Piezoelectric polymer composite film with horizontally oriented zinc oxide nanorods and preparation
By introducing horizontally oriented zinc oxide nanorods into piezoelectric polymer films, it enhances its deformation and piezoelectric response under external forces, the problem of insufficient deformation of existing piezoelectric polymers is solved and tissue repair in the field of biomedical medicine is improved Effect.
Patent Information
- Application Number
- CN202411130984.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing piezoelectric polymers are insufficiently deformed under external forces, resulting in a small piezoelectric response and it is difficult to meet the organizational repair needs in the field of biomedical medicine.
The zinc oxide nanorod and piezoelectric polymer composite film are used to enhance the deformation ability and piezoelectric response of the composite material under external force by horizontally oriented zinc oxide nanorods on the surface or inside of the piezoelectric polymer film.
Under the action of external forces, especially when bending, the composite film produces greater deformation and stronger piezoelectric response, which is suitable for self-powered materials in the field of biomedical medicine, improving the tissue repair effect.
Smart Images

Figure HDA0004997803590000011 
Figure HDA0004997803590000012 
Figure HDA0004997803590000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a zinc oxide / piezoelectric polymer composite film and a preparation method thereof. Background Art
[0002] The human body contains a variety of electrically sensitive tissues, such as bones, skin, nerves, heart and blood vessels. Their electrical activities can be used to reflect the health of the body's life activities and play an important role in the directional migration, adhesion, proliferation of cells and healthy tissue function or wound healing.
[0003] The piezoelectric effect is the ability of certain materials to convert mechanical deformation into surface charge. Materials with piezoelectric properties are becoming more and more common in modern rehabilitation medicine because they are similar to human tissue. Piezoelectric polymers, as a type of flexible electroactive biomaterial, regulate cell behavior through surface charges generated by deformation caused by cell interactions, mechanical signal stimulation, or both. They have a good mechanical match with human tissue and good biocompatibility. The piezoelectric effect is generated by applying mechanical force and does not require an external power source. Therefore, they are widely used in many biomedical fields such as tissue repair and regeneration, biosensing, and drug delivery.
[0004] When piezoelectric materials are used as tissue engineering repair materials, they are usually used as electroactive implants, which use the mechanical deformation of the human heart, muscles, skin, joints and other tissues and organs during movement to achieve the self-generating effect of the piezoelectric material implant, build a dynamic bioelectric microenvironment, and regulate the adhesion, proliferation and differentiation behavior of cells, thereby inducing tissue repair and regeneration. Designing piezoelectric material implants with stronger piezoelectric output performance and piezoelectric sensitivity is of great significance for the material to respond to tiny deformations in human tissues and provide an ideal size of electrical signal to stimulate the damaged part, realize the repair of complex defective tissues, and then achieve better tissue repair and regeneration effects.
[0005] Pure piezoelectric polymers have good flexibility, semi-crystalline characteristics and diversity of crystal structure, which leads to their piezoelectric coefficients being usually smaller than those of inorganic piezoelectric materials. Therefore, piezoelectric polymers usually need to be modified. Existing studies on the modification of piezoelectric polymers are usually based on improving the piezoelectric phase content and crystallinity of piezoelectric polymers to improve their piezoelectricity. For example, the piezoelectric effect of piezoelectric polymers is improved by incorporating functional fillers, and most of the incorporation methods in these studies are simply simple mixing, and there is little attention paid to the improvement of the microstructure of the fillers. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a piezoelectric polymer composite film with horizontally oriented zinc oxide nanorods and its preparation. In the composite film, horizontally oriented zinc oxide nanorods are arranged on the surface and / or inside of the piezoelectric polymer film. Compared with pure piezoelectric polymers, the composite film can produce a larger deformation under the action of external force, especially when bending, thereby producing a larger piezoelectric response and sensitivity, and can be applied to the tissue repair effect of self-powered materials in the biomedical field. The preparation method of the present invention is simple in process, easy to control, easy to implement, and conducive to promotion and application.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] In a first aspect of the present invention, the present invention provides a zinc oxide / piezoelectric polymer composite film, comprising a piezoelectric polymer film and zinc oxide nanorods, wherein the zinc oxide nanorods are arranged in a horizontal orientation and are arranged on the surface and / or inside of the piezoelectric polymer film.
[0009] In some specific examples of the present invention, the diameter of the zinc oxide nanorods is 20 to 600 nm.
[0010] In some specific examples of the present invention, the length of the zinc oxide nanorods is 0.2-20 μm.
[0011] In some specific examples of the present invention, the polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea.
[0012] In a second aspect of the present invention, the present invention provides a method for preparing the above zinc oxide / piezoelectric polymer composite film, comprising the following steps:
[0013] (1) zinc acetate dihydrate and a solvent are mixed, stirred for 10 to 180 minutes, and then a piezoelectric polymer is added thereto, and the stirring is continued for 2 hours to 10 hours to form a mixed solution, wherein the feed ratio of the solvent, zinc acetate dihydrate, and piezoelectric polymer is 1 mL: (0.8 to 55) mg: (40 to 220) mg; the mixed solution is transferred to a substrate, coated into a strip with a thickness of 0.1 mm to 1.5 mm, and dried at a relative vacuum degree of -0.1 to 0 MPa and 30 to 80° C. until the solvent is completely volatilized to obtain a dried strip; the dried strip is annealed at 140 to 300° C. for 30 to 90 minutes to obtain a polymer film with seeds;
[0014] (2) dissolving zinc nitrate hexahydrate and hexamethylenetetramine in a molar ratio of 1:1 in deionized water to prepare a growth solution; in the growth solution, the concentration of zinc nitrate hexahydrate is 0.005-0.05 mol / L, and the concentration of hexamethylenetetramine is 0.005-0.05 mol / L;
[0015] (3) placing the polymer film with seed crystals obtained in step (1) in a reactor liner, adding the growth solution into the reactor liner, placing the reactor liner in a reactor shell, and performing a hydrothermal reaction at 80 to 140° C. for 1 to 8 hours. After unloading the reactor, the reaction product is cleaned and dried to obtain a composite film;
[0016] (4) in an air atmosphere, the composite film is kept on a hot plate at 160 to 300° C. for 0 to 30 minutes and then quenched, and then horizontally stretched at 25 to 100° C. at a stretching ratio of 1:1 to 1:15 to obtain a stretched composite film;
[0017] (5) The stretched composite film is kept on a hot plate at 140 to 300° C. for 0 to 30 min to obtain the target product.
[0018] In some specific examples of the present invention, the method further comprises step (6): subjecting the target product obtained in step (5) to electric polarization treatment by contact electric polarization or corona polarization.
[0019] In some specific examples of the present invention, in step (1), the piezoelectric polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea.
[0020] In some specific examples of the present invention, in step (1), the solvent is selected from at least one of N,N-dimethylformamide, dioxane, dichloromethane and acetone.
[0021] In some specific examples of the present invention, in step (1), the annealing temperature of the strip is 210° C., and the annealing time is 60 min.
[0022] In some specific examples of the present invention, in step (3), the volume of the growth solution is preferably no more than 80% of the volume of the reactor inner tank, and preferably the volume of the growth solution is 70-80% of the volume of the reactor inner tank.
[0023] In some specific examples of the present invention, in step (4), the insulation time on the hot plate is 3 to 15 minutes.
[0024] In some specific examples of the present invention, in step (4), the insulation temperature on the hot plate is 210° C., and the insulation time is 5 min.
[0025] In some specific examples of the present invention, in step (5), the insulation time on the hot plate is 3 to 15 minutes.
[0026] In some specific examples of the present invention, in step (5), the insulation temperature on the hot plate is 180° C., and the insulation time is 3 minutes.
[0027] In the third aspect of the present invention, the present invention provides another method for preparing the above zinc oxide / piezoelectric polymer composite film, comprising the following steps:
[0028] (1) dissolving zinc acetate dihydrate in deionized water to obtain a zinc acetate solution with a concentration of 0.01 to 0.1 mol / L, adding ammonium hydroxide dropwise thereto until the pH reaches 9 to 9.5, stirring for 20 to 60 minutes, and obtaining a mixed solution; taking an appropriate amount of the mixed solution and placing it in a reactor liner, placing the reactor liner in a reactor shell, and keeping the temperature at 80 to 140° C. for 2 to 10 hours for a hydrothermal reaction, and after unloading the reactor, washing the reaction product, centrifuging it, and drying it to obtain zinc oxide nanorod powder;
[0029] (2) mixing the zinc oxide nanorod powder obtained in step (1) with a solvent, and ultrasonically dispersing the mixture for 10 to 120 minutes, and then adding a piezoelectric polymer thereto, and continuing stirring for 2 to 10 hours to form a mixed solution, wherein the feed ratio of the solvent, zinc acetate dihydrate, and piezoelectric polymer is 1 mL: (0.4 to 22) mg: (40 to 220) mg; transferring the mixed solution to a substrate, coating it into a strip with a thickness of 0.1 to 1.5 mm, and drying the strip at 25 to 140° C. until the solvent is completely volatilized, to obtain a composite film;
[0030] (3) The composite film obtained in step (2) is horizontally stretched at a stretching ratio of 1:1 to 1:15 at 25 to 140° C., and then kept on a hot plate at 140 to 300° C. for 0 to 30 minutes to obtain the target product.
[0031] In some specific examples of the present invention, the method further comprises step (4): subjecting the target product obtained in step (3) to electric polarization treatment by contact electric polarization or corona polarization.
[0032] In some specific examples of the present invention, in step (1), the volume of the mixed solution is preferably no more than 80% of the volume of the reactor inner tank, and preferably the volume of the mixed solution is 70-80% of the volume of the reactor inner tank.
[0033] In some specific examples of the present invention, in step (2), the piezoelectric polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea.
[0034] In some specific examples of the present invention, in step (2), the solvent is selected from at least one of N,N-dimethylformamide, dioxane, dichloromethane and acetone.
[0035] In some specific examples of the present invention, in step (3), the insulation time on the hot plate is 3 to 15 minutes.
[0036] In some specific examples of the present invention, in step (3), the insulation temperature on the hot plate is 180° C., and the insulation time is 3 minutes.
[0037] In the present invention, room temperature generally refers to 20 to 27°C.
[0038] Compared with the prior art, the present invention has the following beneficial technical effects:
[0039] (1) The present invention proposes a zinc oxide / piezoelectric polymer composite film having a horizontally oriented zinc oxide nanorod arrangement on the surface and / or inside of the piezoelectric polymer film. Different from the disordered and chaotic arrangement of zinc oxide nanorods grown by general hydrothermal growth, which have insufficient deformation caused by the mutual forces offsetting each other when subjected to external forces, the composite film of the present invention is conducive to generating a larger deformation under the action of external forces, especially when bending occurs, thereby generating a better electromechanical response.
[0040] (2) The present invention proposes two methods for preparing the above zinc oxide / piezoelectric polymer composite film, both of which can be achieved by simple hydrothermal and stretching methods, which are convenient and simple and easy to control.
[0041] (3) The present invention also proposes that the density of zinc oxide nanorods on the surface or inside of the composite film per unit area and the size of the zinc oxide nanorods can be adjusted by regulating parameters such as the raw material feed amount, stretching ratio, reaction temperature and time, thereby achieving the control of the piezoelectric voltage output size and piezoelectric sensitivity of the composite film doped with zinc oxide nanorods when subjected to the same external force, thereby designing a suitable self-powered film for different tissue repair needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is the XRD diagram of the target product 1 obtained in Example 1 and the composite film obtained in step (3).
[0043] Figure 2 This is the FTIR graph of the target product 1 obtained in Example 1.
[0044] Figure 3A This is a SEM image of the composite film obtained in step (3) of Example 1.
[0045] Figure 3B This is a SEM image of the target product 1 obtained in Example 1.
[0046] Figure 4A and Figure 4B They are the electromechanical responses of pure PVTF and the target product 1 obtained in Example 1 after the same treatment.
[0047] Figure 5 It is the XRD diagram of the target product 2 obtained in Example 2 and the composite film obtained in step (3).
[0048] Figure 6 The XRD patterns of the target product 4 obtained in Example 4 and the composite film obtained in step (2) are shown in FIG.
[0049] Fig. 7A is a SEM image of the zinc oxide nanorod powder obtained in step (1) of Example 4.
[0050] Figure 7B This is a cross-sectional SEM image of the target product 4 obtained in Example 4.
[0051] Figure 8 This is a cross-sectional SEM image of the target product 5 obtained in Example 5.
[0052] Fig. 9 This is a cross-sectional SEM image of the target product 6 obtained in Example 6.
[0053] Fig.10 This is a cross-sectional SEM image of the target product 7 obtained in Example 7. DETAILED DESCRIPTION
[0054] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0055] In the following examples and comparative examples, the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased on the market. For example, vinylidene fluoride trifluoroethylene copolymer (i.e., polyvinylidene fluoride trifluoroethylene Poly (vinylidene fluoride-trifluoroethylene), P (VDF-TrFE), abbreviated as PVTF) is produced by Piezotech, France, wherein the molar ratio of vinylidene fluoride monomer to trifluoroethylene monomer is 7:3. The reactor includes a polytetrafluoroethylene high-pressure reactor liner and a stainless steel shell. The volume of the reactor liner is 100mL.
[0056] In the following embodiments and comparative examples:
[0057] The room temperature is 20-27℃.
[0058] Corona polarization method: Place the round-headed electrode needle directly above the sample and connect the positive and negative electrodes of the power supply to the negative electrode plate below the sample. Gradually increase the voltage until the critical voltage is reached for corona discharge. The distance between the discharge needle tip and the film is 1.5 cm, the working voltage is 8 kV, and the polarization is carried out at room temperature for 50 minutes.
[0059] Electrometer test output potential: Spray gold on both sides of the sample film to prepare the counter electrode, connect it with copper wire, and package it with PTE sheet to obtain the packaged sample. Connect the counter electrode to the copper wire and connect it to the electrometer. Bend the sample to the same degree (15-30°), and the electrometer will display the piezoelectric signal generated on the surface of the test sample connected by the copper wire.
[0060] Example 1
[0061] (1) 16.7 mg of zinc acetate dihydrate and 1 mL of N,N-dimethylformamide (DMF) solvent were mixed and stirred for 60 min, and then 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and the stirring was continued for 4 h to form a mixed solution; the mixed solution was transferred to a tempered glass plate, coated into a strip with a thickness of 0.5 mm, and dried at a relative vacuum degree of -0.1 MPa and 37° C. until the DMF solvent was completely evaporated to obtain a dried strip; the dried strip was annealed at 210° C. for 60 min to obtain a PVTF polymer film with seeds;
[0062] (2) dissolving 0.02 mol of zinc nitrate hexahydrate and 0.02 mol of hexamethylenetetramine in 1 L of deionized water to prepare a growth solution;
[0063] (3) placing the PVTF polymer film with seed crystals obtained in step (1) in the inner liner of a reactor, adding 80 mL of the growth solution obtained in step (2) to the inner liner of the reactor, placing the inner liner of the reactor in the outer shell of the reactor, tightening the lid of the reactor, and keeping the temperature at 90° C. for 4 h for hydrothermal reaction. After unloading the reactor, naturally cool it, wash the reaction product with deionized water, and then dry it at 37° C. to obtain a composite film;
[0064] (4) in an air atmosphere, the composite film obtained in step (3) was kept on a hot plate at 210° C. for 5 min and then quenched, and horizontally stretched at room temperature with a stretching ratio of 1:3 (the stretching ratio refers to the length ratio of the stretched portion of the film before and after stretching) to obtain a stretched composite film;
[0065] (5) The stretched composite film obtained in step (4) was kept on a hot plate at 180° C. for 3 min to obtain the target product 1.
[0066] The target product 1 obtained in Example 1 and the composite film obtained in step (3) were subjected to X-ray diffraction analysis, and the XRD patterns thereof are as follows: Figure 1 shown. Figure 1 In the figure, the peak at 19.9° corresponds to the β phase in PVTF, and the (100)(002)(101) crystal plane peaks correspond to ZnO. It can be seen that both the target product 1 and the composite film obtained in step (3) contain vinylidene fluoride trifluoroethylene copolymer and ZnO crystals. Moreover, the zinc oxide in the composite film obtained in step (3) has a (002) C-axis preferred orientation, while the relative intensity of the diffraction peak of the zinc oxide (002) preferred orientation in the target product 1 is weakened, which shows that after directional stretching, the film composition and crystal structure have not changed, but the vertically grown zinc oxide is effectively tilted under the stretching action and presents a horizontally oriented state.
[0067] The target product 1 obtained in this Example 1 was subjected to FTIR analysis, and its FTIR graph is as follows Figure 2 shown. Figure 2 Medium, 843cm -1 With 1285cm -1 The peak position represents CF 2 Symmetric stretching vibration of the group, 1400 cm -1 The peak position represents CH 2 The swinging vibration of the groups indicated that the target product 1 contained vinylidene fluoride-trifluoroethylene copolymer.
[0068] The composite film obtained in step (3) of this embodiment and the target product 1 obtained were subjected to scanning electron microscopy analysis. Figure 3A and Figure 3B shown. Figure 3AIn the composite film, there are several disorderly arranged nanorods on the surface, the length of the nanorods is 1000-2500nm, and the diameter of the nanorods is 90-220nm; Figure 3B In the figure, there are several horizontally oriented nanorods on the surface of the target product 1, with a length of 1000-2500nm and a diameter of 90-220nm. The comparison of SEM images also proves that after directional stretching, the vertically grown zinc oxide nanorods are effectively tilted under the stretching action and present a horizontally oriented state.
[0069] In summary, the target product 1 is a PVTF composite film having horizontally oriented zinc oxide nanorods on the surface.
[0070] The pure PVTF and the target product 1 obtained in Example 1 were polarized by corona polarization, with a polarization voltage of 8 kV and a polarization time of 50 min. The surface electrical signals (i.e., output potential) generated by the two films after polarization under the same deformation conditions were tested by an electrometer. The results are shown in Table 1. Figure 4A and Figure 4B It can be found that: under the same degree of bending deformation, the target product 1 obtained in Example 1 produces a surface electrical signal change of about 2.5V, while pure PVTF produces a surface electrical signal change of about 1.25V. It can be seen that, compared with pure PVTF, the composite film with horizontally oriented zinc oxide nanorods on the surface in the target product 1 obtained in this Example 1 can produce a stronger surface electrical signal after polarization treatment, which means that the zinc oxide nanorod structure with horizontally oriented surface helps to improve the piezoelectric response effect of the polarized film under bending deformation.
[0071] Example 2
[0072] (1) 8.4 mg of zinc acetate dihydrate and 1 mL of N,N-dimethylformamide (DMF) solvent were mixed and stirred for 60 min, and then 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and the stirring was continued for 4 h to form a mixed solution; the mixed solution was transferred to a tempered glass plate, coated into a strip with a thickness of 0.5 mm, and dried at a relative vacuum degree of -0.1 MPa and 37°C until the DMF solvent was completely evaporated to obtain a dried strip; the dried strip was annealed at 210°C for 60 min to obtain a PVTF polymer film with seed crystals;
[0073] (2) dissolving 0.02 mol of zinc nitrate hexahydrate and 0.02 mol of hexamethylenetetramine in 1 L of deionized water to prepare a growth solution;
[0074] (3) placing the PVTF polymer film with seed crystals obtained in step (1) in the inner liner of a reactor, adding 80 mL of the growth solution obtained in step (2) to the inner liner of the reactor, placing the inner liner of the reactor in the outer shell of the reactor, tightening the lid of the reactor, and keeping the temperature at 90° C. for 4 h for hydrothermal reaction. After unloading the reactor, naturally cool it, wash the reaction product with deionized water, and then dry it at 37° C. to obtain a composite film;
[0075] (4) in an air atmosphere, the composite film obtained in step (3) was kept on a hot plate at 210° C. for 5 min and then quenched, and horizontally stretched at room temperature with a stretching ratio of 1:3 (the stretching ratio refers to the length ratio of the stretched portion of the film before and after stretching) to obtain a stretched composite film;
[0076] (5) The stretched composite film obtained in step (4) was kept on a hot plate at 180° C. for 3 min to obtain the target product 2.
[0077] The target product 2 obtained in Example 2 and the composite film obtained in step (3) were subjected to X-ray diffraction analysis, and the XRD patterns thereof are as follows: Figure 5 shown. Figure 5 In the graph, the peak at 19.9° corresponds to the β phase in PVTF, and the (100)(002)(101) crystal plane peaks correspond to ZnO. It can be seen that both the target product 2 and the composite film obtained in step (3) contain vinylidene fluoride trifluoroethylene copolymer and ZnO crystals. Moreover, the zinc oxide in the composite film obtained in step (3) has a (002) C axis preferred orientation, while the relative intensity of the diffraction peak of the zinc oxide (002) preferred orientation in the target product 2 is weakened, which shows that after directional stretching, the film composition and crystal structure have not changed, but the vertically grown zinc oxide is effectively tilted under the stretching action and presents a horizontally oriented state. The SEM image also confirms this point. There are several horizontally oriented nanorods on the surface of the target product 2, the length of the nanorods is 500 to 1200 nm, and the diameter of the nanorods is 80 to 120 nm. That is, the target product 2 is a PVTF composite film with horizontally oriented zinc oxide nanorods on the surface.
[0078] Example 3
[0079] (1) 5.0 mg of zinc acetate dihydrate and 1 mL of N,N-dimethylformamide (DMF) solvent were mixed and stirred for 60 min, and then 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and the mixture was stirred for 4 h to form a mixed solution; the mixed solution was transferred to a tempered glass plate, coated into a strip with a thickness of 0.5 mm, and dried at a relative vacuum degree of -0.1 MPa and 37° C. until the DMF solvent was completely evaporated to obtain a dried strip; the dried strip was annealed at 210° C. for 60 min to obtain a PVTF polymer film with seeds;
[0080] (2) dissolving 0.02 mol of zinc nitrate hexahydrate and 0.02 mol of hexamethylenetetramine in 1 L of deionized water to prepare a growth solution;
[0081] (3) placing the PVTF polymer film with seed crystals obtained in step (1) in the inner liner of a reactor, adding 80 mL of the growth solution obtained in step (2) to the inner liner of the reactor, placing the inner liner of the reactor in the outer shell of the reactor, tightening the lid of the reactor, and keeping the temperature at 90° C. for 4 h for hydrothermal reaction. After unloading the reactor, naturally cool it, wash the reaction product with deionized water, and then dry it at 37° C. to obtain a composite film;
[0082] (4) in an air atmosphere, the composite film obtained in step (3) was kept on a hot plate at 210° C. for 5 min and then quenched, and horizontally stretched at room temperature with a stretching ratio of 1:3 (the stretching ratio refers to the length ratio of the stretched portion of the film before and after stretching) to obtain a stretched composite film;
[0083] (5) The stretched composite film obtained in step (4) was kept on a hot plate at 180° C. for 3 min to obtain the target product 3.
[0084] XRD and SEM tests showed that the target product 3 was a PVTF composite film with horizontally oriented zinc oxide nanorods on the surface.
[0085] Example 4
[0086] (1) 823 mg of zinc acetate dihydrate was dissolved in 100 mL of deionized water to prepare a 0.0375 mol / L zinc acetate solution, and ammonium hydroxide was added dropwise thereto until the pH reached 9.2, and the mixture was stirred for 20 min to obtain a hydrothermal precursor solution; 80 mL of the hydrothermal precursor solution was placed in a reactor liner, and the reactor liner was placed in the reactor shell, the reactor cover was tightened, and the reaction was carried out at 80° C. for 6 h for hydrothermal reaction, and the reaction was carried out naturally after the reactor was unloaded, and the mixture was washed with deionized water and anhydrous ethanol in turn, centrifuged, and dried at 37° C. to obtain zinc oxide nanorod powder;
[0087] (2) 16.7 mg of the zinc oxide nanorod powder obtained in step (1) was mixed with 1 mL of N,N-dimethylformamide (DMF), and ultrasonically dispersed for 20 min. Then, 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and stirring was continued for 4 h to form a mixed solution. The mixed solution was transferred to a tempered glass plate and coated into a strip with a thickness of 0.5 mm. The strip was dried at 120° C. until the DMF solvent was completely volatilized to obtain a composite film.
[0088] (3) The composite film obtained in step (2) was horizontally stretched at room temperature with a stretching ratio of 1:3, and then kept on a hot plate at 180° C. for 3 min to obtain the target product 4.
[0089] The target product 4 obtained in Example 4 and the composite film obtained in step (2) were subjected to X-ray diffraction analysis, and the XRD pattern thereof is as follows: Figure 6 shown. Figure 6 In the figure, the peak at 19.9° corresponds to the β phase in PVTF, and the (100)(101)(110) crystal plane peaks correspond to ZnO. It can be seen that both the target product 4 and the composite film obtained in step (2) contain vinylidene fluoride trifluoroethylene copolymer and ZnO crystals. Moreover, the relative intensity of the diffraction peaks of zinc oxide (100)(101) and (110) with non-C-axis preferential orientation in the target product 4 is enhanced, which indicates that after directional stretching, the film composition and crystal structure have not changed, but the tilted zinc oxide is effectively tilted under the stretching action and presents a horizontally oriented state.
[0090] At the same time, the zinc oxide powder obtained in step (1) of this embodiment 4 and the cross section of the target product 4 obtained in embodiment 4 were analyzed by scanning electron microscope, and the SEM images were as follows: Fig. 7A and Figure 7B It can be found that the zinc oxide powder obtained in step (1) is zinc oxide nanorods, the length of the nanorods is 800-2000nm, and the diameter of the nanorods is 60-100nm; the target product 4 obtained in Example 4 has a plurality of nanorods arranged in a horizontal orientation, the length of the nanorods is 800-2000nm, and the diameter of the nanorods is 60-100nm.
[0091] That is, the target product 4 is a PVTF composite film having horizontally oriented zinc oxide nanorods inside.
[0092] Example 5
[0093] (1) 823 mg of zinc acetate dihydrate was dissolved in 100 mL of deionized water to prepare a 0.0375 mol / L zinc acetate solution, and ammonium hydroxide was added dropwise thereto until the pH reached 9.2, and stirred for 20 min; an appropriate amount of the obtained solution was placed in the inner tank of a reaction kettle (the volume of the solution was 80% of the volume of the inner tank of the reaction kettle), and then the inner tank of the reaction kettle was placed in the outer shell of the reaction kettle, and the lid of the reaction kettle was tightened, and the reaction was kept at 80° C. for 6 h for hydrothermal reaction, and the solution was washed with deionized water and anhydrous ethanol in turn, centrifuged and dried at 37° C. to obtain zinc oxide nanorod powder;
[0094] (2) 3.3 mg of the zinc oxide nanorod powder obtained in step (1) was mixed with 1 mL of N,N-dimethylformamide (DMF), and ultrasonically dispersed for 20 min. Then, 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and stirring was continued for 4 h to form a mixed solution. The mixed solution was transferred to a tempered glass plate and coated into a strip with a thickness of 0.5 mm. The strip was dried at 120° C. until the DMF solvent was completely volatilized to obtain a composite film.
[0095] (3) The composite film obtained in step (2) was horizontally stretched at room temperature with a stretching ratio of 1:3, and then kept on a hot plate at 180° C. for 3 min to obtain the target product 5.
[0096] XRD test shows that PVTF and ZnO crystals exist in the target product 5, and the relative intensity of the diffraction peak of the non-C-axis preferred orientation of zinc oxide is enhanced. Figure 8 ) shows that there are a number of horizontally oriented nanorods inside the target product 5. That is, the target product 5 is a PVTF composite film having horizontally oriented zinc oxide nanorods inside.
[0097] Example 6
[0098] (1) 823 mg of zinc acetate dihydrate was dissolved in 100 mL of deionized water to prepare a 0.0375 mol / L zinc acetate solution, and ammonium hydroxide was added dropwise thereto until the pH reached 9.2, and stirred for 20 min; an appropriate amount of the obtained solution was placed in the inner tank of a reaction kettle (the volume of the solution was 80% of the volume of the inner tank of the reaction kettle), and then the inner tank of the reaction kettle was placed in the outer shell of the reaction kettle, and the lid of the reaction kettle was tightened, and the reaction was kept at 80° C. for 6 h for hydrothermal reaction, and the solution was washed with deionized water and anhydrous ethanol in turn, centrifuged and dried at 37° C. to obtain zinc oxide nanorod powder;
[0099] (2) 5 mg of the zinc oxide nanorod powder obtained in step (1) was mixed with 1 mL of N,N-dimethylformamide (DMF), and ultrasonically dispersed for 20 min. Then, 133 mg of polyvinylidene fluoride (PVDF) was added thereto, and stirring was continued for 8 h to form a mixed solution. The mixed solution was transferred to a tempered glass plate and coated into a strip with a thickness of 0.5 mm. The strip was dried at 120° C. until the DMF solvent was completely volatilized to obtain a composite film.
[0100] (3) The composite film obtained in step (2) was horizontally stretched at room temperature at a stretching ratio of 1:1.5, and then kept on a hot plate at 180° C. for 3 min to obtain the target product 6.
[0101] XRD test shows that PVDF and ZnO crystals exist in the target product 6, and the relative intensity of the diffraction peak of zinc oxide non-C-axis preferred orientation is enhanced. At the same time, the cross section of the target product 6 obtained in this embodiment 6 is analyzed by scanning electron microscopy. The SEM image is as follows: Fig. 9 As shown. It can be found that there are a number of horizontally oriented nanorods inside the target product 6. That is, the target product 6 is a PVDF composite film with horizontally oriented zinc oxide nanorods inside.
[0102] Example 7
[0103] (1) 823 mg of zinc acetate dihydrate was dissolved in 100 mL of deionized water to prepare a 0.0375 mol / L zinc acetate solution, and ammonium hydroxide was added dropwise thereto until the pH reached 9.2, and stirred for 20 min; an appropriate amount of the obtained solution was placed in the inner tank of a reaction kettle (the volume of the solution was 80% of the volume of the inner tank of the reaction kettle), and then the inner tank of the reaction kettle was placed in the outer shell of the reaction kettle, and the lid of the reaction kettle was tightened, and the reaction was kept at 80° C. for 6 h for hydrothermal reaction, and the solution was washed with deionized water and anhydrous ethanol in turn, centrifuged and dried at 37° C. to obtain zinc oxide nanorod powder;
[0104] (2) 2.5 mg of the zinc oxide nanorod powder obtained in step (1) and 1 mL of 1,4-dioxane were mixed and ultrasonically dispersed for 20 min, and then 50 mg of polylactic acid was added thereto. The mixture was stirred for 10 h to form a mixed solution. The mixed solution was transferred to a tempered glass plate and coated into a strip with a thickness of 0.5 mm. The strip was dried at 37° C. until the 1,4-dioxane solvent was completely volatilized to obtain a composite film.
[0105] (3) The composite film obtained in step (2) was horizontally stretched at room temperature with a stretching ratio of 1:2, and then kept on a hot plate at 180° C. for 3 min to obtain the target product 7.
[0106] XRD test shows that polylactic acid and ZnO crystals exist in the target product 7, and the relative intensity of the diffraction peak of the non-C-axis preferred orientation of zinc oxide is enhanced. At the same time, the cross section of the target product 7 obtained in this example 7 is analyzed by scanning electron microscopy. The SEM image is as follows: Fig.10 As shown, it can be found that there are a number of horizontally oriented nanorods inside the target product 7. That is, the target product 7 is a polylactic acid composite film having horizontally oriented zinc oxide nanorods inside.
[0107] Example 8
[0108] (1) 823 mg of zinc acetate dihydrate was dissolved in 100 mL of deionized water to prepare a 0.0375 mol / L zinc acetate solution, and ammonium hydroxide was added dropwise thereto until the pH reached 9.2, and stirred for 20 min; the obtained solution was placed in a reactor liner (the volume of the solution was 80% of the volume of the reactor liner), and then the reactor liner was placed in the reactor shell, the reactor cover was tightened, and the reaction was carried out at 80° C. for 6 h for hydrothermal reaction, and the solution was washed with deionized water and anhydrous ethanol in turn, centrifuged and dried at 37° C. to obtain zinc oxide nanorod powder;
[0109] (2) 8.4 mg of the zinc oxide nanorod powder obtained in step (1) was mixed with 1 mL of N,N-dimethylformamide (DMF), and ultrasonically dispersed for 20 min. Then, 167 mg of vinylidene fluoride trifluoroethylene copolymer (PVTF) was added thereto, and stirring was continued for 4 h to form a mixed solution. The mixed solution was transferred to a tempered glass plate and coated into a strip with a thickness of 0.5 mm. The strip was dried at 120° C. until the DMF solvent was completely volatilized to obtain a composite film.
[0110] (3) The composite film obtained in step (2) was horizontally stretched at room temperature with a stretching ratio of 1:3, and then kept on a hot plate at 180° C. for 3 min to obtain the target product 8.
[0111] XRD and SEM tests show that: PVTF and ZnO crystals exist in the target product 8, and the relative intensity of the diffraction peak of the non-C-axis preferred orientation of zinc oxide is enhanced; the target product 8 is a PVTF composite film with horizontally oriented zinc oxide nanorods inside.
[0112] As can be seen from Examples 1 to 8, by two different preparation methods, horizontally oriented zinc oxide nanorods can be obtained on the surface or inside of the PVTF composite film, respectively. Moreover, both preparation methods can be achieved by simple hydrothermal and stretching methods, which are convenient and simple and easy to control. For example, the density of the zinc oxide nanorods arranged on the surface or inside of the composite film per unit area and the size of the zinc oxide nanorods can be adjusted by adjusting parameters such as the raw material feed amount, stretch ratio, reaction temperature and time, so as to achieve the piezoelectric voltage output size and piezoelectric sensitivity of the composite film doped with zinc oxide nanorods when subjected to the same external force. The performance is regulated, so as to design a suitable self-powered film for different tissue repair needs. Different from the general hydrothermal growth of disordered and chaotically arranged zinc oxide nanorods, the deformation caused by the mutual force offset when subjected to external force is insufficient. The composite film of the present invention is conducive to generating a larger deformation under the action of external force, especially when bending, thereby generating a better electromechanical response. Moreover, in Example 1, under the same degree of bending deformation, the surface electrical signal change generated by the composite film of the present invention is about twice the surface electrical signal change generated by the pure piezoelectric polymer. It is obvious that the composite film with horizontally oriented zinc oxide nanorods on the surface can generate a stronger surface electrical signal after polarization treatment, which means that the zinc oxide nanorod structure with horizontally oriented surface helps to improve the piezoelectric response effect of the polarized film under bending deformation.
[0113] It can be seen that the purpose of the present invention has been completely and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments. Without departing from the principles, the implementation methods can be modified arbitrarily. Therefore, the present invention includes all modified implementation methods based on the spirit and scope of the claims.
Claims
1. A zinc oxide / piezoelectric polymer composite film, comprising a piezoelectric polymer film and zinc oxide nanorods, characterized in that: The zinc oxide nanorods are arranged in a horizontal orientation, and the zinc oxide nanorods are arranged on the surface and / or inside of the piezoelectric polymer film.
2. The zinc oxide / piezoelectric polymer composite film according to claim 1, characterized in that: The diameter of the zinc oxide nanorod is 20-600nm.
3. The zinc oxide / piezoelectric polymer composite film according to claim 1, characterized in that: The length of the zinc oxide nanorods is 0.2-20 μm.
4. The zinc oxide / piezoelectric polymer composite film according to any one of claims 1 to 3, characterized in that: The polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea.
5. The method for preparing the zinc oxide / piezoelectric polymer composite film according to any one of claims 1 to 4, comprising the following steps: (1) zinc acetate dihydrate and a solvent are mixed, stirred for 10 to 180 minutes, and then a piezoelectric polymer is added thereto, and the stirring is continued for 2 hours to 10 hours to form a mixed solution, wherein the feed ratio of the solvent, zinc acetate dihydrate, and piezoelectric polymer is 1 mL: (0.8 to 55) mg: (40 to 220) mg; the mixed solution is transferred to a substrate, coated into a strip with a thickness of 0.1 mm to 1.5 mm, and dried at a relative vacuum degree of -0.1 to 0 MPa and 30 to 80° C. until the solvent is completely volatilized to obtain a dried strip; the dried strip is annealed at 140 to 300° C. for 30 to 90 minutes to obtain a polymer film with seeds; (2) dissolving zinc nitrate hexahydrate and hexamethylenetetramine in a molar ratio of 1:1 in deionized water to prepare a growth solution; in the growth solution, the concentration of zinc nitrate hexahydrate is 0.005-0.05 mol / L, and the concentration of hexamethylenetetramine is 0.005-0.05 mol / L; (3) placing the polymer film with seed crystals obtained in step (1) in a reactor liner, adding the growth solution into the reactor liner, placing the reactor liner in a reactor shell, and performing a hydrothermal reaction at 80 to 140° C. for 1 to 8 hours. After unloading the reactor, washing the reaction product and drying it to obtain a composite film; (4) in an air atmosphere, the composite film is kept on a hot plate at 160 to 300° C. for 0 to 30 minutes and then quenched, and then horizontally stretched at 25 to 100° C. at a stretching ratio of 1:1 to 1:15 to obtain a stretched composite film; (5) The stretched composite film is kept on a hot plate at 140 to 300° C. for 0 to 30 min to obtain the target product.
6. The preparation method according to claim 5, characterized in that: The method further comprises step (6): polarizing the target product obtained in step (5) by using contact polarization or corona polarization.
7. The preparation method according to claim 5 or 6, characterized in that: In step (1), the polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea; and the solvent is selected from at least one of N,N-dimethylformamide, dioxane, dichloromethane and acetone.
8. The method for preparing the zinc oxide / piezoelectric polymer composite film according to any one of claims 1 to 4, comprising the following steps: (1) dissolving zinc acetate dihydrate in deionized water to obtain a zinc acetate solution with a concentration of 0.01 to 0.1 mol / L, adding ammonium hydroxide dropwise thereto until the pH reaches 9 to 9.5, stirring for 20 to 60 minutes, and obtaining a mixed solution; taking an appropriate amount of the mixed solution and placing it in a reactor liner, placing the reactor liner in a reactor shell, and keeping the temperature at 80 to 140° C. for 2 to 10 hours for a hydrothermal reaction, washing the reaction product after unloading the reactor, centrifuging it, and drying it to obtain zinc oxide nanorod powder; (2) mixing the zinc oxide nanorod powder obtained in step (1) with a solvent, and ultrasonically dispersing the mixture for 10 to 120 minutes, and then adding a piezoelectric polymer thereto, and continuing stirring for 2 to 10 hours to form a mixed solution, wherein the feed ratio of the solvent, zinc acetate dihydrate, and piezoelectric polymer is 1 mL: (0.4 to 22) mg: (40 to 220) mg; transferring the mixed solution to a substrate, coating it into a strip with a thickness of 0.1 to 1.5 mm, and drying the strip at 25 to 140° C. until the solvent is completely volatilized, to obtain a composite film; (3) The composite film obtained in step (2) is horizontally stretched at a stretching ratio of 1:1 to 1:15 at 25 to 140° C., and then kept on a hot plate at 140 to 300° C. for 0 to 30 minutes to obtain the target product.
9. The preparation method according to claim 8, characterized in that: The method further comprises step (4): subjecting the target product obtained in step (3) to electric polarization treatment by using contact electric polarization or corona polarization method.
10. The preparation method according to claim 8 or 9, characterized in that: In step (1), the polymer is selected from at least one of polyvinylidene fluoride, vinylidene fluoride trifluoroethylene copolymer, polytrifluoroethylene, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluorochlorovinyl ether, polylactic acid, polyamide, polyacrylonitrile, odd-numbered nylon, silk fibroin, polyhydroxybutyrate, polyhydroxybutyrate valerate and polyurea; and the solvent is selected from at least one of N,N-dimethylformamide, dioxane, dichloromethane and acetone.