Preparation method of transparent electrode and perovskite solar cell

By using a dual-target co-sputtering method to dope selenium into a transparent oxide film in perovskite solar cells, a selenium-doped transparent conductive film is formed. This solves the problem of low carrier concentration and conductivity in transparent conductive oxide films, improves electrode performance and cell efficiency, and is suitable for large-area cell fabrication.

CN119031804APending Publication Date: 2024-11-26TRINA SOLAR CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411040357.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing transparent conductive oxide thin films have low carrier concentration and conductivity in perovskite solar cells, which limits their development in top electrodes.

Method used

A selenium-doped transparent conductive film was deposited on the surface of a perovskite solar cell substrate using a dual-target co-sputtering method. By adjusting the selenium doping amount and sputtering parameters, a composite film was formed to improve the carrier concentration and conductivity.

Benefits of technology

It improves the carrier extraction capability of transparent electrodes and the stability of perovskite solar cells, enhances photoelectric conversion efficiency, and simplifies the fabrication process, making it suitable for large-area perovskite solar cells and tandem cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031804A_ABST
    Figure CN119031804A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a preparation method of a transparent electrode. The preparation method comprises the following steps: depositing and preparing the transparent electrode on the surface of a perovskite solar cell substrate by adopting double-target co-sputtering; wherein the transparent electrode is a selenium-doped transparent conductive film, and the doping mass percentage content of selenium in the selenium-doped transparent conductive film is 0.2%-5%. According to the technical scheme, the selenium element can be doped in the transparent oxide thin film through double-target co-sputtering, the selenium-doped transparent conductive thin film is formed, and the carrier concentration and conductivity in the transparent electrode are effectively improved; by adjusting the doping amount of selenium, perovskite light absorption layers of different systems are matched; by adopting the preparation method of the transparent electrode, the carrier extraction capability of the transparent electrode and the stability of the perovskite solar cell are improved, the damage of plasma to the substrate film in the sputtering process is effectively reduced, the overall preparation process is simple, and the preparation of the large-area perovskite solar cell and the laminated cell is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a method for preparing a transparent electrode and a perovskite solar cell, a method for preparing a perovskite solar cell, a photovoltaic module, and a photovoltaic system. Background Art

[0002] Perovskite solar cells (PSCs) have attracted much attention among the third generation of solar cells due to their excellent photoelectric performance, high photoelectric conversion efficiency, low solution preparation cost and simple process. Among them, transparent conductive oxide (TCO) films have broad application prospects in touch screens, optical coatings and thin-film solar cells due to their low resistivity and high transmittance in the visible light range.

[0003] Transparent conductive oxide films are often used as transparent electrodes due to their excellent properties such as low resistivity, high transmittance in the visible light range, and good chemical stability. However, due to the low carrier concentration and conductivity of these transparent conductive films, their development in the top electrode of perovskite solar cells is limited to a certain extent.

[0004] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention

[0005] The embodiments of the present application provide a method for preparing a transparent electrode and a perovskite solar cell, a method for preparing a perovskite solar cell, a photovoltaic module, and a photovoltaic system to solve or alleviate one or more of the technical problems raised above.

[0006] In a first aspect, an embodiment of the present application provides a method for preparing a transparent electrode, comprising the following steps: The transparent electrode is deposited on the surface of the perovskite solar cell substrate by dual-target co-sputtering; Wherein, the transparent electrode is a selenium-doped transparent conductive film, and the doping mass percentage of selenium in the selenium-doped transparent conductive film is 0.2% to 5%.

[0007] Optionally, the target materials used in the dual-target co-sputtering include a selenium target and an oxide target, and during the dual-target co-sputtering, the dual-target co-sputtering includes a first sputtering step and a second sputtering step; During the first sputtering step, the sputtering power of the selenium target is 5-15W, and the sputtering power of the oxide target is 15-50W; During the second sputtering step, the sputtering power of the selenium target is 20-45W, and the sputtering power of the oxide target is 45-150W.

[0008] Optionally, during the first sputtering step, the sputtering time of the selenium target and the oxide target is 1 to 20 minutes. More preferably, the sputtering time is 5 to 10 minutes; In the second sputtering process, the sputtering time of the selenium target and the oxide target is 1 to 60 minutes. More preferably, the sputtering time is 10 to 40 minutes.

[0009] Optionally, the oxide target includes one of an ITO target, an IZO target, a FTO target, an IWO target, an AZO target and an AGO target.

[0010] Optionally, during the dual-target co-sputtering process, the reaction chamber of the magnetron sputtering apparatus is evacuated before the co-sputtering, and an inert gas is continuously introduced into the reaction chamber; Wherein, the flow rate of the inert gas is 10-50 sccm, the pressure of the reaction chamber is 0.1-1.0 Pa, and the temperature of the reaction chamber is 20-25°C.

[0011] Optionally, the transparent electrode has a thickness of 100-500 nm.

[0012] In a second aspect, an embodiment of the present application provides a perovskite solar cell, comprising a conductive substrate, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer, and a transparent electrode stacked in sequence; Wherein, the transparent electrode is formed by any of the above-mentioned methods for preparing a transparent electrode.

[0013] Optionally, the perovskite solar cell includes a formal perovskite solar cell or an inverted perovskite solar cell.

[0014] Optionally, the buffer layer is a metal oxide film, and the metal oxide film includes a molybdenum oxide film and a tin oxide film; when the perovskite solar cell is a formal structure, the molybdenum oxide film is used as the buffer layer; when the perovskite solar cell is a trans structure, the tin oxide film is used as the buffer layer; the thickness of the buffer layer is 10~30nm.

[0015] Optionally, the conductive substrate includes a flexible substrate or a rigid substrate, wherein the rigid substrate includes one of ITO (indium tin oxide) transparent conductive glass, FTO (fluorine-doped tin oxide) transparent conductive glass, IWO (tungsten-doped indium oxide) transparent conductive glass and AZO (aluminum-doped zinc oxide) transparent conductive glass.

[0016] Optionally, the perovskite light absorbing layer is prepared by a solution method.

[0017] In a third aspect, an embodiment of the present application provides a method for preparing a perovskite solar cell, comprising: providing a conductive substrate; forming a hole transport layer on the upper surface of the conductive substrate; Forming a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer and a transparent electrode in sequence on the surface of the hole transport layer; Wherein, the transparent electrode is formed by any of the above-mentioned methods for preparing a transparent electrode.

[0018] Optionally, the perovskite light-absorbing layer comprises a perovskite material and an organic solvent, the perovskite material is an ABX3 structure; A is a monovalent cation; B is a divalent cation; X is a monovalent anion; wherein the concentration of B is 200 mg / mL to 600 mg / mL; Wherein, A includes one or more of methylamine, formamidine, acetamidine, cesium and rubidium; B includes one or more of lead, tin, copper and germanium; X includes F - ,I - Br - , Cl - 、BF4 - PF6 - and SCN - One or more of; The organic solvent includes one or more of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), acetonitrile (ACN), dimethylpyrrolidone (NMP), 2-methoxyethanol, and γ-butyrolactone.

[0019] Optionally, the preparation material of the electron transport layer includes PCBM ([6,6]-phenyl-C 71 -isomethyl butyrate), SnO2, TiO2, ZnO2, Al2O3, C 60 and ICBA (Indene-C 60 diadducts).

[0020] Optionally, the hole transport layer is made of a material selected from the group consisting of an organic hole transport material, an inorganic hole transport material, and a self-assembled monolayer material (SAM). More preferably, the hole transport layer is made of a SAM material.

[0021] Optionally, the preparation material of the hole transport layer (HTL) includes [2-(9H-carbazole-9-yl)ethyl]phosphonic acid and its derivatives, [2-(9H-carbazole-9-yl)butyl]phosphonic acid and its derivatives, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, polyethylene terephthalate, polymer of 3-hexylthiophene, PEDOT:PSS (poly 3,4-ethylenedioxythiophene:polystyrene sulfonate), polyethylenedioxythiophene-polystyrene sulfonate (PEDOT:PSS), NiO x and one or more of CuSCN.

[0022] Optionally, the buffer layer is prepared from materials including BCP (2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline), MoO x One or more of .

[0023] In a fourth aspect, an embodiment of the present application provides a photovoltaic module, comprising at least one battery string, wherein the battery string comprises the perovskite solar cell as described above.

[0024] In a fifth aspect, an embodiment of the present application provides a photovoltaic system, comprising the photovoltaic assembly as described above.

[0025] The above technical solution adopted in the embodiment of the present application may have the following advantages: The dual-target co-sputtering method is adopted to form a composite film, i.e., a selenium-doped transparent conductive film, by doping selenium in a transparent oxide film, which effectively improves the carrier concentration and conductivity in the transparent electrode; the doping amount of selenium can also be adjusted to match the perovskite light-absorbing layer of different systems; and the preparation process of the transparent electrode is optimized to improve the photoelectric performance of the transparent electrode. The dual-target co-sputtering method of the present application is used to prepare a transparent electrode, which can not only achieve precise control of the film thickness and doping ratio of the transparent electrode, improve the carrier extraction ability of the transparent electrode and the stability of the perovskite solar cell, and thus improve the photoelectric conversion efficiency of the perovskite solar cell; it can also effectively reduce the damage of the plasma to the substrate film during the sputtering process; and the overall preparation process is simple, which is more conducive to the preparation of large-area perovskite solar cells and stacked cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0027] Figure 1 It is a schematic diagram of the structure of a perovskite solar cell provided in an embodiment of the present application.

[0028] Description of reference numerals: 1. Conductive substrate; 2. Hole transport layer; 3. Perovskite light absorption layer; 4. Passivation layer; 5. Electron transport layer; 6. Buffer layer; 7. Electrode. DETAILED DESCRIPTION

[0029] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.

[0030] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not indicate that the present application discloses the existence of the first element, component, region, layer or part.

[0031] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0033] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0034] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.

[0035] The present invention provides a method for preparing a transparent electrode, comprising the following steps: The transparent electrode is deposited on the surface of the perovskite solar cell substrate by dual-target co-sputtering; The transparent electrode is a selenium-doped transparent conductive film, and the doping mass percentage of selenium in the selenium-doped transparent conductive film is 0.2% to 5%.

[0036] In the embodiment of the present application, dual-target co-sputtering is adopted, and selenium is doped in the transparent oxide film to form a composite film, that is, a selenium-doped transparent conductive film, which effectively improves the carrier concentration and conductivity in the transparent electrode; the doping amount of selenium can also be adjusted to match the perovskite light-absorbing layer of different systems; and the preparation process of the transparent electrode is optimized to improve the photoelectric performance of the transparent electrode. The preparation method of the present application is used to prepare the transparent electrode, which can not only realize the precise control of the film thickness and doping ratio of the transparent electrode, improve the carrier extraction ability of the transparent electrode and the stability of the perovskite solar cell, and improve the photoelectric conversion efficiency of the perovskite solar cell; it can also effectively reduce the damage of the plasma to the substrate film during the sputtering process; and the overall preparation process is simple, which is more conducive to the preparation of large-area perovskite solar cells and stacked cells.

[0037] The selenium doping mass percentage in the transparent conductive film used in the embodiment of the present application is 0.2% to 5%, which can make the selenium-doped transparent conductive film achieve better performance and effect. When the selenium doping mass percentage is lower than 0.2%, it cannot provide enough free carriers, resulting in insufficient conductivity of the transparent electrode, affecting its conductive performance; when the selenium doping mass percentage is higher than 5%, it will lead to excessive introduction of impurity energy levels in the transparent electrode, thereby increasing electron-impurity scattering, causing its conductivity to decrease; and it will also change the optical properties of the transparent electrode, resulting in a decrease in its transparency; in addition, it will also affect the stability and durability of the transparent electrode, resulting in it being easy to be oxidized and unstable.

[0038] It should be noted that selenium (Se) as a doping element has excellent photoelectric properties. Under heating or illumination conditions, it has electrical properties of high sensitivity and fast response, and has high carrier mobility and excellent environmental stability. Introducing selenium into a transparent oxide film to form a selenium-doped transparent conductive film (composite film) can introduce additional free electrons or increase the carrier concentration, thereby reducing resistance and improving the conductivity of the selenium-doped transparent conductive film; in addition, the transparency, refractive index and other optical parameters of the selenium-doped transparent conductive film can also be adjusted, thereby changing the response and applicability of the selenium-doped transparent conductive film to light; at the same time, the doping of selenium will also improve the stability of the selenium-doped transparent conductive film.

[0039] In an optional embodiment, the target materials used in the dual-target co-sputtering include a selenium target and an oxide target, and in the process of the dual-target co-sputtering, the dual-target co-sputtering includes a first sputtering step and a second sputtering step; In the first step of sputtering, the sputtering power of the selenium target is 5~15W, and the sputtering power of the oxide target is 15~50W; During the second sputtering step, the sputtering power of the selenium target is 20~45W, and the sputtering power of the oxide target is 45~150W.

[0040] In an embodiment of the present application, during the first sputtering step and the second sputtering step, the sputtering power of the selenium target is less than or equal to the sputtering power of the oxide target. The selenium target with lower sputtering power can better control the doping content to reduce the introduction of excessive selenium into the transparent oxide film, thereby avoiding affecting the performance and structure of the selenium-doped transparent conductive film. In addition, by adjusting the sputtering power of the selenium target and the oxide target, the thickness and doping ratio of the selenium-doped transparent conductive film can be accurately controlled, thereby improving the carrier concentration and conductivity of the selenium-doped transparent conductive film.

[0041] In an optional embodiment, during the first sputtering step, the sputtering time of the selenium target and the oxide target is 1 to 20 minutes. More preferably, the sputtering time is 5 to 10 minutes.

[0042] In the second step of sputtering, the sputtering time of the selenium target and the oxide target is 1 to 60 minutes. More preferably, the sputtering time is 10 to 40 minutes.

[0043] In the embodiment of the present application, if the sputtering time of the selenium target and the oxide target is too short, the selenium doping content will be too low. The purpose of the first sputtering step is to form a thin buffer layer on the substrate to reduce the damage to the substrate battery caused by subsequent sputtering. In addition, since the density of the film sputtered at low power is poor, it cannot be sputtered for too long, otherwise the buffer layer formed will be too thick, which will affect the carrier transmission performance and reduce the efficiency of the battery.

[0044] In an optional embodiment, the oxide target includes one of an ITO target, an IZO target, a FTO target, an IWO target, an AZO target, and an AGO target.

[0045] In the embodiments of the present application, the selected oxide target material is doped with selenium, which can make it have better transparency, conductivity and chemical stability; and the doping of selenium can adjust the composition ratio of the film, thereby optimizing the photoelectric performance. At the same time, selenium and oxide target materials have complementary properties, and the two can be combined to make the film have more comprehensive performance.

[0046] In an optional embodiment, during the dual-target co-sputtering process, the reaction chamber of the magnetron sputtering apparatus is evacuated before the co-sputtering, and an inert gas is continuously introduced into the reaction chamber; Among them, the flow rate of the inert gas is 10-50 sccm (such as 10 sccm, 30 sccm, 50 sccm), the pressure of the reaction chamber is 0.1-1.0 Pa (such as 0.1 Pa, 0.5 Pa, 1.0 Pa), and the temperature of the reaction chamber is 20-25°C (such as 20°C, 23°C, 25°C).

[0047] In an optional embodiment, the thickness of the transparent electrode is 100-500 nm. (Exemplarily, the thickness of the transparent electrode is 100 nm, 300 nm, 500 nm) In the embodiment of the present application, when the thickness of the transparent electrode is less than 100 nm, the square resistance of the film is relatively high, which will affect the carrier transport performance and further affect the efficiency of the perovskite solar cell; when the thickness of the transparent electrode is higher than 500 nm, problems such as reduced optical transmittance and high carrier concentration will occur, which will in turn affect the charge transfer efficiency and reduce the photoelectric performance of the device.

[0048] The present application may also provide a method for preparing a perovskite solar cell, comprising the following steps: Step S1: providing a conductive substrate; Step S2: forming a hole transport layer on the upper surface of the conductive substrate; Step S3: preparing a perovskite light absorbing layer on the upper surface of the hole transport layer; Step S4: forming a passivation layer on the upper surface of the perovskite light absorbing layer, Step S5: forming an electron transport layer on the upper surface of the passivation layer; Step S6: forming a buffer layer on the upper surface of the electron transport layer; Step S7: using the transparent electrode preparation method of any of the above embodiments to form a transparent electrode on the upper surface of the buffer layer; Among them, the conductive substrate, hole transport layer, perovskite light absorption layer, passivation layer, electron transport layer and buffer layer stacked in sequence constitute the base.

[0049] In some embodiments, the conductive substrate includes, but is not limited to, indium tin oxide (ITO) transparent conductive glass, fluorine-doped tin oxide (FTO) transparent conductive glass, tungsten-doped indium oxide (IWO) transparent conductive glass, and aluminum-doped zinc oxide (AZO) transparent conductive glass. The conductive substrate can be cleaned, laser etched, and ultraviolet treated. The step of cleaning the conductive substrate may include: placing the conductive substrate in an ultrasonic cleaning instrument, ultrasonically cleaning it with deionized water, isopropanol, and ethanol, respectively, the cleaning time for each step is 20-40 minutes (for example, 20 minutes, 30 minutes, 40 minutes), and then drying it with nitrogen after cleaning. The step of ultraviolet treating the conductive substrate may include: treating the conductive substrate with a UV-zone, wherein the treatment time is 20-40 minutes (for example, 20 minutes, 30 minutes, 40 minutes).

[0050] In some embodiments, the preparation material of the hole transport layer includes organic hole transport materials, inorganic hole transport materials, self-assembled monolayer materials (Self-Assembled Monolayer, referred to as SAM), etc., preferably SAM materials. The preparation materials of the hole transport layer include [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (abbreviated as 2PACZ), (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid (abbreviated as MeO-2PACZ), (4-(3,6-dimethyl-9H-carbazole-9-yl)ethyl)phosphonic acid (abbreviated as Me-4PACZ), (2-(4-(bis(4-methoxyphenyl)amino)phenyl)-1-cyanotitanyl)phosphonic acid (abbreviated as MPA-CPA) and (4-(2,7-dibromo-9,9-dimethylacridin-10(9H)yl)butyl)phosphonic acid (abbreviated as DMAcPA), PEDOT:PSS (poly 3,4-ethylenedioxythiophene:polystyrene sulfonate), NiO x and one or more of CuSCN, placing a hole transport layer solution on the upper surface of a conductive substrate, and then preparing a hole transport layer by solution spin coating. The spin coating speed is 5000-8000 rpm (e.g., 5000 rpm / min, 6500 rpm / min, 8000 rpm / min), and the time is 40-60s (e.g., 40s, 50s, 60s). Finally, an annealing treatment is performed to remove the solvent, and the temperature of the annealing treatment is 100°C and the time is 10min.

[0051] In some embodiments, the perovskite precursor solution is coated on the surface of the hole transport layer by a one-step spin coating method or a slit coating method to obtain a perovskite light absorbing layer. The coating speed may be 4000-5000 rpm / min (e.g., 4000rpm / min, 4500 rpm / min, 5000 rpm / min), and the coating time may be 30-40s (e.g., 30s, 35s, 40s). The perovskite light absorbing layer includes a perovskite material and an organic solvent, the perovskite material is an ABX3 structure; A is a monovalent cation; B is a divalent cation; X is a monovalent anion; wherein the concentration of B is 200mg / mL to 600mg / mL; wherein A includes one or more of methylamine, formamidine, acetamidine, cesium and rubidium; B includes one or more of lead, tin, copper and germanium; X includes F - ,I - Br - , Cl - 、BF4 - PF6 - and SCN -One or more of; the organic solvent includes one or more of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), acetonitrile (ACN), dimethylpyrrolidone (NMP), 2-methoxyethanol, and γ-butyrolactone.

[0052] In some embodiments, the passivation layer is prepared from one or more of 2-thiopheneethylamine hydrochloride (TEACl), 1,4-phenylenediamine hydroiodide (PDADI), and phenylethylamine iodide (PEAI), and the thickness of the passivation layer is 10-30 nm (e.g., 10 nm, 20 nm, 30 nm). The substrate of the passivation layer after evaporation is heated at 100-150°C (e.g., 100°C, 120°C, 150°C) for 3-5 min (e.g., 3 min, 6 min, 10 min). The passivation layer can be prepared by spin coating, vacuum evaporation, magnetron sputtering, atomic layer deposition, etc. When vacuum evaporation is used, the evaporation rate is 0.3-1 Å / s (e.g., 0.3 Å / s, 0.5 Å / s, 1 Å / s).

[0053] In some embodiments, the preparation material of the electron transport layer includes PCBM ([6,6]-phenyl-C 71 -isomethyl butyrate), TiO2, SnO2, ZnO2, Al2O3, C 60 and ICBA (Indene-C 60 The electron transport layer can be prepared by spin coating, vacuum evaporation, magnetron sputtering, atomic layer deposition and the like. When the vacuum evaporation method is used, the evaporation rate is 0.2Å / s, the evaporation time is 1500s, and the evaporation thickness is 30nm.

[0054] In some embodiments, the buffer layer is prepared from materials including BCP (2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline), MoO x The buffer layer can be prepared by spin coating, vacuum evaporation, magnetron sputtering, atomic layer deposition and the like. When the vacuum evaporation method is used, the evaporation rate is 0.1Å / s, the evaporation time is 1500s, and the evaporation thickness is 15nm.

[0055] In some embodiments, the transparent electrode is a selenium-doped transparent conductive film, which is prepared by dual-target co-sputtering, wherein the target materials used in sputtering include a selenium target and an oxide target, and the oxide target includes one of an ITO target, an IZO target, a FTO target, an IWO target, an AZO target and an AGO target.

[0056] In some embodiments, the transparent electrode can also be prepared by thermal evaporation, vacuum evaporation, sputtering, atomic layer deposition, 3D printing, screen printing, inkjet printing and other methods. When the vacuum evaporation method is used, the evaporation rate is 1Å / s, the evaporation time is 2000s, and the final evaporation thickness is 200nm.

[0057] like Figure 1 As shown, an embodiment of the present application provides a perovskite solar cell, which is formed by the preparation method of the perovskite solar cell of any of the above embodiments, including: a conductive substrate 1, a hole transport layer 2, a perovskite light absorption layer 3, a passivation layer 4, an electron transport layer 5, a buffer layer 6, and a transparent electrode 7 stacked in sequence.

[0058] The following specific examples further illustrate the present application, but should not be construed as limiting the present application. Without departing from the spirit and substance of the present application, modifications or replacements made to the methods, steps or conditions of the present application are within the scope of the present application.

[0059] [Example 1] like Figure 1 As shown, the specific structure of a perovskite solar cell is: A conductive substrate 1, a hole transport layer 2, a perovskite light absorption layer 3, a passivation layer 4, an electron transport layer 5, a buffer layer 6, and an electrode 7 are stacked in sequence.

[0060] The specific preparation process of a perovskite solar cell is as follows: Step S1a: providing a conductive substrate 1, wherein the conductive substrate 1 is indium tin oxide (ITO); and cleaning the conductive substrate 1, and drying it with nitrogen after cleaning; Step S2a: dissolving the hole transport layer preparation material 2PACZ in an IPA (isopropyl alcohol) solution to prepare a hole transport layer solution, the concentration of which is 1 mg / mL; then applying the hole transport layer solution to the upper surface of the conductive substrate 1 by spin coating and performing an annealing treatment to remove the solvent, thereby preparing a hole transport layer 2. The temperature of the annealing treatment is 100° C., the time is 10 min, and the thickness of the hole transport layer 2 is 2 nm; Step S3a: The perovskite materials FAI, PbI2, MACl, MAI, and CsI powders are mixed to obtain a mixture, and 1 mL of an organic solvent (DMF:NMP volume ratio of 5:1) is added to the mixture to dissolve the mixture to obtain Cs 0.05 FA 0.90 MA 0.05 PbI3 perovskite precursor solution; The perovskite precursor solution is spin-coated on the upper surface of the hole transport layer 2 by a spin coating method, and a one-step annealing treatment is performed to remove the solvent to prepare the perovskite light absorbing layer 3. The temperature of the one-step annealing treatment is 150° C. and the time is 30 minutes. Step S4a: depositing a passivation layer material 1,4-phenylenediamine hydroiodide (PDADI) on the upper surface of the perovskite light absorbing layer 3 by evaporation to form a passivation layer 4, the thickness of the passivation layer 4 being 1 nm; Step S5a: Depositing C on the upper surface of the passivation layer 4 by thermal evaporation 60 To form an electron transport layer 5, the thickness of the electron transport layer 5 is 30 nm; Step S6a: using a thermal evaporation method to deposit SnO2 on the upper surface of the electron transport layer 5 to form a buffer layer 6, the thickness of the buffer layer 6 is 20 nm; Step S7a: Partially shield the substrate with a mask, place it in the reaction chamber of the magnetron sputtering instrument, and evacuate the reaction chamber to a vacuum degree of 3×10 -4 Pa; then, inert gas argon is continuously introduced into the reaction chamber, and the argon gas flow rate is maintained at 20 sccm, and the temperature of the reaction chamber is 25°C; after the argon gas flow rate is stabilized, the pressure of the chamber is increased to 0.1 Pa; after the pressure of the reaction chamber is stabilized, the distance between the substrate and the selenium target is adjusted to 25 cm, and the distance between the substrate and the oxide target (ITO target) is adjusted to 20 cm; in the process of dual-target co-sputtering, the dual-target co-sputtering includes the first step of sputtering and the second step of sputtering; In the first sputtering process, the sputtering powers of the selenium target and the oxide target (ITO target) are 10 W and 30 W respectively, and the sputtering time is 3 minutes to obtain a preliminary transparent electrode; then in the second sputtering process, sputtering is continued on the preliminary transparent electrode, and the sputtering powers of the selenium target and the oxide target (ITO target) are adjusted to 30 W and 70 W respectively, and the sputtering time is 20 minutes to obtain a selenium-doped transparent conductive film as a transparent electrode for perovskite solar cells, and the thickness of the transparent electrode is 400 nm; wherein, the doping mass percentage of selenium in the selenium-doped transparent conductive film is 0.2%.

[0061] The conductive substrate 1, the hole transport layer 2, the perovskite light absorption layer 3, the passivation layer 4, the electron transport layer 5 and the buffer layer 6 which are stacked in sequence constitute a base.

[0062] [Example 2] The perovskite solar cell of Example 2 was prepared by referring to the preparation method of Example 1, except that, in step S7a, the flow rate of argon gas was maintained at 10 sccm, and after the flow rate of argon gas was stabilized, the pressure of the chamber was increased to 0.1 Pa, and in the first sputtering process, the sputtering powers of the selenium target and the oxide target (IZO target) were 5 W and 15 W, respectively, and the sputtering time was 5 min, to obtain a preliminary transparent electrode; then, in the second sputtering process, sputtering was continued on the preliminary transparent electrode, and the sputtering powers of the selenium target and the oxide target (IZO target) were adjusted to 20 W and 45 W, respectively, and the sputtering time was 15 min, to obtain a selenium-doped transparent conductive film as a transparent electrode of the perovskite solar cell, and the thickness of the transparent electrode was 100 nm; wherein, the doping mass percentage of selenium in the selenium-doped transparent conductive film was 5%.

[0063] [Example 3] The perovskite solar cell of Example 3 was prepared by referring to the preparation method of Example 1, except that, in step S7a, the flow rate of argon gas was maintained at 10 sccm. After the flow rate of argon gas was stabilized, the pressure of the chamber was increased to 0.1 Pa. In the first sputtering process, the sputtering powers of the selenium target and the oxide target (FTO target) were 15 W and 50 W, respectively, and the sputtering time was 4 min, to obtain a preliminary transparent electrode; then, in the second sputtering process, sputtering was continued on the preliminary transparent electrode, and the sputtering powers of the selenium target and the oxide target (FTO target) were adjusted to 45 W and 150 W, respectively, and the sputtering time was 18 min, to obtain a selenium-doped transparent conductive film as a transparent electrode for the perovskite solar cell, and the thickness of the transparent electrode was 500 nm; the doping mass percentage of selenium in the selenium-doped transparent conductive film was 3%.

[0064] [Example 4] - [Example 6] The perovskite solar cells of Examples 4 to 6 were prepared by referring to the preparation method of Example 1, with the only difference being that in step S7a, different oxide targets were used: the oxide target used in Example 4 was an IWO target, the oxide target used in Example 5 was an AZO target, and the oxide target used in Example 6 was an AGO target.

[0065] In order to more clearly illustrate the technical effects of the embodiments of the present application, the present application also points out the structure and preparation method of the perovskite solar cell of Comparative Example 1.

[0066] [Comparative Example 1] The perovskite solar cell of Comparative Example 1 was prepared by referring to the preparation method of Example 1, with the only difference being that in step S7a, during the first sputtering step, the sputtering power of the oxide target (ITO target) was 30 W, and a preliminary transparent electrode was obtained; then, during the second sputtering step, the oxide target (ITO target) was used to continue sputtering on the preliminary transparent electrode, and the sputtering power of the oxide target (ITO target) was 70 W to obtain a transparent electrode, and the thickness of the transparent electrode was 400 nm.

[0067] [Comparative Example 2] The perovskite solar cell of Comparative Example 2 was prepared by referring to the preparation method of Comparative Example 1, except that, in step S7a, the oxide target used was an IZO target.

[0068] The following is a performance test of the perovskite solar cells provided in Examples 1-6 of the present application and Comparative Examples 1-2, so as to obtain the fill factor open circuit voltage Voc, FF, short circuit current density Jsc, and photoelectric conversion efficiency PCE of the corresponding battery devices, and the test results are shown in Table 1.

[0069] Table 1 Performance test results of perovskite solar cells of Examples 1-6 and Comparative Examples 1-2

[0070] It can be seen from Table 1 that compared with comparative examples 1-2, the short-circuit current density, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cells of Examples 1-6 of the present application are significantly improved, which indicates that the preparation method in Examples 1-6 of the present application is used to introduce selenium as a doping element into the oxide film to form a selenium-doped transparent conductive film (transparent electrode), which can improve the carrier extraction ability of the transparent electrode and the stability of the perovskite solar cell, thereby improving the photoelectric conversion efficiency of the perovskite solar cell.

[0071] In summary, by adopting the dual-target co-sputtering method, selenium is doped into the transparent oxide film to form a composite film, i.e., a selenium-doped transparent conductive film, which effectively improves the carrier concentration and conductivity in the transparent electrode; the doping amount of selenium can also be adjusted to match the perovskite light-absorbing layer of different systems; and the preparation process of the transparent electrode is optimized to improve the photoelectric performance of the transparent electrode. The dual-target co-sputtering method of the present application is used to prepare the transparent electrode, which can not only realize the precise control of the film thickness and doping ratio of the transparent electrode, but also improve the carrier extraction ability of the transparent electrode and the stability of the perovskite solar cell, thereby improving the photoelectric conversion efficiency of the perovskite solar cell; it can also effectively reduce the damage of the plasma to the substrate film during the sputtering process; and the overall preparation process is simple, which is more conducive to the preparation of large-area perovskite solar cells and stacked cells.

[0072] The embodiment of the present application may also provide a photovoltaic module (not shown), including at least one battery string, the battery string including at least two perovskite solar cells as described above, and adjacent perovskite solar cells may be connected together by serial welding.

[0073] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box, and the junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid and then connected to the mains network to realize solar power supply. The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above-mentioned photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it is understandable that the application scenarios of photovoltaic systems are not limited to this, that is to say, photovoltaic systems can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.

[0074] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.

[0075] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0076] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0077] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a transparent electrode, characterized in that: The following steps are involved: The transparent electrode is deposited on the surface of the perovskite solar cell substrate by dual-target co-sputtering; Wherein, the transparent electrode is a selenium-doped transparent conductive film, and the doping mass percentage of selenium in the selenium-doped transparent conductive film is 0.2% to 5%.

2. The method for preparing a transparent electrode according to claim 1, characterized in that: The target materials used in the dual-target co-sputtering include a selenium target and an oxide target. During the dual-target co-sputtering, the dual-target co-sputtering includes a first sputtering step and a second sputtering step. During the first sputtering step, the sputtering power of the selenium target is 5 to 15 W, and the sputtering power of the oxide target is 15 to 50 W; During the second sputtering step, the sputtering power of the selenium target is 20-45W, and the sputtering power of the oxide target is 45-150W.

3. The method for preparing a transparent electrode according to claim 2, characterized in that: During the first sputtering step, the sputtering time of the selenium target and the oxide target is 1 to 20 minutes; During the second sputtering step, the sputtering time of the selenium target and the oxide target is 1 to 60 minutes.

4. The method for preparing a transparent electrode according to claim 2, characterized in that: The oxide target includes one of an ITO target, an IZO target, a FTO target, an IWO target, an AZO target and an AGO target.

5. The method for preparing a transparent electrode according to any one of claims 1 to 4, characterized in that: During the dual-target co-sputtering process, the reaction chamber of the magnetron sputtering apparatus is evacuated before the co-sputtering, and an inert gas is continuously introduced into the reaction chamber; Wherein, the flow rate of the inert gas is 10-50 sccm, the pressure of the reaction chamber is 0.1-1.0 Pa, and the temperature of the reaction chamber is 20-25°C.

6. The method for preparing a transparent electrode according to any one of claims 1 to 4, characterized in that: The thickness of the transparent electrode is 100-500 nm.

7. A perovskite solar cell, characterized in that: It includes a conductive substrate, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer, and a transparent electrode which are stacked in sequence; Wherein, the transparent electrode is formed by the preparation method of the transparent electrode according to any one of claims 1-6.

8. A method for preparing a perovskite solar cell, characterized in that: include: providing a conductive substrate; forming a hole transport layer on the upper surface of the conductive substrate; Forming a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer and a transparent electrode in sequence on the surface of the hole transport layer; Wherein, the transparent electrode is formed by the preparation method of the transparent electrode according to any one of claims 1-6.

9. A photovoltaic module, characterized in that: include: At least one cell string, the cell string comprising the perovskite solar cell according to claim 7.

10. A photovoltaic system, characterized in that: Comprising the photovoltaic module as claimed in claim 9.

Citation Information

Cited By

  • Preparation method of high-strength nanoscale chip packaging material

    CN120269890A