Preparation method of hybrid lithium ion supercapacitor

The positive electrode material is prepared by solid phase mixing, airflow crushing, subsonic cold spraying, and combined with vacuum evaporation and electrolyte, the uneven distribution and low density problems in the preparation of positive and negative electrode materials of mixed lithium-ion supercapacitors are solved. Improves energy density and cycle stability, simplifies process and reduces costs.

CN119028740AInactive Publication Date: 2024-11-26JIANGXI FUJING ELECTRONICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411225352.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the preparation process of existing hybrid lithium-ion supercapacitors, there are problems such as poor dispersion of specific surface area, low powder compaction density, uneven particle size distribution and inconsistent charge and discharge capacity, which affects its energy storage stability.

Method used

The solid phase mixing method is used to mix ternary lithium batteries, hard carbon and conductive carbon with binder, and the positive electrode material is prepared by air flow pulverization and subsonic cold spraying method, and the negative electrode material is prepared by vacuum evaporation method, and electrolysis is used in capacitor assembly. Liquid and hydroxyapatite agents optimize material distribution and density.

Benefits of technology

It realizes solvent-free operation, improves material utilization and cost-effectiveness, accurately controls the size and thickness of the positive electrode, improves capacity and energy density, enhances cycle stability and high temperature reliability, simplifies the preparation process and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028740A_ABST
    Figure CN119028740A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a hybrid lithium ion supercapacitor, and the hybrid lithium ion supercapacitor mainly comprises a positive electrode, a negative electrode, a diaphragm and an electrolyte between the positive electrode and the negative electrode, and a housing. The positive electrode material comprises an active material, conductive carbon and a binder, wherein the active material comprises a ternary lithium battery material and hard carbon. The preparation method comprises the following steps: firstly, carrying out solid-phase mixing on the active material, the conductive carbon and the PVDF; secondly, mixing and fiberizing by using a binder in a jet milling manner; according to the invention, by optimizing the preparation of the positive and negative electrode materials and redesigning the electrode / electrolyte assembly, the supercapacitor has the advantages of high energy density, power density, safety and long cycle service life, the labor cost is reduced, and the controllable excellent electrode material preparation method is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of layered positive electrode materials, and in particular to a method for preparing a hybrid lithium ion supercapacitor. Background Art

[0002] Hybrid lithium-ion supercapacitors are a new type of electrochemical energy storage device with the characteristics of high energy density and high power density. They are widely used in electric vehicles, energy storage systems and other fields. Traditional lithium-ion batteries have become the mainstream energy storage device due to their high energy density and long charge and discharge cycles, but they often have problems such as slow charge and discharge speeds and short life. In comparison, supercapacitors have the advantages of fast charge and discharge speeds and long life, but their energy density is relatively low. In order to overcome the shortcomings of traditional lithium-ion batteries and supercapacitors, researchers began to explore hybrid lithium-ion supercapacitors. Hybrid lithium-ion supercapacitors combine the high energy density of lithium-ion batteries and the high power density of supercapacitors, while having longer charge and discharge cycles and faster charge and discharge speeds.

[0003] In the existing preparation process of positive and negative electrode materials of hybrid lithium-ion supercapacitors, there are still major problems in processing and performance: the specific surface area is not easy to disperse, the compaction density of the powder is low, the particle size distribution is uneven, and there is inconsistent capacity during the charge and discharge process. The published patent CN105355872A reported that polyacrylonitrile and transition metal nitrate were first mixed in a mass ratio of 1:1, and then the raw silk fiber was obtained by electrostatic spinning, and the carbon-based lithium-ion electrode material was obtained after carbonization. It was found in the experiment that transition metal oxides are easy to agglomerate, the active sites cannot be fully exposed, and the active sites of the carbonized materials are limited, which seriously affects its energy storage stability. At present, the preparation process of traditional hybrid lithium-ion supercapacitor positive and negative electrode materials is complicated and the specific capacity is low. It is urgent to improve the preparation process, and prepare a method for uniformly distributing positive and negative electrode materials while simplifying the steps to obtain a hybrid lithium-ion supercapacitor with good energy storage performance. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing a hybrid lithium-ion supercapacitor, so as to solve the problems raised in the above background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution:

[0006] The present invention provides a method for preparing a hybrid lithium-ion supercapacitor, comprising the following steps:

[0007] Step 1: Preparation of positive electrode materials: solid phase mixing of ternary lithium battery, hard carbon, conductive carbon and binder; secondly, mixing and binder fiberization by air flow milling; then, obtaining electrode sheets on substrates by subsonic cold spraying;

[0008] Step 1: Under vacuum conditions, the metal material is placed into a vacuum coating machine, the temperature is raised to a certain level to vaporize the metal directly, and the metal ions fly to the surface of the substrate and condense into a film of a certain thickness to obtain the negative electrode material;

[0009] Step 2: Capacitor assembly: prepare the positive electrode material, negative electrode material, diaphragm, and electrolyte, and pre-soak the positive electrode material and diaphragm in the electrolyte to fully soak them;

[0010] The metal-film coated negative electrode shell, diaphragm, positive electrode sheet, diaphragm, AC, diaphragm, AC are assembled in order from bottom to top;

[0011] Before covering the positive electrode shell, drip the electrolyte into the negative electrode shell to soak all the contents therein; cover the positive electrode shell, press firmly, seal well, and let it stand to obtain a hybrid lithium-ion supercapacitor.

[0012] Preferably, the ternary lithium battery material includes nickel, cobalt, manganese or nickel, cobalt and aluminum, preferably nickel, cobalt and manganese;

[0013] Hard carbon includes resin carbon of phenolic resin, epoxy resin, polysaccharide alcohol resin; organic polymer carbon of PVA, PVC, PVDF, PAN; biomass carbon of plant residues, preferably organic polymer carbon PVC;

[0014] Conductive carbon materials include graphene, carbon nanotubes, graphite paper, carbon fiber, bamboo charcoal, and activated carbon; activated carbon is preferred;

[0015] The adhesive includes a thermoplastic adhesive, which is polystyrene, polyethylene; an epoxy resin adhesive; a mixture of one or more of polytetrafluoroethylene, polyvinylidene fluoride, a high molecular adhesive of polyethylene oxide, sodium carboxymethyl cellulose CMC, styrene-butadiene rubber SBR, and polyacrylic acid PAA; preferably polyvinylidene fluoride.

[0016] Preferably, a regulator is added to the conductive carbon material in an amount of 10-15% of the total amount of the conductive carbon material;

[0017] The preparation method of the regulator is as follows:

[0018] Add 2-5 parts of nano-silicon dioxide to 5-8 parts of chitosan solution, then add 1-3 parts of flaky talc and 1-2 parts of nano-silica sol, mix and stir thoroughly, and finally wash with water and dry to obtain a nano-silicon dioxide modifier;

[0019] The bentonite is first mixed with a sufficient amount of lanthanum nitrate solution, then filtered and dried. 4-7 parts of dry bentonite, 3-5 parts of phosphate buffer solution, 1-3 parts of sodium dodecylbenzene sulfonate and 2-5 parts of nano-silica modifier are blended and ball-milled thoroughly. The ball-milling speed is 1500r / min. The ball-milling is carried out for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

[0020] Preferably, the mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum nitrate solution is 4-7%.

[0021] Preferably, the solid phase mixing method is to add the ternary lithium battery material, hard carbon, conductive carbon and adhesive into a mixer according to a preset ratio, preferably 80-98%: 1-10%: 1-10;

[0022] The stirring speed is 5 to 200 rmin-1, preferably 100 rmin-1;

[0023] Air flow crushing, control the material flow range to 0.1-1.0m3s, preferably 0.4-0.8m3s;

[0024] The air flow crushing pressure is 1-10KPa, and the preferred pressure is 3-8KPa;

[0025] The crushing power of the air flow crusher is 10-80KW, preferably 25-60KW.

[0026] Preferably, the subsonic cold spray powder feeding rate is 50-500 mg s-1, preferably 100-350 mg s-1; the deposition efficiency is 70-99%, preferably 80-90%; the working gas pressure is 0.1-1 MPa, preferably 0.5 MPa; the thickness of the coating layer is controlled at 3-5000 μm, preferably 5-300 μm.

[0027] Preferably, the working gas pressure in the preparation of the negative electrode material is 10-3Pa-10-7Pa, preferably 10-3Pa-10-6Pa;

[0028] The metal material is lithium, sodium, zinc, potassium, or aluminum, preferably lithium;

[0029] The working temperature is 100-600°C, preferably 300-500°C;

[0030] The holding time is 30-120 min, preferably 60-120 min;

[0031] The thickness of the plated metal layer is 1-100 nm, preferably 20-100 nm.

[0032] Preferably, the pre-immersion time in capacitor assembly is: 0.5h-6h, preferably 1h-6h;

[0033] The amount of electrolyte dripped in is 1-100 μL, preferably 20-100 μL;

[0034] The compaction pressure is 40-70Mpa, preferably 45-70Mpa;

[0035] The standing time is 0.5h-24h, preferably 6h-24h;

[0036] The separator is glass fiber, cellulose, polyethylene, polypropylene, non-woven membrane, composite membrane, preferably composite membrane;

[0037] The lithium salt of the electrolyte is LiPF6, LiClO4, LiBF4, LiAsF6, AN organic electrolyte, preferably LiPF6 and AN organic electrolyte;

[0038] The concentration of the solution is 1M-3M, preferably 1M;

[0039] The battery shell is one of a CR2032 button battery shell group, a detachable two-electrode electrical measurement device, and a soft-pack battery shell group, preferably a CR2032 button battery shell group.

[0040] Preferably, 5-10% of the total amount of the electrolyte is further added to the electrolyte.

[0041] The preparation method of hydroxyapatite agent is as follows:

[0042] Hydroxyapatite is added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment is completed, the mixture is washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution are mixed at a weight ratio of 5:2 and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a hydroxyapatite agent.

[0043] Preferably, the mass fraction of the sodium silicate solution is 2-5%; the mass fraction of the yttrium nitrate solution is 3-6%; the power of the ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] The positive electrode preparation of the present invention adopts a solvent-free mixing scheme to achieve solvent-free operation and further improve environmental protection; the subsonic cold spraying method is used for forming, and compared with the traditional mode, the material utilization rate is greatly improved, the cost is reduced, and the size and thickness of the positive electrode can be accurately controlled to achieve high density, thereby increasing the capacity; the negative electrode adopts a vacuum evaporation method to directly prepare metallic lithium on the steel shell, which has better contact than other negative electrode materials, and the thickness is greatly reduced to achieve a high energy density negative electrode; the vacuum evaporation method can well control the thickness of lithium metal, increase the density of the negative electrode material, and improve its cycle stability; achieve higher energy density, and at the same time, better high-temperature reliability, and realize the preparation of small-volume devices; the preparation process is easy to realize industrial assembly line production, reducing labor costs;

[0046] A regulator is also added to the conductive carbon material. The regulator is immersed in a lanthanum nitrate solution using bentonite and mixed thoroughly. A phosphate buffer solution, sodium dodecylbenzene sulfonate, and a nano-silica modifier are mixed and ball-milled thoroughly. Nano-silica is added to a chitosan solution, and then flaky talcum powder and nano-silica sol are added and mixed and stirred to fully form a nano-silica modifier. The nano-silica modifier is coordinated with bentonite to enhance the charge and discharge performance and cycle stability of the product, and the product performance is significantly improved. At the same time, a hydroxyapatite agent is also added to the electrolyte; the hydroxyapatite agent is ultrasonically treated in a sodium silicate solution, and then mixed and ball-milled with an yttrium nitrate solution at a weight ratio of 5:2. The hydroxyapatite agent and the regulator are coordinated and synergistic, and the performance of the product is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 Figure 1 shows an assembled hybrid lithium-ion supercapacitor with a diameter of 4.8 mm.

[0048] Figure 2 Figure 1 shows an assembled hybrid lithium-ion supercapacitor with a diameter of 6.8 mm.

[0049] Figure 3 CV diagram of the hybrid lithium-ion supercapacitor in Example 1 of the present invention;

[0050] Figure 4 This is an electrochemical impedance diagram of the hybrid lithium-ion supercapacitor in Example 1 of the present invention;

[0051] Figure 5 This is a test diagram of different rates of the hybrid lithium-ion supercapacitor in Example 1 of the present invention;

[0052] Figure 6 This is a graph showing the first charge and discharge voltage of the hybrid lithium-ion supercapacitor in Example 1 of the present invention;

[0053] Figure 7This is a cycle performance diagram of the hybrid lithium-ion supercapacitor in Example 1 of the present invention;

[0054] Figure 8 Schematic diagram of the preparation process of the hybrid lithium-ion supercapacitor in Example 1 of the present invention. DETAILED DESCRIPTION

[0055] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] A method for preparing a hybrid lithium-ion supercapacitor of this embodiment comprises the following steps:

[0057] Step 1: Preparation of positive electrode materials: solid phase mixing of ternary lithium battery, hard carbon, conductive carbon and binder; secondly, mixing and binder fiberization by air flow milling; then, obtaining electrode sheets on substrates by subsonic cold spraying;

[0058] Step 1: Under vacuum conditions, the metal material is placed into a vacuum coating machine, the temperature is raised to a certain level to vaporize the metal directly, and the metal ions fly to the surface of the substrate and condense into a film of a certain thickness to obtain the negative electrode material;

[0059] Step 2: Capacitor assembly: prepare the positive electrode material, negative electrode material, diaphragm, and electrolyte, and pre-soak the positive electrode material and diaphragm in the electrolyte to fully soak them;

[0060] The metal-film coated negative electrode shell, diaphragm, positive electrode sheet, diaphragm, AC, diaphragm, AC are assembled in order from bottom to top;

[0061] Before covering the positive electrode shell, drip the electrolyte into the negative electrode shell to soak all the contents therein; cover the positive electrode shell, press firmly, seal well, and let it stand to obtain a hybrid lithium-ion supercapacitor.

[0062] The ternary lithium battery material of this embodiment includes three elements: nickel, cobalt, manganese or nickel, cobalt, and aluminum, preferably nickel, cobalt, and manganese;

[0063] Hard carbon includes resin carbon of phenolic resin, epoxy resin, polysaccharide alcohol resin; organic polymer carbon of PVA, PVC, PVDF, PAN; biomass carbon of plant residues, preferably organic polymer carbon PVC;

[0064] Conductive carbon materials include graphene, carbon nanotubes, graphite paper, carbon fiber, bamboo charcoal, and activated carbon; activated carbon is preferred;

[0065] The adhesive includes a thermoplastic adhesive, which is polystyrene, polyethylene; an epoxy resin adhesive; a mixture of one or more of polytetrafluoroethylene, polyvinylidene fluoride, a high molecular adhesive of polyethylene oxide, sodium carboxymethyl cellulose CMC, styrene-butadiene rubber SBR, and polyacrylic acid PAA; preferably polyvinylidene fluoride.

[0066] The conductive carbon material of this embodiment also contains a regulator in an amount of 10-15% of the total amount of the conductive carbon material;

[0067] The preparation method of the regulator is as follows:

[0068] Add 2-5 parts of nano-silicon dioxide to 5-8 parts of chitosan solution, then add 1-3 parts of flaky talc and 1-2 parts of nano-silica sol, mix and stir thoroughly, and finally wash with water and dry to obtain a nano-silicon dioxide modifier;

[0069] The bentonite is first mixed with a sufficient amount of lanthanum nitrate solution, then filtered and dried. 4-7 parts of dry bentonite, 3-5 parts of phosphate buffer solution, 1-3 parts of sodium dodecylbenzene sulfonate and 2-5 parts of nano-silica modifier are blended and ball-milled thoroughly. The ball-milling speed is 1500r / min. The ball-milling is carried out for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

[0070] The mass fraction of the chitosan solution in this embodiment is 2-5%; the mass fraction of the lanthanum nitrate solution is 4-7%.

[0071] In the solid phase mixing method of this embodiment, the ternary lithium battery material, hard carbon, conductive carbon and adhesive are added to a mixer according to a preset ratio, preferably 80-98%: 1-10%: 1-10;

[0072] The stirring speed is 5 to 200 rmin-1, preferably 100 rmin-1;

[0073] Air flow crushing, control the material flow range to 0.1-1.0m3s, preferably 0.4-0.8m3s;

[0074] The air flow crushing pressure is 1-10KPa, and the preferred pressure is 3-8KPa;

[0075] The crushing power of the air flow crusher is 10-80KW, preferably 25-60KW.

[0076] The subsonic cold spray powder feeding rate of this embodiment is 50-500 mg s-1, preferably 100-350 mg s-1; the deposition efficiency is 70-99%, preferably 80-90%; the working gas pressure is 0.1-1 MPa, preferably 0.5 MPa; the thickness of the coating layer is controlled at 3-5000 μm, preferably 5-300 μm.

[0077] The working gas pressure in the preparation of the negative electrode material of this embodiment is 10-3Pa-10-7Pa, preferably 10-3Pa-10-6Pa;

[0078] The metal material is lithium, sodium, zinc, potassium, or aluminum, preferably lithium;

[0079] The working temperature is 100-600°C, preferably 300-500°C;

[0080] The holding time is 30-120 min, preferably 60-120 min;

[0081] The thickness of the plated metal layer is 1-100 nm, preferably 20-100 nm.

[0082] Preferably, the pre-immersion time in capacitor assembly is: 0.5h-6h, preferably 1h-6h;

[0083] The amount of electrolyte dripped in is 1-100 μL, preferably 20-100 μL;

[0084] The compaction pressure is 40-70Mpa, preferably 45-70Mpa;

[0085] The standing time is 0.5h-24h, preferably 6h-24h;

[0086] The separator is glass fiber, cellulose, polyethylene, polypropylene, non-woven membrane, composite membrane, preferably composite membrane;

[0087] The lithium salt of the electrolyte is LiPF6, LiClO4, LiBF4, LiAsF6, AN organic electrolyte, preferably LiPF6 and AN organic electrolyte;

[0088] The concentration of the solution is 1M-3M, preferably 1M;

[0089] The battery shell is one of a CR2032 button battery shell group, a detachable two-electrode electrical measurement device, and a soft-pack battery shell group, preferably a CR2032 button battery shell group.

[0090] The electrolyte of this embodiment also contains 5-10% of the total amount of the electrolyte, which is a hydroxyapatite agent;

[0091] The preparation method of hydroxyapatite agent is as follows:

[0092] Hydroxyapatite is added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment is completed, the mixture is washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution are mixed at a weight ratio of 5:2 and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a hydroxyapatite agent.

[0093] The mass fraction of the sodium silicate solution in this embodiment is 2-5%; the mass fraction of the yttrium nitrate solution is 3-6%; the power of the ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min.

[0094] Example 1

[0095] (1) Preparation of positive electrode materials: First, a ternary lithium battery / hard carbon composite material, conductive carbon and a binder are added to a stirring container in a ratio of 80%:10%:10% and stirred to obtain a slurry; secondly, the slurry is mixed and the binder is fiberized by air flow milling, and the material flow rate is controlled at 0.5m3 s, the pressure is controlled at 6KPa, the air flow mill power is controlled at 50KW, and the material temperature is controlled at 80°C; then, a subsonic cold spraying method is used to form a pole piece, the powder feeding rate is controlled at 350mg s-1, the deposition efficiency is controlled at 90%, and the working gas pressure is 0.6MPa; the thickness of the coating layer is controlled at 100μm; finally, a lithium battery positive electrode piece is obtained.

[0096] (2) Preparation of negative electrode materials: Lithium metal is directly evaporated in an argon atmosphere by vacuum evaporation, and lithium metal is plated on the pre-prepared negative electrode shell to obtain the negative electrode material. The working temperature in the experiment is 450°C, the working gas pressure is 10-5Pa; the insulation time is 120min; the thickness of the sputtered metal layer is 25nm;

[0097] (3) Capacitor assembly: prepare positive electrode materials, negative electrode materials, diaphragms, and electrolytes. Soak the positive electrode materials and diaphragms in the electrolyte for 1 hour to fully soak them; assemble them in the order of negative electrode shell coated with metal film, diaphragm, positive electrode sheet, diaphragm, AC, diaphragm, AC from bottom to top; before covering the positive electrode shell, drip 60μL of electrolyte into the negative electrode shell to soak all the contents; cover the positive electrode shell, press firmly with a pressure of 50MPa, seal well, and let it stand for 12 hours to obtain a hybrid lithium-ion supercapacitor.

[0098] Example 2

[0099] Example 2 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the ratio of the ternary lithium / hard carbon composite material: conductive carbon: binder is changed. In Example 2, the ratio = 85%: 10%: 5%, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0100] Example 3

[0101] Example 3 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the ratio of the ternary lithium / hard carbon composite material: conductive carbon: binder is changed. In Example 3, the ratio = 90%: 5%: 5%, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0102]

[0103] Example 4

[0104] Example 4 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the material of the hard carbon is changed. In Example 4, resin carbon is used, and the remaining steps are the same as those in Example 1, which will not be repeated here.

[0105] Example 5

[0106] Example 5 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the hard carbon material is changed. In Example 5, biomass carbon material is used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0107] Example 6

[0108] Example 6 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the power of the airflow milling is changed. In Example 6, 30KW, 40KW, 50KW, and 60KW are used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0109]

[0110] Example 7

[0111] Example 7 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the material flow rate range of the airflow milling is changed. In Example 7, the material flow rate range is controlled at 0.2m3 s, 0.4m3 s, 0.6m3 s, 0.8m3 s, and 1.0m3 s, and the remaining steps are consistent with Example 1 and are not repeated here.

[0112]

[0113] Example 8

[0114] Embodiment 8 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Embodiment 1 in that the type of conductive carbon is changed. In Embodiment 8, ternary lithium / hard carbon composite material + graphene, ternary lithium / hard carbon composite material + carbon nanotube, ternary lithium / hard carbon composite material + graphite paper, ternary lithium / hard carbon composite material + carbon fiber, ternary lithium / hard carbon composite material + bamboo charcoal, ternary lithium / hard carbon composite material + activated carbon are used, and the remaining steps are consistent with Embodiment 1, which will not be repeated here.

[0115] Comparative Example 1

[0116] Comparative Example 1 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 3 in that the coating method of the positive electrode material is changed, and the obtained electrode piece is connected to the button negative electrode steel shell through a conductive graphite slurry, and the rest is the same as Example 3. In Comparative Example 1, a direct extrusion molding method is adopted, and the other steps are consistent with Example 3, which will not be repeated here.

[0117] The hybrid lithium-ion supercapacitors of Example 3 and Comparative Example 1 were subjected to the following performance tests: first cycle retention rate, 10-cycle capacity retention rate, 30-cycle discharge capacity, and 50-cycle discharge capacity. The charge and discharge test equipment was a NEWARE BTS charge and discharge tester produced by Shenzhen Newwell Electronics Co., Ltd. The charge and discharge voltage was 2.5-4.2V, and the current was 1C. The test results are shown in Table 1.

[0118] Table 1 Performance test results of hybrid lithium ion supercapacitors of Example 3 and Comparative Example 1

[0119]

[0120] As can be seen from Table 1, the hybrid lithium-ion supercapacitor of the present invention has good electrochemical performance. By comparing the performance of the hybrid lithium-ion supercapacitor using the ultrasonic spraying method and the direct extrusion molding method in Example 3, it can meet the requirements of high energy density performance, effectively reduce battery capacity attenuation, ensure the cruising range requirements of electric vehicles, and improve the advantages of cycle life, providing a new direction for the development of negative electrode materials for lithium-ion batteries.

[0121] Comparative Example 2

[0122] Comparative Example 2 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the thickness of the coating is changed. In Comparative Example 2, 20 nm, 50 nm, 75 nm, and 100 nm are used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0123] Comparative Example 3

[0124] Comparative Example 3 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the positive electrode active material is changed. In Comparative Example 3, nickel cobalt, nickel aluminum, nickel cobalt manganese, nickel cobalt manganese aluminum, etc. are used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0125] Comparative Example 4

[0126] Comparative Example 4 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the stirring method is changed. In Comparative Example 4, a solvent such as anhydrous ethanol, anhydrous methanol, N,N-dimethylamide, etc. is added, and the remaining steps are consistent with Example 1 and are not repeated here.

[0127] Comparative Example 5

[0128] Comparative Example 5 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in that the negative electrode lithium sheet is used. In Comparative Example 5, the lithium sheet is directly used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0129] Comparative Example 6

[0130] Comparative Example 6 provides a method for preparing a hybrid lithium-ion supercapacitor, which is different from Example 1 in the material of the negative electrode. In Comparative Example 6, sodium metal, aluminum metal, magnesium metal, etc. are used, and the remaining steps are consistent with Example 1, which will not be repeated here.

[0131] Optimization example 1:

[0132] Based on Example 1,

[0133] A regulator is also added to the conductive carbon material, which accounts for 10% of the total amount of the conductive carbon material;

[0134] The preparation method of the regulator is as follows:

[0135] 2 parts of nano-silicon dioxide are added to 5 parts of chitosan solution, and then 1 part of flaky talc and 1 part of nano-silica sol are added and mixed and stirred thoroughly, and finally washed with water and dried to obtain a nano-silicon dioxide modifier;

[0136] The bentonite is first mixed thoroughly with a sufficient amount of lanthanum nitrate solution, then filtered and dried. Four parts of dry bentonite, three parts of phosphate buffer solution, one part of sodium dodecylbenzene sulfonate and two parts of nano-silica modifier are blended and ball-milled thoroughly at a ball-milling speed of 1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

[0137] The mass fraction of the chitosan solution in this embodiment is 2%; the mass fraction of the lanthanum nitrate solution is 4%.

[0138] A hydroxyapatite agent of 5% of the total amount of the electrolyte is also added to the electrolyte;

[0139] The preparation method of hydroxyapatite agent is as follows:

[0140] Hydroxyapatite was added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment was completed, the mixture was washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution were mixed at a weight ratio of 5:2 and ball-milled at a speed of 1000 r / min for 1 hour. After the ball-milling was completed, the mixture was washed with water and dried to obtain a hydroxyapatite agent.

[0141] The mass fraction of the sodium silicate solution in this embodiment is 2%; the mass fraction of the yttrium nitrate solution is 3%; the power of the ultrasonic treatment is 350W, and the ultrasonic time is 20min.

[0142] Optimization example 2:

[0143] Based on Example 1,

[0144] A regulator is also added to the conductive carbon material, accounting for 15% of the total amount of the conductive carbon material;

[0145] The preparation method of the regulator is as follows:

[0146] 5 parts of nano-silicon dioxide are added to 8 parts of chitosan solution, and then 3 parts of flaky talc and 2 parts of nano-silica sol are added and mixed and stirred thoroughly, and finally washed with water and dried to obtain a nano-silicon dioxide modifier;

[0147] The bentonite is first mixed thoroughly with a sufficient amount of lanthanum nitrate solution, then filtered and dried. Seven parts of dry bentonite, five parts of phosphate buffer solution, three parts of sodium dodecylbenzene sulfonate and five parts of nano-silica modifier are blended and ball-milled thoroughly at a ball-milling speed of 1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

[0148] The mass fraction of the chitosan solution in this embodiment is 5%; the mass fraction of the lanthanum nitrate solution is 7%.

[0149] A hydroxyapatite agent of 10% of the total amount of the electrolyte is also added to the electrolyte;

[0150] The preparation method of hydroxyapatite agent is as follows:

[0151] Hydroxyapatite was added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment was completed, the mixture was washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution were mixed at a weight ratio of 5:2 and ball-milled at a speed of 1500 r / min for 1 hour. After the ball-milling was completed, the mixture was washed with water and dried to obtain a hydroxyapatite agent.

[0152] The mass fraction of the sodium silicate solution in this embodiment is 5%; the mass fraction of the yttrium nitrate solution is 6%; the power of the ultrasonic treatment is 400W, and the ultrasonic time is 30min.

[0153] Optimization example 3:

[0154] Based on Example 1,

[0155] A regulator is also added to the conductive carbon material, accounting for 12.5% ​​of the total amount of the conductive carbon material;

[0156] The preparation method of the regulator is as follows:

[0157] 3 parts of nano-silicon dioxide are added to 6.5 parts of chitosan solution, and then 2 parts of flaky talc and 1.5 parts of nano-silica sol are added and mixed and stirred thoroughly, and finally washed with water and dried to obtain a nano-silicon dioxide modifier;

[0158] The bentonite is first mixed thoroughly with a sufficient amount of lanthanum nitrate solution, then filtered and dried. 5.5 parts of dry bentonite, 4 parts of phosphate buffer solution, 2 parts of sodium dodecylbenzene sulfonate and 3.5 parts of nano-silica modifier are blended and ball-milled thoroughly at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

[0159] The mass fraction of the chitosan solution in this embodiment is 3.5%; the mass fraction of the lanthanum nitrate solution is 5.5%.

[0160] A hydroxyapatite agent is also added to the electrolyte in an amount of 7.5% of the total electrolyte amount;

[0161] The preparation method of hydroxyapatite agent is as follows:

[0162] Hydroxyapatite was added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment was completed, the mixture was washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution were mixed at a weight ratio of 5:2 and ball-milled at a speed of 1250 r / min for 1 h. After the ball-milling was completed, the mixture was washed with water and dried to obtain a hydroxyapatite agent.

[0163] The mass fraction of the sodium silicate solution in this embodiment is 3.5%; the mass fraction of the yttrium nitrate solution is 34.5%; the power of the ultrasonic treatment is 375W, and the ultrasonic time is 25min.

[0164]

[0165]

[0166] It can be seen from optimization examples 1-3 that a regulator accounting for 12.5% ​​of the total amount of conductive carbon material is added to the conductive carbon material in the product, and a hydroxyapatite agent accounting for 7.5% of the total amount of the electrolyte is added to the electrolyte. The performance effect of the product is significant. The two are coordinated and enhanced together, and the performance effect of the product is significantly improved.

[0167] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0168] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a hybrid lithium-ion supercapacitor, characterized in that: The following steps are involved: Step 1: Preparation of positive electrode materials: solid phase mixing of ternary lithium battery, hard carbon, conductive carbon and binder; Secondly, the mixing and binder fiberization are carried out by air flow pulverization; then the electrode sheet is obtained on the substrate by subsonic cold spraying; Step 1: Under vacuum conditions, the metal material is placed into a vacuum coating machine, the temperature is raised to a certain level to vaporize the metal directly, and the metal ions fly to the surface of the substrate and condense into a film of a certain thickness to obtain the negative electrode material; Step 2: Capacitor assembly: prepare the positive electrode material, negative electrode material, diaphragm, and electrolyte, and pre-soak the positive electrode material and diaphragm in the electrolyte to fully soak them; The metal-film coated negative electrode shell, diaphragm, positive electrode sheet, diaphragm, AC, diaphragm, AC are assembled in order from bottom to top; Before covering the positive electrode casing, drip electrolyte into the negative electrode casing to soak all the contents therein; Cover the positive electrode shell, press firmly, seal well, and let it stand to obtain a hybrid lithium-ion supercapacitor.

2. The method for preparing a hybrid lithium-ion supercapacitor according to claim 1, characterized in that: Ternary lithium battery materials include nickel, cobalt, manganese or nickel, cobalt, aluminum. Hard carbon includes resin carbon of phenolic resin, epoxy resin, polysaccharide alcohol resin; organic polymer carbon of PVA, PVC, PVDF, PAN; biomass carbon of plant residues; Conductive carbon materials include graphene, carbon nanotubes, graphite paper, carbon fiber, bamboo charcoal, and activated carbon; The adhesive includes a thermoplastic adhesive, which is polystyrene, polyethylene; an epoxy resin adhesive; a polymer adhesive of polytetrafluoroethylene, polyvinylidene fluoride, polyethylene oxide, sodium carboxymethyl cellulose CMC, styrene-butadiene rubber SBR, polyacrylic acid PAA or a mixture thereof.

3. The method for preparing a hybrid lithium-ion supercapacitor according to claim 1, characterized in that: The conductive carbon material is further added with a regulator in an amount of 10-15% of the total amount of the conductive carbon material; The preparation method of the regulator is as follows: Add 2-5 parts of nano-silicon dioxide to 5-8 parts of chitosan solution, then add 1-3 parts of flaky talc and 1-2 parts of nano-silica sol, mix and stir thoroughly, and finally wash with water and dry to obtain a nano-silicon dioxide modifier; The bentonite is first mixed with a sufficient amount of lanthanum nitrate solution, then filtered and dried. 4-7 parts of dry bentonite, 3-5 parts of phosphate buffer solution, 1-3 parts of sodium dodecylbenzene sulfonate and 2-5 parts of nano-silica modifier are blended and ball-milled thoroughly. The ball-milling speed is 1500r / min. The ball-milling is carried out for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a regulator.

4. The method for preparing a hybrid lithium-ion supercapacitor according to claim 3, characterized in that: The mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum nitrate solution is 4-7%.

5. The method for preparing a hybrid lithium-ion supercapacitor according to claim 1, characterized in that: Solid phase mixing method, ternary lithium battery material, hard carbon, conductive carbon and adhesive are added into a mixer according to a preset ratio, preferably 80-98%:1-10%:1-10; The speed of the mixer is 5-200r min-1; the air flow crushing controls the material flow rate in the range of 0.1-1.0m3 s; the air flow crushing pressure is 1-10KPa; and the crushing power of the air flow crusher is 10-80KW.

6. The method for preparing a hybrid lithium-ion supercapacitor according to claim 5, characterized in that: The cold spraying process adopts subsonic spraying equipment, the subsonic cold spraying powder feeding rate is 50-500mg s-1; the deposition efficiency is 70-99%; the working gas pressure is 0.1-1MPa; the thickness of the coating layer is controlled at 3-5000μm.

7. The method for preparing a hybrid lithium-ion supercapacitor according to claim 3, characterized in that: The working gas pressure in the preparation of negative electrode materials is 10-3Pa-10-7Pa; The metal material is lithium, sodium, zinc, potassium, and aluminum; the working temperature is 100-600° C.; the heat preservation time is 30-120 minutes; and the thickness of the plated metal layer is 1-100 nm.

8. The method for preparing a hybrid lithium-ion supercapacitor according to claim 1, characterized in that: The pre-immersion time in capacitor assembly is: 0.5h-6h; the amount of electrolyte dripped is 1-100μL; the compacting pressure is 40-70Mpa; the standing time is 0.5h-24h; The separator is glass fiber, cellulose, polyethylene, polypropylene, non-woven membrane, composite membrane; The lithium salt of the electrolyte is LiPF6, LiClO4, LiBF4, LiAsF6, AN organic electrolyte; The concentration of the electrolyte is 1M-3M; the battery shell is one of a CR2032 button battery shell group, a detachable two-electrode electrical measurement device, and a soft-pack battery shell group.

9. The method for preparing a hybrid lithium-ion supercapacitor according to claim 1, wherein 5-10% of the total amount of the electrolyte is further added to the electrolyte; The preparation method of hydroxyapatite agent is as follows: Hydroxyapatite is added to a sodium silicate solution at a weight ratio of 2:5 for ultrasonic treatment. After the ultrasonic treatment is completed, the mixture is washed with water, filtered and dried. The dried hydroxyapatite and yttrium nitrate solution are mixed at a weight ratio of 5:2 and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a hydroxyapatite agent.

10. The method for preparing a hybrid lithium-ion supercapacitor according to claim 9, wherein the mass fraction of the sodium silicate solution is 2-5%; the mass fraction of the yttrium nitrate solution is 3-6%; the power of the ultrasonic treatment is 350-400 W, and the ultrasonic time is 20-30 min.

Citation Information

Cited By

  • Battery diaphragm and lithium ion battery

    CN121642436A