuO crystal plane and is located in the surface area of ​​the CuO nanoparticles. It is worth noting that the XRD pattern has no impurity peaks of other substances, indicating that the synthesized rGO-CuO / Cu2O nanocomposite material has high purity and crystallinity.

[0053] (2) FT-IR. Figure 2 (b) is the spectrum of CuO and rGO-CuO / Cu2O nanocomposites. Compared with the absorption peak of pure CuO (a), the composite material synthesized by adding GO (b) has an additional absorption peak at 1590 / cm caused by the vibration of the C=C bond. After graphite oxidation, the polar groups will increase significantly. After the hydrothermal reaction, graphene oxide is reduced to rGO, causing the oxygen group (C=O and CO) absorption band of graphene oxide to disappear. It also proves that there are hydroxyl groups on the surface of GO, which makes it easy to form hydrogen bonds with water molecules. Therefore, GO exhibits good hydrophilicity. During the hydrothermal reaction, due to "thermal expansion and contraction", the 3D mesh pores are expanded, resulting in more specific surface area, which is more conducive to the loading of rGO and CuO / Cu2O together, and enhancing the electrochemical activity.

[0054] (3) XPS. In order to study the chemical composition of the final product and the oxidation state of copper in more detail, XPS was used to characterize the preparation of the CuO@rGO composite material. Figure 3As shown in (a), the peaks of Cu2p, O1s and C1s are clearly present. However, in the rGO-CuO / Cu2O composite, the dominant peak is caused by the CO bond in rGO. The surrounding small peaks are accompanied by the breaking and combination of C=O and CC bonds, indicating that the C in rGO is mainly composed of different bonding forms such as aromatic rings, hydroxyl groups, carboxyl groups and epoxy groups. Figure 3 The high-resolution C1s shown in (b) is caused by the CC, CO and C=O bonds of reduced graphene, and the binding energies of the peaks are 284.2 eV, 285.8 eV and 287.8 eV, respectively. Figure 3 (c) It can be seen that two obvious Cu2p 1 / 2 Corresponding to 953.7eV and 952.7eV, two Cu2p 3 / 2 The oscillation satellite peaks at 933.7eV, 932.40eV and 941.9eV can be attributed to Cu2p3 / 2. According to the peaking results of rGO-CuO / Cu2O, the material contains a small amount of Cu + , proving the presence of a small amount of copper(I) oxidation state in the material.

[0055] (4) TEM. To further prove whether CuO is successfully modified on graphene, the TEM morphology of CuO@rGO is shown in Figure 4. Figure 4 As shown in Figure 2, the surface of rGO presents a typical carbon layer, similar to a thin and transparent silk yarn folded together. Figure 4 (cg, regulated by CTAB) It can be seen that CuO is evenly distributed on the outside and inside of the rGO layer, and is composed of single square crystals stacked into a petal structure with a central hole. In addition, Figure 4 (b, without adding CTAB) shows that CuO has good crystallinity and a smooth surface, and its single crystal diameter is about 150nm; Figure 4 As shown in (h), the CuO coated inside the graphene is surrounded by some very small granular crystals. The results obtained by transmission electron microscopy are consistent with those obtained by XPS detection; the crystal defects appearing in the flake CuO molecules are as follows: Figure 4 As shown in (f), crystal defects appear in the CuO flake molecules, which are attributed to the interaction between the oxygen-containing groups in graphene and the copper salt solution to generate Cu 2+ When Cu + There is a certain degree of incomplete oxidation, which eventually leads to Cu + Replace trace Cu 2+ space, while also reducing the overall crystal plane spacing. Figure 4 The X-ray energy dispersive spectrometry analysis of (i) shows the presence of Cu, O and C elements, which is consistent with the XRD measurement results.

[0056] 2. TGA, BET and BJH detection of nano-rGO-CuO / Cu2O electrode

[0057] In a nitrogen atmosphere, the temperature was raised from room temperature to 800°C at a rate of 20°C / min. The thermogravimetric analysis (TGA) curve was as follows: Figure 5 When the temperature rises to 348 °C, the first weight loss zone appears. Since it is close to the melting point of CTAB, it can be considered to correspond to the decomposition of adsorbed CTAB. The subsequent weight loss is due to the thermal reduction of reduced graphene oxide, which causes changes in the ions in the medium and produces Cu 2+ and Cu + .from Figure 5 b It can be seen that the N2 isotherm of the rGO-CuO / Cu2O nanocomposite material presents a typical IV curve form, and an adsorption hysteresis loop with a convex middle appears after the isotherm, indicating that the material has a mesoporous structure.

[0058] The present invention also uses the Brunauer-Emmett-Taylor (BET) method to measure the specific surface area of ​​the rGO-CuO / Cu2O nanocomposite material. The pore size distribution curve is as follows: Figure 5 As shown, the specific surface area of ​​the porous composite material is estimated to be 232 m 2 / g. Figure 5 (b) shows that the rGO-CuO / Cu2O nanocomposite has an adsorption hysteresis loop in the middle convex part after the isotherm, indicating the presence of mesoporous material according to the IUPAC classification, which is attributed to the thermal decomposition change of the oxide precursor to form a pore structure. Figure 5 (b) Inset - The pore size distribution was determined using the Barrett-Joyner-Halenda (BJH) method and was found to be centered at 5 nm with a pore volume of 0.333 cm 3 / g.

[0059] In summary, the prepared material has a larger specific surface area, and the AC contact performance of CuO / Cu2O and rGO is stronger, which can participate in the electrochemical reaction more fully. In addition, the graphene with a 3D network structure as a carrier has more reaction sites, so during the charge and discharge process, the penetration of the electrolyte into the electrode material will be greatly increased, which is conducive to achieving high rate capacity.

[0060] 3. Cyclic voltammetry test of sample materials

[0061] Figure 6(a) is the cyclic voltammetry curves of the three groups of samples in 1 mol / L KOH electrolyte, and the test scan rate and potential window are set to 0.3 mV / s and 0-0.575 V, respectively. The CV curves of rGO / Cu'-CTAB and rGO / Cu' are almost uniform and symmetrical, and the electron transfer is reversible. When the rGO / Cu'-CTAB sample is used, the oxidation current obtains a fast voltammetric response at 0.45 V, and its significant negative shift exceeds 0.02 V compared with rGO / Cu'. Therefore, the effect of CTAB-regulated rGO-CuO / Cu2O nanocomposites on the electrochemical performance is more significant. Compared with CuO and rGO / Cu', the scanning window range of rGO / C'-CTAB is widened, indicating that it has superior electrocatalytic reaction under 0.1 mol-1 KOH. Meanwhile, two clear reduction peaks were observed at 0.23 V and 0.35 V, the peak at 0.35 V was associated with the formation of CuO phase, while the peak at 0.23 V corresponded to the reduction of Cu2O to solid solution phase.

[0062] Figure 6 (b) is the CV curve of rGO / Cu'-CTAB nanocomposite at different scan rates. When the scan rate increases from 0.1mV / s to 1.0mV / s, the shape does not change significantly, and loading CuO / Cu2O on graphene will produce a larger pseudocapacitance.

[0063] according to Figure 6 (c), when the scan rate is 0.1mV / s, the specific capacitance reaches 1354F / g. When the scan rate is increased to 10 times, the specific capacitance is close to 979.2F / g, and the capacity can still reach more than 72% of the maximum value. This shows that with the increase of the scan rate, the rGO-CuO / Cu2O electrode also has excellent capacitance stability. Figure 6 (d) Samples rGO / CuO, rGO / Cu' and rGO / Cu'-CTAB at a current density of 2.5 mA / cm 2 The specific capacity curve at the time of charge and discharge, the specific capacitance increases continuously in the first 2000 cycles of charge and discharge cycles. The rGO-CuO / Cu2O electrode prepared in this experiment requires an additional 2000 charge and discharge cycles to be fully activated. It can be seen that the CTAB-controlled rGO-CuO / Cu2O material has the best recycling ability. After 3000 cycles, the capacity remains good and the capacity loss is not obvious. After 2000 charge and discharge cycles, the specific capacitance of the test sample rGO / Cu'-CTAB reaches the highest capacity of 1392F / g, and the specific capacitance begins to slowly decrease at 2200 cycles. When the cycle reaches 3000 times, the specific flow capacity is 1258F / g. This shows that: with the increase of scan rate, the rGO-CuO / Cu2O electrode still has excellent capacitance stability and superelectric performance.

[0064] 4. Constant current charge and discharge test of sample materials

[0065] Figure 7 (a) is the constant current charge-discharge curve. The potential window corresponding to the electrodes of the three groups of sample materials is 0.05-0.575 V, and the current density is 2.5 mA / cm 2 . As can be seen from the figure, the charging curve consists of two segments. That is, in the voltage range of 0.05-0.4V, the voltage and charging time show a good linear relationship, and this segment of the curve can be expressed as a double-layer capacitance; when the voltage range is 0.4-0.575V, the curve shows a nonlinear relationship, and a Faraday pseudocapacitance reaction occurs, which can be attributed to the capacitance of the CuO@rGO electrode material coming from the double-layer capacitance and the Faraday pseudocapacitance, and can be used as an electrode material for asymmetric hybrid superelectrics. In addition, with the addition of Cu2O and CTAB, the charging time of the capacitor tends to increase; compared with the other two groups of materials, the charging time of the rGO / Cu'-CTAB electrode is longer. The discharge time of rGO / Cu'-CTAB is much longer than that of CuO and rGO / Cu', that is, the corresponding specific capacitance is also larger.

[0066] Figure 7 (b) shows the enlarged curves of the two groups of materials. As the current density increases, the specific capacitance decreases. It is worth noting that at 40 mA / cm 2 At high current density, the retention rate of specific capacitance exceeds 70%. This shows that with the increase of current density, rGO / Cu'-CTAB still has good rate performance. When using a small current discharge, the specific capacitor will have better storage capacitance performance, greatly improve the utilization rate of electrode materials, and make the charge and discharge state more stable.

[0067] 5. Cyclic specific capacitance test of rGO-CuO / Cu2O nanoelectrode

[0068] Figure 8 The rGO-CuO / Cu2O electrode material has a current density of 2.5 mA / cm 2 As the number of cycles increases, no capacitance decay is observed, and the coulombic efficiency of each cycle of charge and discharge is almost 100%. This shows that rGO-CuO / Cu2O has a certain cycle stability as an electrochemical pseudocapacitor electrode material. Figure 6(d), in the first 250 cycles of charge and discharge, the specific capacitance did not decrease, but gradually increased from 430F / g to 852F / g. This is because among many metal oxides, CuO has strong chemical inertness and stable chemical properties, so it must be activated by charge and discharge cycles for a period of time before its electrochemical properties can be fully released. Therefore, the prepared rGO-CuO / Cu2O electrode needs to be fully activated by additional 250 cycles of charge and discharge cycles. When the cycle reaches 2000, it only decays by 3.8% compared with the maximum value, showing good cycle stability.

[0069] VI. Electrochemical reaction kinetics test of RGO / Cu'-CTAB

[0070] Fig. 9 (a) Electrochemical impedance spectroscopy (open circuit voltage 0.1 V, frequency range 10 -2 ~10 5 Hz), the inset is the equivalent circuit diagram of the working electrode (where R Ω is the solution resistance, Cd1 and Cd2 represent the capacitance and the impedance caused by the migration of ions in the electrode respectively; R ct Including the pseudocapacitive charge transfer resistance occurring on the electrode and the diffusion resistance in the low-frequency region). The high-frequency region of the Nyquist curves of all electrodes has a small semicircle, proving that the electrode has a lower charge transfer resistance. The CTAB-regulated rGO / Cu' has the smallest internal impedance and charge transfer impedance, making ion conduction easier. In addition, combining the characteristics of the high-frequency region and the low-frequency region, the rGO / Cu'-CTAB electrode has better electrochemical reaction kinetics.

[0071] To analyze the charge storage dynamics of the rGO / Cu'-CTAB electrode, the capacitive contribution of the electrode was further investigated using CVs. Fig. 9 (b) shows the logi-logv relationship of rGO / Cu'-CTAB. From the slope of curve K, we can see that the b values ​​of the electrodes are 0.540 and 0.414, corresponding to the oxidation peak current and reduction peak current, respectively, indicating that the capacitive energy storage process is mainly dominated by the diffusion-controlled electrochemical process. Fig. 9 As shown in (c), at 0.5 mV / s, the surface-controlled capacitance process of rGO / Cu'-CTAB accounts for 61.4% (shaded area). Fig. 9(d) is the ratio of the surface-controlled capacitance process to the diffusion-controlled electrochemical process at different scanning speeds. At 0.1, 0.2, 0.3, 0.5 and 1.0 mV / s, the ratio of the electrode surface-controlled capacitance process is 49%, 55%, 58%, 61% and 75%, respectively. The contribution rate of the surface-controlled capacitance process increases with the increase of the scanning speed, that is, the redox reaction and charge adsorption / desorption rate on the electrode surface are faster, and rGO / Cu'-CTAB has excellent capacitance performance.

[0072] VII. Electrochemical Performance Measurement of Flexible Asymmetric Supercapacitors

[0073] In order to further evaluate the practical application of rGO / Cu'-CTAB, the present invention assembled an asymmetric flexible supercapacitor and tested its electrochemical performance. To optimize the electrochemical performance of FASC and establish a reliable potential window, CV ( Fig.10 c) and GCD( Fig. 9 d). The GCD curve is approximately a symmetrical triangle, with good reversibility. The FASC curve does not change significantly in shape, with good reversibility and charge-discharge capability ( Fig.10 e).

[0074] In addition, at 2.5 mA / cm 2 and 40mA / cm 2 At current values ​​of 1.34 F / g, FASC provides high specific capacitances of 98.62 F / g and 71.34 F / g ( Fig.10 f), indicating that when the current increases 10 times, the capacitance retention rate is 72.3%. Fig.10 g, at 2.5 mA cm -2 The cycling stability of the flexible (rGO / Cu'-CTAB / / AC)@FASC was tested at a high current density of 4000. After constant current charge and discharge, the specific capacitance value can be maintained at about 94.8%, showing good cycling stability. Fig.10 h describes the Nyquist impedance diagram of (rGO / Cu'-CTAB / / AC)@FASC. According to the intercept of the curve with the horizontal axis in the figure, the equivalent series resistance is 0.275Ω. The semicircle diameter in the high-frequency region is small, and the slope of the straight line in the low-frequency region is large, indicating that (CuO@rGO / / AC)@FASC regulated by CTAB has a small charge transfer resistance and ion diffusion resistance.

[0075] In summary, the present invention adopts electrochemical precipitation-hydrothermal method, under the regulation of surfactant CTAB, assisted by the synergistic effect of CuO and Cu2O, rGO is used as the carrier of CuO, and the amount of copper source is controlled to prepare rGO-CuO / Cu2O nanocomposite materials with novel structure.2 At a current density of , the capacity retention rate after 4000 charge and discharge cycles is 88.3%. The preparation method of the present invention is simple, low-cost, and easy to operate. A nanocomposite electrode material with a high surface area to volume ratio and the characteristics of 3D mesh structure graphene with strong loading capacity is constructed. Through electrochemical testing, the rGO-CuO / Cu2O electrode exhibits good pseudocapacitive characteristics, good rate performance, and long-lasting charge and discharge cycle performance. It has great application value in selecting electrode materials, is an innovation in nanoelectrodes, and has significant social and economic benefits.

[0076] It should be pointed out that the above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession can make changes or modify the technical contents disclosed above into equivalent embodiments with equivalent changes without departing from the scope of the technical solution of the present invention, which all fall within the protection scope of the present invention.

Claims

1. A method for preparing a CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB, characterized in that: The following steps are involved: 1) Weigh 30-32 mg of single-layer graphene into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 5-8 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A; 2) Weigh 0.10g-0.30g of copper acetate into a small beaker, add 10ml of deionized water, dissolve under ultrasonic for 0.5h, then transfer to a magnetic stirrer, drop 4mm concentrated ammonia water, continue stirring for 1.5h, then slowly add surfactant CTAB to obtain solution B; 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1) and continue stirring for 0.5-1h. After the stirring is completed, use a pipette to transfer 2.5mL of 2mol / L NaOH solution, add it to the above mixed solution and continue stirring for 0.5h to obtain solution C; 4) The solution C obtained in step 3) is transferred to a high-pressure reactor and maintained at 180° C. for hydrothermal reaction for 20 hours. After the reaction is completed, the precipitate is separated and repeatedly washed with anhydrous ethanol, deionized water, and anhydrous ethanol, and then placed in a vacuum drying oven at 60-80° C. for 24 hours to obtain the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB, which is labeled as rGO / Cu'-CTAB.

2. The method for preparing the CTAB-regulated rGO-loaded CuO / Cu2O nanoelectrode according to claim 1, characterized in that: The following steps are involved: 1) Weigh 30 mg of single-layer graphene and put it into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 5 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A; 2) Weigh 0.10g of copper acetate into a small beaker, add 10ml of deionized water, and dissolve by ultrasonic for 0.5h. Then transfer the solution to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, and then slowly add the surfactant CTAB into the solution to obtain solution B; 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1) and continue stirring for 0.5 h. After the stirring is completed, use a pipette to transfer 2.5 mL of 2 mol / L NaOH solution, add it to the above mixed solution and continue stirring for 0.5 h to obtain solution C; 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180°C for reaction for 20 hours, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 60°C for 24 hours, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

3. The method for preparing the CTAB-regulated rGO-loaded CuO / Cu2O nanoelectrode according to claim 1, characterized in that: The following steps are involved: 1) Weigh 31 mg of single-layer graphene into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 6 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A; 2) Weigh 0.20g of copper acetate into a small beaker, add 10ml of deionized water, and dissolve under ultrasonic for 0.75h. Then transfer the solution to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, and then slowly add the surfactant CTAB into the solution to obtain solution B; 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1) and continue stirring for 0.5 h. After the stirring is completed, use a pipette to transfer 2.5 mL of 2 mol / L NaOH solution, add it to the above mixed solution and continue stirring for 0.5 h to obtain solution C; 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180°C for reaction for 20 hours, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 70°C for 24 hours, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

4. The method for preparing the CTAB-regulated rGO-loaded CuO / Cu2O nanoelectrode according to claim 1, characterized in that: The following steps are involved: 1) Weigh 32 mg of single-layer graphene into a 100 ml beaker, add 25 ml of distilled water and 10 ml of DMF, stir with a glass rod for 8 minutes, and then put it into an ultrasonic instrument at 50°C for 2 hours to make it evenly dispersed to obtain solution A; 2) Weigh 0.30g of copper acetate into a small beaker, add 10ml of deionized water, and dissolve by ultrasonic for 0.5h. Then transfer the solution to a magnetic stirrer, drop 4ml of concentrated ammonia water, continue stirring for 1.5h, and then slowly add the surfactant CTAB into the solution to obtain solution B; 3) Slowly add the solution B obtained in step 2) into the solution A obtained in step 1) and continue stirring for 1 hour. After the stirring is completed, use a pipette to transfer 2.5 mL of 2 mol / L NaOH solution, add it to the above mixed solution and continue stirring for 0.5 hour to obtain solution C; 4) The solution C obtained in step 3) was poured into the lining of a high-temperature and high-pressure reactor, placed in an oven at 180°C for reaction for 20 hours, and then the precipitate was repeatedly rinsed with anhydrous ethanol, deionized water and anhydrous ethanol in sequence, and finally dried in a vacuum drying oven at 80°C for 24 hours, and the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB was collected and labeled as rGO / Cu'-CTAB.

5. Application of the CuO / Cu2O nanoelectrode loaded with rGO layer regulated by CTAB prepared by the preparation method according to any one of claims 1 to 4 in a flexible asymmetric supercapacitor.

6. The method for preparing the flexible asymmetric supercapacitor according to claim 5, characterized in that: The following steps are involved: 1) Preparation of gel electrolyte: First, 2.0 g PVA was dissolved in 20 ml deionized water and stirred at 80 °C for 2 h. Then, 8.4 g KOH was dissolved in 20 ml deionized water and slowly dripped into the PVA solution. The solution was stirred continuously until the colloidal solution became clear. Finally, the colloidal solution was placed at room temperature for 10 h to obtain a PVA / KOH gel. 2) Assembling asymmetric flexible supercapacitor (rGO / Cu'-CTAB / / AC)@FASC: First, 0.04g of active material rGO / Cu'-CTAB, 0.04g of activated carbon, 0.005g of polytetrafluoroethylene, and 0.005g of acetylene black were placed in an agate mortar, and anhydrous ethanol was added to make a uniform viscous state. The mixture was fully ground to obtain a uniform slurry, which was evenly coated on the flexible carbon cloth. The coating area was controlled to be 1cm 2 , the coating mass is controlled at 0.8-1.2 mg, the positive and negative electrodes are obtained, the electrodes are placed in a vacuum drying oven, dried at 80 ° C for 24 h, and then the PVA / KOH gel obtained in step 1) is evenly applied on the electrodes, and the positive and negative electrodes are separated by a cellulose separator to avoid short circuit, and the asymmetric flexible supercapacitor (rGO / Cu'-CTAB / / AC)@FASC is obtained.