Modified lysine-based polymers and compositions comprising same

By performing Michael addition reaction on the lysine polymer, a biodegradable detergent composition is formed, which solves the problems of high toxicity and corrosion in the manufacturing process of existing bio-based dispersants, and achieves low cost and low toxicity and efficient detergent production.

CN119032120APending Publication Date: 2024-11-26BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032496.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-04
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing bio-based dispersants have high toxicity and corrosion in the manufacturing process, resulting in increased environmental pollution and production costs, and it is difficult to achieve the demand for biodegradable detergents.

Method used

The lysine-based polymer is used to modify its anti-ashing properties by using unsaturated carboxylic acids or unsaturated carboxylic acid esters to form a biodegradable detergent composition for use as a dispersant.

Benefits of technology

A biodegradable dispersant with acceptable ash resistance and primary detergent under low cost and low toxicity conditions is achieved, reducing the risk of pollution to the environment and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070290910000081
    Figure BDA0005070290910000081
  • Figure BDA0005070290910000082
    Figure BDA0005070290910000082
  • Figure BDA0005070290910000101
    Figure BDA0005070290910000101
Patent Text Reader

Abstract

The present invention relates to a modified lysine-based polymer obtainable or obtained by a process comprising subjecting at least a portion of the free amino groups in a lysine-based polymer to Michael addition with a Michael acceptor selected from at least one of unsaturated carboxylic acids and unsaturated carboxylic acid esters, and a detergent composition comprising the modified lysine-based polymer. The invention also relates to a method of preserving an aqueous detergent composition comprising a modified lysine-based polymer, and to a method of washing fabrics or cleaning hard surfaces using a detergent composition comprising a modified lysine-based polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modified lysine-based polymer, a detergent composition comprising the modified lysine-based polymer, and use of the modified lysine-based polymer in a detergent composition, in particular as a dispersant. Background Art

[0002] Dispersants play an important role in various industrial and household formulations today, for example in laundry detergent formulations to prevent graying of textiles. Dispersants are developed with a view to achieving a dispersing effect, in order to avoid undesirable phenomena such as scaling or dirt deposits, for example during washing and cleaning processes.

[0003] Most dispersants used today are petroleum-based rather than bio-based. Recently, bio-based products and products containing bio-based ingredients have been gaining more and more attention from consumers due to the sustainability of biomass resources. In the context of this trend, bio-based dispersants have brought new challenges to manufacturers, especially in household detergent applications.

[0004] WO 2021228642 A1 discloses the use of carboxymethylated polylysine as a dispersant. Carboxymethylated polylysine is manufactured by, for example, modifying biodegradable polylysine with chloroacetate. Although carboxymethylated polylysine shows acceptable anti-ashing performance, its manufacture still has the disadvantage that sodium chloroacetate is toxic and corrosive. The residue of the modifier chloroacetate in the final product should be strictly limited due to its toxicity. In addition, due to the corrosiveness of chloroacetate, a container made of special and expensive materials is required to handle it.

[0005] Therefore, there is a need to provide a biodegradable chemical as a dispersant that can be used in industrial and household formulations. It would be more desirable if the biodegradable dispersant could be made from less toxic and corrosive materials and at reduced cost. Summary of the invention

[0006] It is an object of the present invention to provide a biodegradable chemical which can provide at least acceptable anti-ashing performance and / or primary detergency for detergents, in particular for laundry detergents, and which can be manufactured using a more cost-effective process.

[0007] It has been found that the objects of the present invention can be achieved by lysine-based polymers in which at least a portion of the free amino groups contained in the polymer have been modified via Michael addition with unsaturated carboxylic acids or unsaturated carboxylic acid esters.

[0008] In one aspect, the present invention relates to a modified lysine-based polymer obtainable or obtained by a process comprising subjecting at least a portion of the free amino groups in the lysine-based polymer to Michael addition with a Michael acceptor selected from unsaturated carboxylic acids and unsaturated carboxylic acid esters.

[0009] In another aspect, the present invention relates to a detergent composition comprising the modified lysine-based polymer as described in the first aspect.

[0010] In yet another aspect, the present invention relates to the use of the modified lysine-based polymer as described in the first aspect in a detergent composition.

[0011] In a further aspect, the present invention relates to the use of a modified lysine-based polymer as described in the first aspect as a dispersant.

[0012] It has been found that the modified lysine-based polymers according to the present invention show acceptable anti-ashing performance and primary detergency compared to commercially available non-biodegradable chelating agents and dispersants, while being biodegradable. In addition, the unsaturated carboxylic acids and unsaturated carboxylic acid esters as modifiers are less toxic and less corrosive than chloroacetic acid and its salts used to make biodegradable carboxymethylated polylysine in WO 2021228642 A1. DETAILED DESCRIPTION

[0013] The present invention will now be described in detail below. It should be understood that the present invention can be implemented in many different ways and should not be construed as being limited to the embodiments set forth herein. Unless otherwise mentioned, all technical terms and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs.

[0014] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0015] As used herein, the terms "comprise," "comprising," and the like are used interchangeably with "contain," "containing," and the like and are to be interpreted in a non-limiting, open-ended manner. That is, for example, additional components or elements may be present. The expression "consisting of" or "consisting essentially of," or cognates may be included in "comprise" or cognates.

[0016] As used herein, the term "biodegradable" generally refers to materials that are capable of being degraded by the action of naturally occurring microorganisms (such as bacteria, fungi and algae), ambient heat, moisture or other environmental factors.

[0017] As used herein, the term "lysine-based polymer" is intended to mean a polymer in which lysine accounts for the major molar proportion, i.e., greater than 50 mol% of all monomers constituting the polymer, which can be a homopolymer of lysine in which lysine accounts for 100 mol% of the monomers constituting the polymer or a copolymer of lysine and one or more comonomers.

[0018] As used herein, the term "free amino group" refers to an amino group -NH2 that has not undergone condensation with a carboxyl group or modification via Michael addition.

[0019] As used herein, the term "modified lysine-based polymer" is intended to refer to a lysine-based polymer containing amino groups that have been modified via Michael addition of free amino groups contained in the lysine-based polymer with an unsaturated carboxylic acid or an unsaturated carboxylic acid ester. It should be understood that the term "modified lysine-based polymer" is intended to encompass unneutralized, partially neutralized, and fully neutralized forms with respect to any carboxyl groups that may be present in the polymer.

[0020] As used herein, the term "structural unit" is intended to refer to the smallest molecular residue derived from a monomer after polymerization (i.e., polycondensation of the monomer). It should be understood that the term "structural unit" may also contain a moiety derived from a Michael acceptor if free amino groups are present after polycondensation of the monomer and the amino groups are modified via Michael addition.

[0021] Herein, the terms "one or more structural units from a lysine monomer" and "one or more lysine structural units" are used interchangeably. Likewise, the terms "structural units from at least one dicarboxylic acid of formula (I)" and "one or more dicarboxylic acid structural units" are used interchangeably.

[0022] As used herein, unless the context clearly indicates otherwise, when referring to the modified lysine-based polymer according to the present invention, the K-value refers to the corresponding parameter of the lysine-based polymer before modification via Michael addition.

[0023] <Modified lysine-based polymer>

[0024] The modified lysine-based polymer according to the present invention may be a modified lysine homopolymer, or a modified copolymer of a major proportion (eg, greater than 50 mol%) of lysine and a minor proportion (eg, less than 50 mol%) of at least one other monomer.

[0025] Useful unsaturated carboxylic acids as Michael acceptors for modifying lysine-based polymers via Michael addition can be selected from the group consisting of α,β-ethylenically unsaturated monocarboxylic acids having 3 to 10 carbon atoms, α,β-ethylenically unsaturated dicarboxylic acids having 4 to 8 carbon atoms, α,β-ethylenically unsaturated tricarboxylic acids having 4 to 8 carbon atoms, and α,β-ethylenically unsaturated carboxylic acids having more carboxylic acid groups.

[0026] Preferably, the unsaturated carboxylic acid may be selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid and aconitic acid.

[0027] More preferably, the unsaturated carboxylic acid may be selected from the group consisting of acrylic acid, maleic acid and itaconic acid, among which acrylic acid may be particularly mentioned.

[0028] Unsaturated carboxylic acid esters available as Michael acceptors for modifying lysine-based polymers via Michael addition may be selected from any ester of unsaturated carboxylic acids as described above. Preferably, the unsaturated carboxylic acid ester may be selected from polyoxyalkylene esters or blocked polyoxyalkylene esters of unsaturated carboxylic acids as described above, preferably blocked polyethylene oxide esters, blocked polypropylene oxide esters or blocked polybutylene oxide esters of unsaturated carboxylic acids as described above, or combinations thereof. More preferably, blocked polyethylene oxide esters of unsaturated carboxylic acids may be mentioned, such as blocked polyethylene oxide esters of acrylic acid, maleic acid or itaconic acid, in particular acrylic acid.

[0029] In the capped polyoxyalkylene esters of unsaturated carboxylic acids, suitable capping groups can be selected from C1-C4-alkyl or C1-C4-hydroxyalkyl groups, such as methyl, ethyl, propyl, isopropyl, butyl, hydroxymethyl, hydroxyethyl, hydroxypropyl or hydroxybutyl.

[0030] Examples of end-capped polyoxyalkylene esters of unsaturated carboxylic acids may include, but are not limited to, polyethylene oxide mono(C1-C4-alkyl) ether acrylates, polyethylene oxide mono(C1-C4-alkyl) ether maleates, polyethylene oxide mono(C1-C4-alkyl) ether itaconates, preferably polyethylene oxide monomethyl ether acrylates, polyethylene oxide monomethyl ether maleates, polyethylene oxide monomethyl ether itaconates, more preferably polyethylene oxide monomethyl ether acrylates.

[0031] The polyalkylene oxide moiety in the polyalkylene oxide ester of unsaturated carboxylic acid or the capped polyalkylene oxide ester may have a number average molecular weight of 100 to 2,000, preferably 200 to 1,200, more preferably 400 to 800.

[0032] The unsaturated carboxylic acids and unsaturated carboxylic acid esters that can be used to modify the lysine-based polymers in the present invention are also generally referred to herein as Michael acceptors.

[0033] As homopolymers of lysine to be modified (also referred to as lysine homopolymers), both straight-chain polylysine and branched polylysine are available. Known polylysine can have a straight-chain or branched structure, depending on the production process. For example, ε-straight-chain polylysine is generally prepared by a microbial fermentation process as is well known in the art. Since lysine has one reactive carboxyl group and two reactive amino groups (α-NH2 and ε-NH2) / molecule, branched polylysine is generally produced by thermal polycondensation of lysine. For purposes of the present invention, the type of polylysine structure (straight or branched), the arrangement of those structural units, and the degree of branching are not critical.

[0034] In some embodiments of the present invention, the modified lysine-based polymer may be a linear or branched lysine homopolymer that has been modified with a Michael acceptor as described above. In particular, the lysine homopolymer may be ε-linear polylysine or branched polylysine.

[0035] As the copolymer of lysine to be modified (also referred to as lysine copolymer), the polymerization product of more than 50 mol% of lysine and dicarboxylic acid or its amide-forming derivative is available. Therefore, the copolymer of lysine will contain the amide part produced by lysine and dicarboxylic acid or its amide-forming derivative. The copolymer of lysine can be prepared by the thermal polycondensation of lysine and dicarboxylic acid or any suitable polymerization reaction of lysine and amide-forming derivative of dicarboxylic acid.

[0036] In some other embodiments of the present invention, the modified lysine-based polymer can be a copolymer of lysine that has been modified with a Michael acceptor as described above, wherein the copolymer of lysine comprises greater than 50 mol % of structural units derived from lysine monomers and less than 50 mol % of structural units derived from at least one dicarboxylic acid or its amide-forming derivatives.

[0037] In particular, the copolymer of lysine may be a polymer comprising

[0038] (A) 60 to 99 mol % of structural units derived from lysine monomers,

[0039] (B) 1 to 40 mol % of structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof

[0040] HOOC-R1-COOH (I)

[0041] in

[0042] R1 is a direct bond or an aliphatic straight-chain alkylene group, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted alkyl, unsubstituted or substituted alkoxy, unsubstituted or substituted alkylthio, unsubstituted or substituted alkylamino, di(alkyl)amino, alkylene, hydroxyl, mercapto, amino and halogen.

[0043] As used herein, the term "aliphatic straight chain alkylene group" refers to a divalent group derived from an unsaturated or saturated acyclic hydrocarbon, which may or may not be interrupted by at least one heteroatom selected from O, S and N. Typically, the alkylene group herein will have 1 to 24 carbon atoms (C1-C 24 -alkylene), preferably 1 to 18 carbon atoms (C1-C 18 -alkylene), more preferably 1 to 12 carbon atoms (C1-C 12 -alkylene). Examples of aliphatic straight-chain alkylene groups are especially alkylene and alkenylene.

[0044] As used herein, the term "alkylene" refers to a saturated divalent group derived from a straight chain alkane, which may or may not be interrupted by at least one heteroatom selected from O, S and N. Typically, the alkylene group herein will have 1 to 24 carbon atoms (C1-C 24 -alkylene), preferably 1 to 18 carbon atoms (C1-C 18 -alkylene), more preferably 1 to 12 carbon atoms (C1-C 12 -alkylene), for example C1-C4-alkylene and C1-C2-alkylene. Examples of alkylene are especially methylene, ethylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene, undecamethylene, dodecamethylene, hexamethylene, octadecamethylene, etc.

[0045] As used herein, the term "alkenylene" refers to an unsaturated divalent group derived from a straight chain olefin wherein any double bonds are in an internal position. Typically, alkenylene herein will have 2 to 24 carbon atoms (C2-C 24 -alkenyl), preferably 2 to 18 carbon atoms (C2-C 18 -alkenyl), more preferably 2 to 12 carbon atoms (C2-C 12 Examples of alkenylene are especially ethenylene, 1,3-propenylene, 1,4-but-2-enylene, 1,5-pent-2-enylene, 1,6-hex-3-enylene and the like.

[0046] The term "alkyl" as used herein and in the alkyl portion of alkoxy, alkylthio, alkylamino, dialkylamino, etc., refers to a group generally having 1 to 18 carbon atoms (C1-C 18 -alkyl), preferably 1 to 12 carbon atoms (C1-C12 The term "alkyl" refers to a saturated straight-chain or branched hydrocarbon radical having 1 to 8 carbon atoms (C1-C8-alkyl) or 1 to 6 carbon atoms (C1-C6-alkyl), for example a C1-C4-alkyl and a C1-C2-alkyl radical. Examples of alkyl radicals are especially methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methylbutyl, 1-ethylpropyl, neopentyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 1-ethylbutyl, 2-ethylbutyl, n-heptyl, 1-methylhexyl, 2-methylhexyl, 1-ethylpentyl, 1-propylbutyl, 2-ethylpentyl, n-octyl, 1-methylheptyl, 2-methylheptyl, 1-ethylhexyl, 2-ethylhexyl, 1-propylpentyl, 2-propylpentyl, n-nonyl, etc.

[0047] The term "alkoxy" as used herein refers to an alkyl group attached via an oxygen atom, which may be represented by -O-alkyl, wherein alkyl is as defined above.

[0048] The term "alkylthio" as used herein refers to an alkyl group attached via a sulfur atom, which may be represented by -S-alkyl, wherein alkyl is as defined above.

[0049] As used herein, the terms "alkylamino" and "di(alkyl)amino" refer to an amino group (-NH2) in which the hydrogen atom is replaced by one or two alkyl groups, respectively, wherein alkyl is as defined above.

[0050] As used herein, the term "alkylene" refers to an unsaturated divalent group derived from an alkane having two valences on the same carbon atom, which can be represented by *=CR a R b , where the asterisk (*) indicates the position at which the alkylene group is attached to the rest of the moiety, and R a and R b H or alkyl is provided, respectively. Typically, the alkylene group herein will have 1 to 6 carbon atoms (C1-C6-alkylene), preferably 1 to 4 carbon atoms (C1-C4-alkylene). Examples of alkylene are especially methylene, ethylene, propylene, etc.

[0051] The term "halogen" as used herein refers to fluorine, bromine, chlorine and iodine.

[0052] In a specific embodiment, the modified lysine-based polymer according to the present invention comprises structural units derived from lysine monomers represented by, for example,

[0053]

[0054] in

[0055] R2 and R3 are independently H or R4, provided that at least one of R2 and R3 is R4,

[0056] R4 represents a moiety derived from a Michael acceptor via Michael addition, and

[0057] *Indicates the position where a building block is attached to any other building block via an amide linkage.

[0058] In some embodiments, the modified lysine-based polymer according to the present invention comprises at least one of the structural units (Ua) and (Ub) as described above, wherein R4 in (Ua) and (Ub) represents a moiety represented by formula (II):

[0059]

[0060] in

[0061] R5 and R6 are independently H, C1-C6-alkyl, carboxyl (-COOH), -COOM, -(C1-C4-alkylene)-COOH or -(C1-C4-alkylene)-COOM,

[0062] R7 is H, C1-C6-alkyl, -(CH2CH2O) n -R8 or M,

[0063] R8 is C1-C4-alkyl,

[0064] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0065] n is a number in the range of 2 to 40, and

[0066] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0067] Preferably, the modified lysine-based polymer according to the present invention comprises structural unit (Ua) and / or structural unit (Ub), wherein R4 represents a moiety represented by formula (II), wherein

[0068] R5 and R6 are independently H, C1-C4-alkyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0069] R7 is H, -(CH2CH2O) n -R8 or M,

[0070] R8 is C1-C2-alkyl,

[0071] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0072] n is a number in the range of 4 to 25, and

[0073] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0074] More preferably, the modified lysine-based polymer according to the present invention comprises structural unit (Ua) and / or structural unit (Ub), wherein R4 represents a moiety represented by formula (II), wherein

[0075] R5 is H, methyl, carboxyl (-COOH), or -COOM,

[0076] R6 is H, methyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0077] R7 is H, -(CH2CH2O) n -R8 or M,

[0078] R8 is C1-C2-alkyl,

[0079] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0080] n is a number in the range of 8 to 15, and

[0081] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0082] Most preferably, the modified lysine-based polymer according to the present invention comprises structural unit (Ua) and / or structural unit (Ub), wherein R4 represents a moiety represented by formula (II), wherein

[0083] R5 is H, carboxyl (-COOH), or -COOM,

[0084] R6 is H, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0085] R7 is H, -(CH2CH2O) n -R8 or M,

[0086] R8 is a methyl group,

[0087] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0088] n is a number in the range of 8 to 15, and

[0089] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0090] In particular, the modified lysine-based polymer according to the present invention comprises a structural unit (Ua) and / or a structural unit (Ub) wherein R4 represents a moiety represented by

[0091]

[0092] in,

[0093] R7 is H, -(CH2CH2O) n -R8 or M,

[0094] R8 is a methyl group,

[0095] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0096] n is a number in the range of 8 to 15, and

[0097] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0098] More particularly, R7 in formula (II-1) is H, -(CH2CH2O) n -R8 or M, and in formulas (II-2), (II-3) and (II-4) is H or M, wherein R8, M and n are as described above for formulas (II-1), (II-2), (II-3) and (II-4).

[0099] In each of formula (II) and formulae (II-1) to (II-4) as described above, M is preferably a cation selected from sodium, potassium, calcium, magnesium, ammonium or amine cations.

[0100] Every kind of lysine structural unit as described above can be connected to identical or different lysine structural unit to form amide linking bond, such as *-Ua-Ua-*, *-Ua-Ub-*, *-Ub-Ub-* and any other possible linking bond.Should be understood that the modified polymer based on lysine can comprise more than one type of above amide linking bond.Lysine structural unit as described above can also be connected to dicarboxylic acid structural unit in the case of the multipolymer of lysine as described in the present invention.

[0101] The modified lysine-based polymer according to the present invention may include a dicarboxylic acid structural unit represented by, for example, formula (III),

[0102]

[0103] in

[0104] R1 is as defined herein above for formula (I),

[0105] *Indicates the position where a building block is attached to any other building block via an amide linkage.

[0106] It is to be understood that each building block of formula (III) as described above may be linked to two lysine building blocks by the same or different linkages.

[0107] It should also be understood that when R1 is an alkylene group substituted by an amino group (NH2), the dicarboxylic acid structural unit contained in the carboxyalkyl-modified lysine-based polymer according to the present invention can also be in any other possible form. The amino substituent is reactive with the carboxyl group contained in the lysine monomer and the dicarboxylic acid and can form a corresponding amide linkage.

[0108] In a specific embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 24 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 18 -alkyl, unsubstituted or substituted C1-C 18 -alkoxy, unsubstituted or substituted C1-C 18 -alkylthio, unsubstituted or substituted C1-C 18 -alkylamino, di(C1-C 18 -alkyl)amino, C1-C6-alkylene, hydroxy, mercapto, amino and halogen.

[0109] In a preferred embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 18 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 12 -alkyl, unsubstituted or substituted C1-C 12 -alkoxy, unsubstituted or substituted C1-C 12 -alkylthio, unsubstituted or substituted C1-C 12 -alkylamino, di(C1-C 12 -alkyl)amino, C1-C4-alkylene, hydroxy, mercapto, amino and halogen.

[0110] In a more preferred embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 12 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C8-alkyl, unsubstituted or substituted C1-C8-alkoxy, unsubstituted or substituted C1-C8-alkylthio, unsubstituted or substituted C1-C8-alkylamino, di(C1-C8-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

[0111] In a further preferred embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, unsubstituted or substituted C1-C4-alkoxy, unsubstituted or substituted C1-C4-alkylthio, unsubstituted or substituted C1-C4-alkylamino, di(C1-C4-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

[0112] In a further preferred embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C4-alkylene, hydroxy, mercapto and amino.

[0113] In a most preferred embodiment, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C2-alkylene, hydroxyl and amino.

[0114] In particular, the modified lysine-based polymer according to the present invention comprises (B) structural units derived from at least one of oxalic acid, malonic acid, succinic acid, maleic acid, fumaric acid, tartaric acid, aspartic acid, glutaric acid, itaconic acid, glutamic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid and dodecanedioic acid, more preferably at least one of succinic acid, tartaric acid, glutaric acid, adipic acid, most preferably tartaric acid or adipic acid.

[0115] Preferably, the modified lysine-based polymer according to the present invention comprises

[0116] (A) 70 to 97 mol % of lysine structural units; and

[0117] (B) 3 to 30 mol% of dicarboxylic acid structural units.

[0118] More preferably, the modified lysine-based polymer according to the present invention comprises;

[0119] (A) 75 to 97 mol % of lysine structural units; and

[0120] (B) 4 to 25 mol% of dicarboxylic acid structural units.

[0121] Most preferably, the modified lysine-based polymer according to the present invention comprises

[0122] (A) 75 to 95 mol % of lysine structural units; and

[0123] (B) 5 to 25 mol% of dicarboxylic acid structural units.

[0124] The carboxymethylated lysine-based polymers according to the present invention can be prepared from lysine-based polymers having a K-value in the range of 8 to 20, more preferably 9 to 15, and most preferably 9.5 to 13, as determined according to DIN ISO 1628-1 with a 1 wt% solution of the corresponding lysine-based polymer in water at 23° C. The K-value is generally referred to as intrinsic viscosity and is an indirect measure of the molecular weight of the polymer.

[0125] The modified lysine-based polymer according to the invention has a degree of modification (DM) via Michael addition of at least 10%, for example 20%, 30%, 35%, 40%, 45%, 50%, 60%, 65%, 70%, 80% or more. For example, the DM may be in the range of 10% to 70%, preferably 20% to 50%.

[0126] In this paper, the degree of modification (DM) is theoretically defined according to the following equation:

[0127] The moiety derived from the Michael acceptor after Michael addition

[0128]

[0129] The measurement of DM can be based on the distribution to 1 The resonance signal of the corresponding proton in the hydrolysis product measured by H NMR in D2O is performed by hydrolyzing the modified lysine-based polymer and determining the mole number of the part derived from the Michael acceptor after Michael addition, the mole number of the structural unit of lysine, and the mole number of the dicarboxylic acid structural unit having an amino group when present. It should be understood that the measured DM value may not be completely the same as the theoretical value due to the limitation of the measurement method.

[0130] The modified lysine-based polymer according to the present invention has a weight average molecular weight (Mw) in the range of 600 to 20,000 g / mol, preferably 700 to 17,000 g / mol, more preferably 800 to 13,000 g / mol, and / or has a number average molecular weight (Mn) in the range of 500 to 20,000 g / mol, preferably 600 to 15,000 g / mol, more preferably 700 to 12,000 g / mol. The average molecular weight can be determined according to the method described herein below.

[0131] There are no particular restrictions on the process for preparing the modified lysine-based polymer according to the present invention. Generally, the modified lysine-based polymer according to the present invention can be prepared by a process comprising reacting a lysine-based polymer with a Michael acceptor as described above under controlled conditions for Michael addition between free amino groups and an unsaturated carboxylic acid or an unsaturated carboxylic acid ester as a Michael acceptor. It is conceivable that the modified lysine-based polymer can also be prepared by a process comprising reacting a lysine-based polymer with an unsaturated carboxylic acid as a Michael acceptor and optionally esterifying. Known conditions for Michael addition between free amino groups and unsaturated carboxylic acids or unsaturated carboxylic acid esters can be applied without restriction.

[0132] It has been found that the modified lysine-based polymers according to the present invention are useful as dispersants and / or chelating agents in detergent compositions.

[0133] <Detergent Composition>

[0134] According to the present invention, the detergent composition may be any composition comprising a surfactant or a mixture of surfactants to provide a cleaning benefit. In particular, the detergent composition is a laundry detergent composition.

[0135] There is no restriction on the formulation of the detergent composition. The modified lysine-based polymer according to the present invention can be used in any conventional formulation of a detergent composition such as a laundry detergent composition. It should be understood that the modified lysine-based polymer according to the present invention can be used in a detergent composition in addition to or in place of a dispersant and / or a chelating agent (which would otherwise be included in a conventional formulation of a detergent composition).

[0136] In some embodiments of the present invention, the laundry detergent composition comprises the modified lysine-based polymer according to the present invention in an amount of 0.5% to 30% by weight, preferably 1% to 25% and more preferably 1% to 15% (e.g. 1% to 10% by weight) based on the total solids content of the detergent composition.

[0137] As an essential component for providing cleaning efficacy to the detergent composition, at least one of cationic, anionic, nonionic and amphoteric surfactants may be included depending on the specific application and desired properties of the detergent composition.

[0138] Nonionic surfactants

[0139] Useful nonionic surfactants may include, but are not limited to, condensation products of (1) alcohols with ethylene oxide, (2) alcohols with ethylene oxide and another alkylene oxide, (3) polypropylene glycol with ethylene oxide, or (4) ethylene oxide with the reaction product of ethylenediamine and propylene oxide, fatty acid amides, and semi-polar nonionic surfactants.

[0140] The condensation products of alcohols with ethylene oxide are derived from, for example, 22 -alkyl, preferably C 10 To C 18 -alkyl alcohols, which may be straight-chain or branched, primary or secondary. The alcohols are condensed with about 1 to 25 mol and preferably with about 3 to 18 mol of ethylene oxide per mole of alcohol.

[0141] The condensation products of alcohols with ethylene oxide and further alkylene oxides can be constructed according to the scheme RO-EO-AO or RO-AO-EO, wherein R is a primary or secondary, branched or straight chain C8 to C 22 -alkyl, preferably C 10 To C 18 -alkyl, EO is ethylene oxide and AO comprises an alkylene oxide, preferably propylene oxide, butylene oxide or pentylene oxide.

[0142] The condensation products of polypropylene glycol and ethylene oxide contain a hydrophobic portion preferably having a molecular weight of about 1,500 to about 1,800. The addition of up to about 40 moles of ethylene oxide to the hydrophobic portion results in an amphiphilic compound.

[0143] The condensation products of ethylene oxide with the reaction products of ethylenediamine and propylene oxide contain a hydrophobic portion consisting of the reaction products of ethylenediamine and propylene oxide and generally having a molecular weight of about 2,500 to about 3,000. Ethylene oxide is added up to a polyoxyethylene content of up to about 40% to about 80% by weight based on the hydrophobic unit and a molecular weight of about 5,000 to about 11,000.

[0144] The fatty acid amides may be those of the formula

[0145]

[0146] in

[0147] R 1 is an alkyl group having 7 to 21 and preferably 9 to 17 carbon atoms, and

[0148] R 2 are independently hydrogen, C1 to C4-alkyl, C1 to C4-hydroxyalkyl or (C2H4O) x H, where x varies from 1 to 3.

[0149] C8 to C 20 - Fatty acid amides, such as monoethanolamide, diethanolamide and diisopropanolamide.

[0150] As semi-polar nonionic surfactants, there may be mentioned 18 -alkyl, preferably C 10 To C 14 -alkyl water-soluble amine oxides, water-soluble phosphine oxides and water-soluble sulfoxides. 10 -C 12 -Alkoxyethyl dihydroxyethylamine oxide.

[0151] Anionic surfactants

[0152] Useful anionic surfactants may include, but are not limited to, alkenyl- or alkylbenzene sulfonates, alkane sulfonates, olefin sulfonates, alkyl ester sulfonates, alkyl sulfates, alkyl ether sulfates, alkyl carboxylates (soaps). The counterions present are alkali metal cations (preferably sodium or potassium), alkaline earth metal cations (e.g. calcium or magnesium) and also ammonium and substituted ammonium compounds (e.g. monoethanolammonium, diethanolammonium or triethanolammonium cations) and mixtures of the above cations therefrom.

[0153] The alkenyl- or alkylbenzene sulfonate may contain branched or straight-chain, optionally hydroxy-substituted alkenyl or alkyl groups, preferably straight-chain C9 to C 25 -alkyl.

[0154] Alkane sulfonates are available on a large industrial scale in the form of secondary alkane sulfonates in which the sulfonic group is attached to a secondary carbon atom of the alkyl moiety. The alkyl group may in principle be saturated, unsaturated, branched or straight-chain and may optionally be hydroxy-substituted. Preferred secondary alkane sulfonates contain straight-chain C9 to C 25 -alkyl, preferably C 10 To C 20 -alkyl and more preferably C 12 To C 18 -alkyl.

[0155] Olefin sulfonates are obtained by sulfonating C8 to C 24 And preferably C 14 To C 16 -α-olefins and subsequent neutralization. Due to their production process, these olefin sulfonates may contain small amounts of hydroxyalkane sulfonates and alkane disulfonates.

[0156] Alkyl ester sulfonates are derived from, for example, C8 to C 20 - a linear ester of a carboxylic acid (ie, a fatty acid) which is sulfonated with sulfur trioxide. The compound of the formula

[0157]

[0158] in

[0159] R' is C8 to C 20 -alkyl, preferably C 10 To C 16 -alkyl, and R" is C1 to C6-alkyl, preferably methyl, ethyl or isopropyl. Methyl ester sulfonates are particularly preferred, wherein R 1 It is C 10 To C 16 -alkyl.

[0160] Alkyl sulfates are surfactants of the formula ROSO3M', where R is C 10 To C 24 -alkyl and preferably C 12 To C 18 -alkyl. M' is a counterion as described at the beginning of the anionic surfactant.

[0161] Alkyl ether sulfates have the general structure RO(A) m SO3M, where R is C 10 To C 24 -alkyl and preferably C 12 To C 18-alkyl, wherein A is an alkoxy unit, preferably ethoxy, and m is a value from about 0.5 to about 6, preferably between about 1 and about 3, and M is a cation, such as sodium, potassium, calcium, magnesium, ammonium or a substituted ammonium cation.

[0162] Alkyl carboxylates are often referred to by the term "soap". The soap can be based on a saturated or unsaturated, preferably natural, straight-chain C8 to C 18 -fatty acids. Saturated fatty acid soaps include, for example, salts of lauric acid, myristic acid, palmitic acid, stearic acid, hydrogenated erucic acid and behenic acid, and in particular soap mixtures derived from natural fatty acids such as coconut, palm kernel or tallow fatty acids. Known alkenyl succinates may also be used with soap or as a soap substitute.

[0163] Further anionic surfactants are salts of acylaminocarboxylic acids, acyl sarcosinates, fatty acid-protein condensation products obtained by reaction of fatty acid chlorides with oligopeptides; salts of alkylsulfonamidocarboxylic acids; salts of alkyl and alkylaryl ether carboxylic acids; sulfonated polycarboxylic acids, alkyl and alkenyl glycerol sulfates (e.g. oleyl glycerol sulfate), alkylphenol ether sulfates, alkyl phosphates, alkyl ether phosphates, isethionates (e.g. acyl isethionates), N-acylaminoethanesulfonates, alkyl succinates, sulfosuccinates, monoesters of sulfosuccinates (especially saturated and unsaturated C 12 To C 18 -monoesters) and diesters of sulfosuccinates (especially saturated and unsaturated C 12 To C 18 -diesters), sulfates of alkyl polysaccharides (such as alkyl polysaccharides and sulfates of alkyl polysaccharides, such as alkyl polysaccharides and alkyl polyethoxy carboxylates (such as formula RO(CH2CH2) k Those of CH2COOM, where R is C8 to C 22 -alkyl, k is a number from 0 to 10 and M is a cation).

[0164] Cationic surfactants

[0165] The cationic surfactants that can be used are R 1 N(CH3)3 + X - , R 1 R 2 N(CH 3)2 + X - , R 1 R 2 R 3 N(CH3) + X - or R 1 R 2 R3 R 4 N + X - A substituted or unsubstituted straight-chain or branched quaternary ammonium salt, wherein R 1 , R 2 , R 3 and R 4 are independently unsubstituted C8 to C 24 -alkyl and preferably C8 to C 18 -alkyl, hydroxyalkyl having 1 to 4 carbon atoms, phenyl, C2 to C 18 -alkenyl, C7 to C 24 -Arylalkyl, (C2H4O) x H, wherein x is from about 1 to about 3, the alkyl group optionally contains one or more ester groups, and X is a suitable anion. Useful cationic surfactants may also be cyclic quaternary ammonium salts.

[0166] Amphoteric / Zwitterionic Surfactants

[0167] Available amphoteric surfactants can be aliphatic derivatives of secondary or tertiary amines or aliphatic derivatives of heterocyclic secondary and tertiary amines, wherein the aliphatic group can be straight or branched and wherein one of the aliphatic substituents contains at least about 8 carbon atoms or about 8 to about 18 carbon atoms, and at least one of the aliphatic substituents contains an anionic water-soluble group, such as carboxylate, sulfonate, sulfate. Suitable amphoteric surfactants also include sarcosinate, glycinate, taurate and mixtures thereof. Examples of materials as amphoteric surfactants are known in the art, such as from WO 2005095569A1.

[0168] Useful zwitterionic surfactants can be derivatives of secondary and tertiary amines, derivatives of heterocyclic secondary and tertiary amines, or derivatives of quaternary ammonium, quaternary phosphonium or tertiary sulfonium compounds. Suitable examples of zwitterionic surfactants include, but are not limited to, betaines, such as alkyl betaines and alkyl amido betaines, such as N-alkyl-N,N-dimethyl-N-carboxymethyl betaine, N-(alkylamidopropyl)-N,N-dimethyl-N-carboxymethyl betaine, alkyl dimerethoxy betaine, alkylamine oxides, and sulfo and hydroxy betaines, such as N-alkyl-N,N-dimethylamino-1-propane sulfonate, each of which has a linear or branched C8 to C 22 -alkyl, preferably C8 to C 18 -alkyl and more preferably C 12 To C 18 -alkyl.

[0169] 1. In an exemplary embodiment of the present invention, the laundry detergent composition may contain 0.1% to 80% by weight of at least one surfactant selected from anionic surfactants, amphoteric surfactants and nonionic surfactants, based on the total solid content of the detergent composition. Some preferred laundry detergent compositions of the present invention may contain at least one anionic or nonionic surfactant.

[0170] Additives

[0171] The detergent compositions may further contain conventional adjuncts for modifying the performance characteristics of the detergent compositions.

[0172] Suitable adjuvants for detergent compositions may include, but are not limited to, builders, such as complexing agents, ion exchangers and precipitants, bleaches, bleach activators, corrosion inhibitors, foam boosters, defoamers, dyes, fillers, color protectants, optical brighteners, disinfectants, alkalis, antioxidants, thickeners, spices, solvents, solubilizers, softeners and antistatic agents, in addition to the modified lysine-based polymers according to the present invention. As examples, some adjuvants are described below.

[0173] Typically, the detergent composition may comprise at least one builder selected from organic and inorganic builders. Examples of suitable inorganic builders are sodium sulfate or sodium carbonate or silicates, in particular sodium disilicate and sodium metasilicate, zeolites, layered silicates, in particular those of the formula α-Na2Si2O5, β-Na2Si2O5 and δ-Na2Si2O5. Examples of suitable organic builders are fatty acid sulfonates, α-hydroxypropionic acid, alkali metal malonates, fatty acid sulfonates, alkyl and alkenyl disuccinates, tartrate diacetate, tartrate monoacetate, oxidized starch, methylglycine diacetic acid and alkali metal salts thereof (in particular Na-salt), N,N-dicarboxymethylglutamic acid and alkali metal salts thereof (in particular Na-salt), citric acid and Na-salt thereof, and polymeric builders, such as polycarboxylates and polyaspartic acid.

[0174] The detergent composition may comprise builders in a total amount of, for example, 10 to 70% by weight, preferably up to 50% by weight, based on the total solids content of the detergent composition. In the context of the present invention, the modified lysine-based polymers according to the invention are not counted as builders.

[0175] The detergent composition may include at least one defoaming agent selected from, for example, silicone oil and paraffin oil. The total amount of the defoaming agent may be 0.05 to 0.5% by weight based on the total solid content of the detergent composition.

[0176] The detergent composition may contain at least one bleaching agent. The bleaching agent may be selected from chlorine bleach and peroxide bleach.

[0177] Peroxide bleaching agents can be selected from inorganic peroxide bleaching agents and organic peroxide bleaching agents. Preferred inorganic peroxide bleaching agents are selected from alkali metal percarbonates, alkali metal perborates and alkali metal persulfates. In solid detergent compositions for hard surface cleaning and in solid laundry detergent compositions, alkali metal percarbonates, especially sodium percarbonate, are preferably used in a coated form. Such coatings may be of organic or inorganic nature. Examples are glycerol, sodium sulfate, silicates, sodium carbonate and any combination thereof, such as a combination of sodium carbonate and sodium sulfate. An example of an organic peroxide bleaching agent is percarboxylic acid.

[0178] Suitable chlorine-containing bleaches are, for example, 1,3-dichloro-5,5-dimethylhydantoin, N-chlorosulfonamide, chloramine T, chloramine B, sodium hypochlorite, calcium hypochlorite, magnesium hypochlorite, potassium hypochlorite, potassium dichloroisocyanurate and sodium dichloroisocyanurate. The laundry detergent composition may contain chlorine-containing bleaches in a total amount of, for example, 3 to 10% by weight, based on the total solids content of the detergent composition.

[0179] The detergent composition may also contain at least one bleach activator, for example N-methylmorpholinium-acetonitrile salt ("MMA salt"), trimethylammonium acetonitrile salt, N-acylimide such as N-nonanoylsuccinimide, 1,5-diacetyl-2,2-dioxohexahydro-1,3,5-triazine ("DADHT") or quaternary ammonium nitrile salt (trimethylammonium acetonitrile salt). Further examples of bleach activators are tetraacetylethylenediamine (TAED) and tetraacetylhexanediamine.

[0180] The detergent composition may contain at least one corrosion inhibitor. Examples of suitable corrosion inhibitors are triazoles, in particular benzotriazole, bisbenzotriazole, aminotriazole, alkylaminotriazole, phenol derivatives such as hydroquinone, pyrocatechol, hydroxyhydroquinone, gallic acid, phloroglucinol or pyrogallol. The detergent composition may contain the corrosion inhibitor in a total amount of 0.1 to 1.5% by weight, based on the total solids content of the detergent composition.

[0181] The detergent composition according to the invention additionally comprises at least one enzyme. Preferably, the at least one enzyme is a detergent enzyme.

[0182] Suitable enzymes can be classified as oxidoreductases (EC 1), transferases (EC 2), hydrolases (EC 3), lyases (EC 4), isomerases (EC 5), or ligases (EC 6) (EC numbering is according to the Enzyme Nomenclature Recommendations of the Nomenclature Committee of the International Union of Biochemistry and Molecular Biology (1992), including its supplements published 1993-1999). Preferably, the enzyme is a hydrolase (EC 3).

[0183] Preferably, the enzyme is selected from the group consisting of proteases, amylases, lipases, cellulases, mannanases, hemicellulases, phospholipases, esterases, pectinases, lactases, peroxidases, xylanases, cutinases, pectate lyases, keratinases, reductases, oxidases, phenoloxidases, lipoxygenases, ligninases, pullulanases, tannases, pentosanases, malanases, beta-glucanases, arabinosidases, hyaluronidases, chondroitinases, laccases, nucleases, deoxy ribonucleases, phosphodiesterases, phytases, carbohydrases, galactanases, xanthanases, xyloglucanases, oxidoreductases, perhydrolases, aminopeptidases, asparaginases, carbohydrases, carboxypeptidases, catalases, chitinases, cyclodextrin glycosyltransferases, α-galactosidases, β-galactosidases, glucoamylases, α-glucosidases, β-glucosidases, invertases, ribonucleases, transglutaminases and dispersins and any combination thereof. More preferably, the enzyme is selected from the group consisting of proteases, amylases, lipases, cellulases, mannanases, xylanases, deoxyribonucleases, dispersases, pectinases, oxidoreductases and cutinases and any combination thereof. In particular, the enzyme is a protease, preferably a serine protease, more preferably a subtilisin.

[0184] Such one or more enzymes may be incorporated into the composition at a level sufficient to provide an effective amount for achieving a beneficial effect, preferably for a primary cleaning effect and / or a secondary cleaning effect, such as an anti-ashing or anti-pilling effect (e.g., in the case of cellulases). Preferably, the enzyme is present in the composition in an amount of 0.00001% to 5%, preferably 0.00001% to 2%, more preferably 0.0001% to 1%, or even more preferably 0.001% to 0.5% enzyme protein by weight of the composition.

[0185] Preferably, the detergent composition according to the present invention may further comprise an enzyme stabilizing system. Preferably, the composition according to the present invention comprises an enzyme stabilizing system in an amount of 0.001% to 10%, 0.005% to 8%, or 0.01% to 6% based on the total weight of the composition. The enzyme stabilizing system may be any stabilizing system compatible with the enzyme.

[0186] Preferably, the enzyme stabilization system comprises at least one compound selected from the group consisting of: polyols (such as 1,3-propylene glycol, ethylene glycol, glycerol, 1,2-propylene glycol or sorbitol), inorganic salts (such as CaCl2, MgCl2 or NaCl), short-chain (preferably C1-C6) carboxylic acids and salts thereof (such as formic acid, formates (preferably sodium formate), acetic acid, acetate or lactate), borates, boric acid, boronic acid (preferably 4-formylphenylboronic acid (4-FPBA)), peptide aldehydes, peptide acetals and peptide aldehyde bisulfite adducts. Preferably, the enzyme stabilization system comprises a combination of at least two of the compounds selected from the group consisting of inorganic salts, polyols and short-chain carboxylic acids, and preferably a combination of one or more compounds selected from the group consisting of borates, boric acid, boronic acid (preferably 4-formylphenylboronic acid (4-FPBA)), peptide aldehydes, peptide acetals and peptide aldehyde bisulfite adducts. In particular, if a protease is present in the composition, a protease inhibitor may be added, which is preferably selected from borates, boric acid, boronic acid (preferably, 4-FPBA), peptide aldehydes (preferably, peptide aldehydes such as Z-VAL-H or Z-GAY-H), peptide acetals and peptide aldehyde bisulfite adducts.

[0187] The detergent composition comprising the modified lysine-based polymer according to the present invention may also comprise at least one antimicrobial agent and / or preservative.

[0188] Antimicrobials are chemical compounds that kill microorganisms or inhibit their growth or reproduction. The microorganisms can be bacteria, yeasts or molds.

[0189] Preservatives are antimicrobial agents that can be added to aqueous products and compositions to maintain the original performance, properties and integrity of the products and compositions by killing contaminating microorganisms or inhibiting their growth. Examples of preservatives are listed in patent application WO 2021 / 115912 A1, pages 35 to 39.

[0190] Of particular interest are the following antimicrobial agents and / or preservatives:

[0191] 4,4'-Dichloro-2-hydroxydiphenyl ether (Synonyms: 5-chloro-2-(4-chlorophenoxy)phenol, Diclosan, DCPP);

[0192] 2-Phenoxyethanol (Synonyms: phenoxyethanol, methylphenyl glycol, phenoxyethanol, ethylene glycol phenyl ether, ethylene glycol monophenyl ether, 2-(phenoxy)ethanol, 2-phenoxy-1-ethanol);

[0193] 2-Bromo-2-nitropropane-1,3-diol (Synonyms: 2-bromo-2-nitro-1,3-propanediol, bronopol);

[0194] Glutaraldehyde (Synonyms: 1-5-glutaraldehyde, pentane-1,5-dialdehyde, glutaral, glutardialdehyde);

[0195] Glyoxal (Synonyms: ethandial, oxyacetaldehyde, 1,2-glyoxal);

[0196] 2-Butyl-benzo[d]isothiazol-3-one (BBIT);

[0197] 2-Methyl-2H-isothiazol-3-one (MIT);

[0198] 2-Octyl-2H-isothiazol-3-one (OIT);

[0199] 5-Chloro-2-methyl-2H-isothiazol-3-one (CIT or CMIT);

[0200] · a mixture of 5-chloro-2-methyl-2H-isothiazol-3-one (CMIT) and 2-methyl-2H-isothiazol-3-one (MIT) (CMIT / MIT mixture);

[0201] 1,2-Benzisothiazol-3(2H)-one (BIT);

[0202] Hexa-2,4-dienoic acid (commonly known as "sorbic acid") and its salts, such as calcium sorbate, sodium sorbate; potassium (E,E)-hexa-2,4-dienoate (potassium sorbate);

[0203] Lactic acid and its salts; L-(+)-lactic acid; in particular sodium lactate;

[0204] Benzoic acid and salts of benzoic acid, for example, sodium benzoate, ammonium benzoate, calcium benzoate, magnesium benzoate, MEA benzoate, potassium benzoate;

[0205] Salicylic acid and its salts, for example calcium salicylate, magnesium salicylate, MEA salicylate, sodium salicylate, potassium salicylate, TEA salicylate;

[0206] Benzalkonium chloride, benzalkonium bromide, benzalkonium saccharinate;

[0207] Didecyldimethylammonium chloride (DDAC);

[0208] · N-(3-aminopropyl)-N-dodecylpropane-1,3-diamine (diamine);

[0209] Peracetic acid; and

[0210] Hydrogen peroxide.

[0211] The at least one antimicrobial agent or preservative may be added to the detergent composition in an amount of 0.0001% to 10% based on the total weight of the composition.

[0212] Preferably, the detergent composition comprises 2-phenoxyethanol in an amount of 2 ppm to 5%, preferably 0.1% to 2%, or 4,4'-dichloro-2-hydroxydiphenyl ether (DCPP) in an amount of 0.001% to 3%, preferably 0.002% to 1%, more preferably 0.01% to 0.6%, based on the total weight of the composition.

[0213] Suitable types and dosages of conventional adjuvants for detergent compositions, especially laundry detergent compositions, are well known in the art and can be found, for example, in WO 2017174413 A1 and WO 2015187757 A1.

[0214] Example

[0215] Various embodiments are listed below. It will be understood that the embodiments listed below can be combined with all aspects of the scope of the present invention and other embodiments.

[0216] 1. A modified lysine-based polymer obtainable or obtained by a process comprising subjecting at least a portion of the free amino groups in the lysine-based polymer to Michael addition with a Michael acceptor selected from at least one of an unsaturated carboxylic acid and an unsaturated carboxylic acid ester.

[0217] 2. A modified lysine-based polymer according to embodiment 1, wherein the Michael acceptor is at least one selected from the group consisting of: α,β-ethylenically unsaturated monocarboxylic acids having 3 to 10 carbon atoms, α,β-ethylenically unsaturated dicarboxylic acids having 4 to 8 carbon atoms, α,β-ethylenically unsaturated tricarboxylic acids having 4 to 8 carbon atoms, α,β-ethylenically unsaturated carboxylic acids having more carboxylic acid groups, and any esters thereof.

[0218] 3. A modified lysine-based polymer according to embodiment 2, wherein the Michael acceptor is at least one selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid and any esters thereof.

[0219] 4. The modified lysine-based polymer according to embodiment 3, wherein the Michael acceptor is at least one selected from the group consisting of acrylic acid, maleic acid, itaconic acid, and any esters thereof.

[0220] 5. The modified lysine-based polymer according to any one of the preceding embodiments, wherein the ester is selected from polyoxyalkylene esters or blocked polyoxyalkylene esters of the unsaturated carboxylic acid, preferably blocked polyethylene oxide esters, blocked polypropylene oxide esters or blocked polybutylene oxide esters, or combinations thereof.

[0221] 6. The modified lysine-based polymer according to any one of the preceding embodiments, wherein the capped polyethylene oxide ester contains a capping group selected from C1-C4-alkyl or C1-C4-hydroxyalkyl.

[0222] 7. The modified lysine-based polymer according to embodiment 5 or 6, wherein the polyalkylene oxide or capped polyalkylene oxide portion has a number average molecular weight of 100 to 2,000, preferably 200 to 1,200 and more preferably 400 to 800.

[0223] 8. A modified lysine-based polymer comprising structural units derived from a lysine monomer represented by:

[0224]

[0225] in

[0226] R2 and R3 are independently H or R4, provided that at least one of R2 and R3 is R4,

[0227] * indicates the position where this building block is attached to any other building block via an amide linkage,

[0228] R4 is a moiety represented by formula (II)

[0229]

[0230] in

[0231] R5 and R6 are independently H, C1-C6-alkyl, carboxyl (-COOH), -COOM, -(C1-C4-alkylene)-COOH or -(C1-C4-alkylene)-COOM,

[0232] R7 is H, C1-C6-alkyl, -(CH2CH2O) n -R8 or M,

[0233] R8 is C1-C4-alkyl,

[0234] M is a cation selected from the group consisting of alkali metal cations, alkaline earth metal cations, ammonium and amine cations,

[0235] n is a number in the range of 2 to 40, and

[0236] ** indicates the position where the moiety is attached to the N atom carrying R4.

[0237] 9. The modified lysine-based polymer of embodiment 8, wherein:

[0238] R5 and R6 are independently H, C1-C4-alkyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0239] R7 is H, -(CH2CH2O) n -R8 or M,

[0240] R8 is C1-C2-alkyl, and

[0241] n is a number in the range of 4 to 25.

[0242] 10. The modified lysine-based polymer of embodiment 9, wherein:

[0243] R5 is H, methyl, carboxyl (-COOH), or -COOM,

[0244] R6 is H, methyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0245] R7 is H, -(CH2CH2O) n -R8 or M,

[0246] R8 is C1-C2-alkyl, and

[0247] n is a number in the range of 8 to 15.

[0248] 11. The modified lysine-based polymer of embodiment 10, wherein:

[0249] R5 is H, carboxyl (-COOH), or -COOM,

[0250] R6 is H, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM,

[0251] R7 is H, -(CH2CH2O) n -R8 or M, and

[0252] R8 is methyl.

[0253] 12. The modified lysine-based polymer of any preceding embodiment, which is a modified lysine homopolymer.

[0254] 13. The modified lysine-based polymer according to any one of the preceding embodiments 1 to 11, which is a modified lysine copolymer comprising greater than 50 mol % of structural units derived from lysine monomers and less than 50 mol % of structural units derived from at least one dicarboxylic acid or an amide-forming derivative thereof.

[0255] 14. The modified lysine-based polymer according to embodiment 13, comprising

[0256] (A) 60 to 99 mol % of structural units derived from lysine monomers,

[0257] (B) 1 to 40 mol % of structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof

[0258] HOOC-R1-COOH(I)

[0259] in

[0260] R1 is a direct bond or an aliphatic straight-chain alkylene group, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted alkyl, unsubstituted or substituted alkoxy, unsubstituted or substituted alkylthio, unsubstituted or substituted alkylamino, di(alkyl)amino, alkylene, hydroxyl, mercapto, amino and halogen.

[0261] 15. The modified lysine-based polymer according to embodiment 14, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 24 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 18 -alkyl, unsubstituted or substituted C1-C 18 -alkoxy, unsubstituted or substituted C1-C 18 -alkylthio, unsubstituted or substituted C1-C 18 -alkylamino, di(C1-C 18 -alkyl)amino, C1-C6-alkylene, hydroxy, mercapto, amino and halogen.

[0262] 16. The modified lysine-based polymer according to embodiment 15, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 18 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 12 -alkyl, unsubstituted or substituted C1-C 12 -alkoxy, unsubstituted or substituted C1-C 12 -alkylthio, unsubstituted or substituted C1-C 12 -alkylamino, di(C1-C 12 -alkyl)amino, C1-C4-alkylene, hydroxy, mercapto, amino and halogen.

[0263] 17. The modified lysine-based polymer according to embodiment 16, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 12 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C8-alkyl, unsubstituted or substituted C1-C8-alkoxy, unsubstituted or substituted C1-C8-alkylthio, unsubstituted or substituted C1-C8-alkylamino, di(C1-C8-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

[0264] 18. The modified lysine-based polymer according to embodiment 17, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, unsubstituted or substituted C1-C4-alkoxy, unsubstituted or substituted C1-C4-alkylthio, unsubstituted or substituted C1-C4-alkylamino, di(C1-C4-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

[0265] 19. The modified lysine-based polymer according to embodiment 18, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C4-alkylene, hydroxy, mercapto and amino.

[0266] 20. The modified lysine-based polymer of embodiment 19, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C2-alkylene, hydroxyl and amino, preferably at least one of oxalic acid, malonic acid, succinic acid, maleic acid and fumaric acid, tartaric acid, aspartic acid, glutaric acid, itaconic acid, glutamic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid and dodecanedioic acid.

[0267] 21. The modified lysine-based polymer according to any one of the preceding embodiments 14 to 20, comprising

[0268] (A) 70 to 97 mol% of structural units derived from lysine monomers; and

[0269] (B) 3 to 30 mol % of structural units derived from at least one dicarboxylic acid of the formula (I) or an amide-forming derivative thereof.

[0270] 22. The modified lysine-based polymer according to embodiment 21, comprising

[0271] (A) 75 to 97 mol% of structural units derived from lysine monomers; and

[0272] (B) 4 to 25 mol % of structural units derived from at least one dicarboxylic acid of the formula (I) or an amide-forming derivative thereof.

[0273] 23. The modified lysine-based polymer according to embodiment 22, comprising

[0274] (A) 75 to 95 mol % of lysine structural units; and

[0275] (B) 5 to 25 mol% of dicarboxylic acid structural units.

[0276] 24. The modified lysine-based polymer of any preceding embodiment having a degree of modification via Michael addition of at least 10%, such as at least 20%.

[0277] 25. The modified lysine-based polymer of any preceding embodiment, having a weight average molecular weight (Mw) in the range of 600 to 20,000 g / mol, and / or having a number average molecular weight (Mn) in the range of 500 to 20,000 g / mol.

[0278] 26. A detergent composition, preferably a laundry detergent composition, comprising the modified lysine-based polymer according to any one of preceding embodiments 1 to 25.

[0279] 27. The detergent composition according to embodiment 26, wherein the detergent composition comprises the modified lysine-based polymer in an amount of 0.5% to 30%, preferably 1% to 25% and more preferably 1% to 15% by weight based on the total solid content of the detergent composition.

[0280] 28. The detergent composition according to embodiment 25 or 26, comprising 2-phenoxyethanol, preferably in an amount of 2 ppm to 5%, more preferably 0.1% to 2% by weight based on the total weight of the detergent composition.

[0281] 29. The detergent composition according to embodiment 25 or 26, comprising 4,4'-dichloro-2-hydroxydiphenyl ether, preferably in an amount of 0.001% to 3%, preferably 0.002% to 1%, more preferably 0.01% to 0.6% based on the total weight of the detergent composition.

[0282] 30. The detergent composition of any preceding embodiment 26 to 29 comprising at least one enzyme, preferably at least one enzyme selected from the group consisting of proteases, amylases, lipases, cellulases, mannanases, xylanases, DNases, dispases, pectinases, oxidoreductases and cutinases.

[0283] 31. Use of a modified lysine-based polymer as defined in any one of embodiments 1 to 25 in a detergent composition, especially a laundry detergent composition.

[0284] 32. Use of a modified lysine-based polymer as defined in any one of embodiments 1 to 25 as a dispersant.

[0285] 33. A method of preserving an aqueous detergent composition comprising the modified lysine-based polymer of any preceding embodiments 1 to 25 from microbial contamination or growth, comprising adding 2-phenoxyethanol to the detergent composition.

[0286] 34. A method of laundering fabrics or cleaning hard surfaces comprising antimicrobial treatment of the fabrics or hard surfaces with a detergent composition comprising the modified lysine-based polymer according to any one of preceding embodiments 1 to 25 and 4,4'-dichloro-2-hydroxydiphenyl ether.

[0287] The following examples are provided to illustrate the present invention but are not intended to limit the present invention.

[0288] Examples

[0289] Description of materials used in the examples:

[0290]

[0291]

[0292] Determination of molecular weight

[0293] The number average (Mn) and weight average (Mw) molecular weights of the modified lysine-based polymers prepared in the following examples were determined by measuring the unmodified lysine-based polymers by gel permeation chromatography (GPC) and then converting the measured values ​​to the molecular weights of the modified polymers based on the corresponding degree of modification (DM). The definition and determination of the DM of the lysine-based polymers modified by Michael addition are as described above. The DM of the carboxymethylated lysine-based polymers is defined according to the following equation and determined according to a similar procedure similar to that of the lysine-based polymers modified by Michael addition,

[0294]

[0295] Unmodified lysine-based polymers were analyzed by cascade columns (i.e., TSKgelG4000, G3000, G3000, 300 x 7.8 mm) at 35°C and a flow rate of 0.8 ml / min in an aqueous eluent containing 0.1 M NaCl and 0.1 wt% trifluoroacetic acid. For analysis, unmodified polymers were dissolved in the eluent at a concentration of 1.5 mg / ml at room temperature and filtered through a 0.22 μm membrane, and 100 μL were injected in an Agilent 1100 chromatography system after 2 hours. Relative molecular weights were characterized by refractive index detection relative to a calibration curve obtained with polyvinyl pyrrolidone standards, ranging between 620 and 1,060,000 g / mol.

[0296] Confirmation of polymer composition

[0297] All polymer compositions were 1 H-NMR spectrum confirmed.

[0298] Preparation Example

[0299] Example 1: Lysine Homopolymer Modified by Michael Addition of Acrylic Acid

[0300] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After a reaction time of 3 hours, water was further distilled off under reduced pressure (670 mbar). Finally, 103g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.1.

[0301] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 50 g of lysine homopolymer, 64.74 g of acrylic acid, and 114.74 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 99.1 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 35%, and the molecular weights as determined were Mn = 718 g / mol and Mw = 883 g / mol.

[0302] Example 2: Lysine Homopolymer Modified by Michael Addition of Acrylic Acid

[0303] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After 3.5 hours of reaction time, water was further distilled off under reduced pressure (670 mbar). Finally, 102g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.1.

[0304] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 15 g of lysine homopolymer, 19.42 g of acrylic acid, and 34.42 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 99.1 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 52%, and the molecular weights as determined were Mn = 817 g / mol and Mw = 1,005 g / mol.

[0305] Example 3: Lysine Homopolymer Modified by Michael Addition of Acrylic Acid

[0306] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After 3.5 hours of reaction time, water was further distilled off under reduced pressure (670 mbar). Finally, 102g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.1.

[0307] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 30 g of lysine homopolymer, 38.85 g of acrylic acid, and 68.84 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 96.0 wt%, as determined by 1 As determined by H NMR. 1The degree of modification (DM) of the polymer determined by H NMR was 68%, and the molecular weights as determined were Mn = 911 g / mol and Mw = 1,120 g / mol.

[0308] Example 4: Lysine Homopolymer Modified by Michael Addition of Acrylic Acid

[0309] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After a reaction time of 3 hours, water was further distilled off under reduced pressure (670 mbar). Finally, 103g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.1.

[0310] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 25 g of lysine homopolymer, 32 g of acrylic acid, and 57 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 99.5 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 98%, and the molecular weight as determined was M n =1,086 g / mol and M w =1,336 g / mol.

[0311] Example 5: Lysine Homopolymer Modified by Michael Addition of Acrylic Acid

[0312] Into a 1000ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and Dean-Stark receiver, an aqueous solution of 500g of L-Lysine (50wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After 4.5 hours of reaction time, water was further distilled off under reduced pressure (670 mbar). Finally, 272g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 12.5.

[0313] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 25 g of lysine homopolymer, 16 g of acrylic acid, and 57 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 99.0 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 30%, and the molecular weight as determined was M n =1,936 g / mol and M w =3,595 g / mol.

[0314] Example 6: Poly(lysine-co-tartaric acid) modified via Michael addition of acrylic acid at a molar ratio of lysine to tartaric acid of 90:10

[0315] Into the 1000ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with decompression connection and receiver, 400g of lysine, 46g of tartaric acid and 190g of DI water are loaded.The mixture is heated to an internal temperature of 160 ℃ under agitation.After the reaction time of 2 hours and 25 minutes, water is further distilled off under reduced pressure (670 mbar).Finally, 221g of water distillate is collected, and highly viscous polymer is discharged in the silicone container as quickly as possible, while it is still hot and flowable.The k-value of lysine copolymer is determined to be 11.9.

[0316] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 80 g of a lysine copolymer, 37.17 g of acrylic acid, and 117 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 98.4 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 22%, and the molecular weights as determined were Mn = 1,253 g / mol and Mw = 2,605 g / mol.

[0317] Example 7: Poly(lysine-co-tartaric acid) modified via Michael addition of acrylic acid at a molar ratio of lysine to tartaric acid of 80:20

[0318] 200g of lysine, 22.82g of tartaric acid and 108g of DI water are loaded into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with decompression connection and receiver. The mixture is heated to an internal temperature of 160 ℃ for 2h 50min under agitation, with continuous water separation. When 108g of distilled water is collected, the tartaric acid of additional 28.52g is introduced into the reactor. After the total reaction time of 3h 50min, water is further distilled off under reduced pressure (900 mbar). Finally, 132g of water distillate is collected, and highly viscous polymer is discharged in a silicone container as quickly as possible, while it is still hot and flowable. The k-value of lysine is determined to be 12.3.

[0319] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 60 g of a lysine copolymer, 30.88 g of acrylic acid, and 120 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 93.28 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 37%, and the molecular weights as determined were Mn = 1,021 g / mol and Mw = 1,799 g / mol.

[0320] Example 8: Poly(lysine-co-adipic acid) modified via Michael addition of acrylic acid at a molar ratio of lysine to adipic acid of 80:20

[0321] 200g of lysine, 22.21g of adipic acid and 100g of DI water are loaded into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver. The mixture is heated to an internal temperature of 160°C for 2h 50min under agitation, with continuous water separation. Then, an additional 27.77g of adipic acid is introduced into the reactor. After the total reaction time of 3h 50min, water is further distilled off under reduced pressure (900 mbar). Finally, 117g of water distillate is collected, and highly viscous polymer is discharged as quickly as possible into a silicone container, while it is still hot and flowable. The k-value of lysine copolymer is determined to be 11.2.

[0322] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 36.94 g of a lysine copolymer, 19.12 g of acrylic acid, and 60 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The solid content was 100% and the active substance content was 96.9 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 38.24%, and the molecular weights as determined were Mn = 934 g / mol and Mw = 1,705 g / mol.

[0323] Example 9: Lysine Homopolymer Modified by Michael Addition of Itaconic Acid

[0324] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After a reaction time of 3 hours, water was further distilled off under reduced pressure (670 mbar). Finally, 104g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.2.

[0325] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 20 g of lysine homopolymer, 46.75 g of itaconic acid, and 66.75 g of DI water. The pH of the mixture was close to 4 and was precisely adjusted to 4 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The final product had a solid content of 100% and an active substance content of 67.4 wt%, as determined by 1 As determined by H NMR.1 The degree of modification (DM) of the polymer determined by H NMR was 22%, and the molecular weight as determined was M n =740 g / mol and M w =911 g / mol.

[0326] Example 10: Lysine Homopolymer Modified by Michael Addition of Maleic Acid

[0327] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After a reaction time of 3 hours, water was further distilled off under reduced pressure (670 mbar). Finally, 104g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.2.

[0328] 25g of lysine homopolymer, 52g of maleic acid and 77g of DI water were charged into a 250ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. The pH of the mixture was adjusted to 10 by adding 29g of solid NaOH. The mixture was then heated to an internal temperature of 95°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, unreacted maleic acid was precipitated by adjusting the pH to 3.2 by adding HCl solution (36wt%). The filtrate was collected and freeze-dried to obtain a final product with a solid content of 100% and an active substance content of 92.1wt%, as described by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by HNMR was 73%, and the molecular weight as determined was M n =1,186 g / mol and M w =1,459 g / mol.

[0329] Example 11: ε-Polylysine Modified by Michael Addition of Itaconic Acid

[0330] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 20 g of ε-polylysine, 46.75 g of itaconic acid, and 66.75 g of DI water. The pH of the mixture was close to 4 and was precisely adjusted to 4 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70° C. for 24 hours under stirring. After the reaction mixture was cooled to 25° C., the modified polymer was precipitated with an excess of acetone (1:10 by weight). The final product had a solid content of 100% and an active substance content of 74.78 wt %, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 33%, and the molecular weights as determined were Mn = 10,091 g / mol and Mw = 10,574 g / mol.

[0331] Example 12: ε-Polylysine Modified by Michael Addition of Maleic Acid

[0332] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 25 g of ε-polylysine, 52.14 g of maleic acid, and 77.14 g of DI water. The pH of the mixture was adjusted to 1.4 by adding HCl solution (36 wt %). The mixture was then heated to an internal temperature of 95 ° C for 24 hours under stirring. After the reaction mixture was cooled to 25 ° C, the modified polymer was precipitated with an excess of acetone (1: 10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40 ° C for more than 48 hours to obtain the final product. The final product has a solid content of 100% and an active substance content of 68.77 wt %, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 37%, and the molecular weight as determined was M n =10,089 g / mol and M w =10,572 g / mol.

[0333] Example 13: ε-Polylysine Modified by Michael Addition of Acrylic Acid

[0334] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 30 g of ε-polylysine, 38.84 g of acrylic acid, and 68.84 g of DI water. The pH of the mixture was close to 3 and was precisely adjusted to 3 by adding a small amount of HCl (1 mol / L) or NaOH (1 mol / L) solution. The mixture was then heated to an internal temperature of 70°C for 24 hours under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 hours to obtain the final product. The final product had a solid content of 100% and an active substance content of 95.86 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 65%, and the molecular weight as determined was M n =10,553 g / mol and M w =11,058 g / mol.

[0335] Example 14: Lysine Homopolymer Modified via Michael Addition of mPEG-Acrylate

[0336] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and receiver, an aqueous solution of 350g of L-Lysine (71wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After a reaction time of 3 hours, water was further distilled off under reduced pressure (670 mbar). Finally, 106g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.6.

[0337] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 8.54 g of lysine homopolymer, 32.03 g of mPEGA 480 (poly(ethylene glycol) methyl ether acrylate) (mPEG-acrylate, Mn=480) and 121.7 g of glycerol. The mixture was heated to an internal temperature of 70° C. for 4 h under stirring. After the reaction mixture was cooled to 25° C., the solution was collected as a final product having a solid content of 23.23% and an active substance content of 23.23 wt %, as determined by 1 As determined by H NMR. 1The degree of modification (DM) of the polymer as determined by H NMR was 26%, and the molecular weights as determined were Mn = 2,233 g / mol and Mw = 3,388 g / mol.

[0338] Example 15: Lysine Homopolymer Modified via Michael Addition of mPEG-Acrylate

[0339] Into a 1000ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with reduced pressure connection and Dean-Stark receiver, an aqueous solution of 500g of L-Lysine (50wt%) was loaded. The mixture was heated to an internal temperature of 160°C under stirring with continuous water separation. After 4 hours of reaction time, water was further distilled off under reduced pressure (670 mbar). Finally, 264g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 11.2.

[0340] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 8.54 g of lysine homopolymer and 102.5 g of water. The pH of the solution was adjusted to 6 by adding a HCl (1 mol / L) solution. Then, 25.62 g of mPEGA 480 was added, and the mixture was heated to an internal temperature of 60° C. for 8 h under stirring. After the reaction mixture was cooled to 25° C., the solution was collected as a final product having a solid content of 50.8% and an active substance content of 37.6 wt %, as described by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 24%, and the molecular weights as determined were Mn = 2,693 g / mol and Mw = 3,884 g / mol.

[0341] Example 16: ε-Polylysine Modified via Michael Addition with mPEG-Acrylate

[0342] A 500 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 8.54 g of linear ε-polylysine and 179.3 g of water. The pH of the solution was adjusted to 6 by adding a HCl (1 mol / L) solution. Then, 51.23 g of mPEGA 480 was added, and the mixture was heated to an internal temperature of 60° C. for 8 hours under stirring. After the reaction mixture was cooled to 25° C., the solution was collected as a final product having a solid content of 49.4% and an active substance content of 27.1 wt %, as described by 1 As determined by H NMR. 1The degree of modification (DM) of the polymer as determined by HNMR was 39%, and the molecular weights as determined were Mn = 23,749 g / mol and Mw = 24,885 g / mol.

[0343] Example 17: Poly(lysine-co-tartaric acid) modified via Michael addition of mPEG-acrylate at a molar ratio of lysine to tartaric acid of 80:20

[0344] Into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with decompression connection and Dean-Stark receiver, an aqueous solution of 165g of L-Lysine (50wt%) and 9.4g of tartaric acid suspended in 9.5g of water were loaded. The mixture was heated to an internal temperature of 160°C for 2h 25min under stirring, with continuous water separation. Then, additional 11.8g of tartaric acid was introduced into the reactor. Finally, 94g of water distillate was collected, and highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine copolymer was determined to be 11.5.

[0345] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 8.54 g of lysine copolymer and 71.73 g of water. The pH of the solution was adjusted to 6 by adding HCl (1 mol / L) solution. Then, 15.37 g of mPEGA480 was added, and the mixture was heated to an internal temperature of 60° C. for 8 hours under stirring. After the reaction mixture was cooled to 25° C., the solution was collected as a final product having a solid content of 47.0% and an active substance content of 35.7 wt %, as described by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by HNMR was 17%, and the molecular weights as determined were Mn = 1,295 g / mol and Mw = 1,709 g / mol.

[0346] Application Examples

[0347] I. Anti-ashing performance

[0348] Test I.1

[0349] The laundry process was simulated in the laboratory using a Terg-o-meter (RHLG-IV, from Shanghai Bank Equipment Co. Ltd, China) comprising 12 drums with corresponding rotor blades as washing units, generally following GBT 13174-2008.

[0350] Before washing, all fabrics used were pretreated with softener. 7 g of the softener formulation shown in Table 1 was diluted in 10 L of tap water (25° C.) and transferred to a mini washing machine (Hair MW-PQ28SW). 300 g of the fabric to be used was placed in the washing machine and stirred for 3 min. The unrinsed treated fabric was then transferred to another washing machine of the same model to spin dry for 1 minute and then dried at 40° C. for 1 hour.

[0351] The washing units were operated at a stirring speed of 120 revolutions per minute (rpm) and each was filled with 1 L of hard water (100 ppm Ca:Mg=3:2). 3 pieces of each type of white test fabric (15 pieces in total) were washed in the same drum at 30°C with 10 g of a red clay and oil mixture in a wash liquor containing 0.93 g of a detergent having a formulation as shown in Table 2. After washing, the fabric was removed from the washing unit, drained and rinsed twice in 10 L of tap water for 30 seconds each. The wash cycle was repeated twice more with a new red clay and oil mixture and a new wash liquor. After rinsing in the third wash cycle, the test fabric was dried in air instead. The details of the wash cycle are summarized in Table 3.

[0352] The anti-greying properties of the fabrics were measured by using a spectrophotometer Elrepho 2000 from Datacolor at 457 nm. 之前 ) and after 3 wash cycles (R 之后 ) is characterized by the difference in remission.

[0353] The remission difference (ΔR) was calculated according to the following equation:

[0354] ΔR=R 之前 -R 之后 .

[0355] The smaller the ΔR value, the better the performance.

[0356] The results are summarized in Table 5.

[0357] Table 1

[0358]

[0359] Table 2

[0360]

[0361]

[0362] Table 3

[0363]

[0364]

[0365] Table 4

[0366]

[0367] Table 5

[0368] additive ΔR, total for all fabrics ΔR, total for cotton fabrics Blank Batch 248.87 152.84 Modified PEI-1 187.04 118.02 Modified PEI-2 231.41 148.10 Example 1 218.52 127.63 Example 2 204.16 120.19 Example 3 225.01 131.55 Example 4 218.57 132.51 Example 5 184.56 110.43 Example 9 241.87 147.51 Example 10 231.03 136.50 Example 11 217.87 132.29 Example 12 200.05 124.95 Example 13 201.55 122.65 Example 14 228.99 144.49 Example 15 221.37 140.02 Example 16 219.95 140.98 Example 17 196.31 123.78

[0369] Test I.2

[0370] A Terg-o-meter (RHLG-IV, from Shanghai Banking Equipment Co., Ltd., China) comprising 12 drums with corresponding rotor blades as washing units was used, generally following GBT 13174-2008, to simulate the laundry process in the laboratory. The washing units were operated at the same stirring speed of 120 revolutions per minute (rpm), and each was filled with 1 L of water. The white test fabric was washed in the same drum at 30 ° C with 10 g of a red clay and oil mixture in a washing liquid containing a detergent having a formulation as shown in Table 6. After washing, the fabric was removed from the washing unit, drained and rinsed twice in 10 L of tap water for 30 seconds each. The washing cycle was repeated twice with a new red clay and oil mixture and a new washing liquid. After rinsing in the third washing cycle, the test fabric was dried in air instead. The details of the washing cycle are summarized in Table 7.

[0371] The anti-greying properties of the fabrics were measured by measuring the fabrics before washing (R 之前 ) and after 3 wash cycles (R 之后 ) to characterize the difference in relief.

[0372] The remission difference (ΔR) was calculated according to the following equation:

[0373] ΔR=R 之前 -R 之后 .

[0374] The smaller the ΔR value, the better the performance.

[0375] Table 6

[0376]

[0377] a) Based on the active substance content of all ingredients

[0378] Table 7

[0379]

[0380] Table 8

[0381] additive ΔR, total for all fabrics Blank Batch 277.5 Modified PEI-1 227.0 Modified PEI-2 273.2 Example 6 238.00 Example 7 195.42 Example 8 249.90

[0382] II. Primary detergency of liquid laundry preparations

[0383] Test II.1

[0384] The primary detergency of the liquid laundry formulations as shown in Table 9 was measured at full scale using a domestic washing machine according to the protocol as described in Table 10. A Soil Monitor was used for evaluating the detergency of bleachable stains.

[0385] Table 9

[0386]

[0387] a) Based on the active substance content of all ingredients

[0388] Table 10

[0389]

[0390] The primary detergency is characterized by the ΔE value calculated according to DIN EN ISO 11664-4 (June 2012) according to the following equation:

[0391] ΔE=(ΔL *2 +Δa *2 +Δb *2 ) 1 / 2 ,

[0392] in

[0393] ΔL*=L* 洗涤 -L* 初始 ; Δa * =a* 洗涤 -a* 初始 ; and Δb * =b* 洗涤 -b* 初始 .

[0394] The spectrophotometer MACH 5 from Color Consult, supplied by CFT, NL-Vlaardingen, was used to measure L on stained fabrics before and after washing. * 、a * 、b * The higher the ΔE value, the better the performance. The results are summarized in Table 11.

[0395] Table 11

[0396] additive ΔE, Sum of soiled fabrics with bleachable stains blank 0.83 Modified PEI-1 1.29 Modified PEI-2 0.71 Example 2 1.17

[0397] Test II.2

[0398] The primary detergency of the liquid laundry formulations as shown in Table 12 was measured at full scale using a domestic washing machine according to the protocol as described in Table 13. A Soil Monitor was used for evaluating the detergency of bleachable stains.

[0399] Table 12

[0400]

[0401]

[0402] a) Based on the active substance content of all ingredients

[0403] Table 13

[0404]

[0405] The primary detergency was characterized according to the protocol described in Test II.1. The results are summarized in Table 14.

[0406] Table 14

[0407]

[0408] III. Compatibility with Biocides in Liquid Laundry Formulations

[0409] Liquid laundry detergent formulations were prepared containing 1% by weight of a polymer of the invention as shown in the examples in Table 15 and / or 0.3% of a biocide HP 100 (from BASF) and / or 1% phenoxyethanol ( PE, BASF). The formulations were prepared by first preparing a premix containing surfactants, solvents, fatty acids, citric acid and NaOH as shown in Table 15 and up to 90% water. The premix was prepared by adding all components to the appropriate amount of water and stirring at room temperature. Subsequently, the pH was set to pH = 8.5 using NaOH. The final formulation was then prepared by stirring at room temperature: 90% of the premix, appropriate concentrations of polymer and / or HP 100 (commercial product of BASF SE containing 30% of the biocide active substance 4,4'-dichloro-2-hydroxydiphenyl ether) and / or 2-phenoxyethanol and water totaling 100%. For comparison purposes, a standard liquid detergent formulation containing neither the polymer according to the invention nor the biocide was prepared.

[0410] All amounts indicated in Table 15 are provided as active ingredients.

[0411]

[0412]

[0413] It is clear from the above table that the polymers according to the present invention can be used with biocides HP 100 (4,4'-dichloro-2-hydroxydiphenyl ether) or PE (2-phenoxyethanol) was incorporated in liquid laundry formulations without any instability or turbidity.

[0414] III. Biodegradability of Modified Lysine-Based Polymers

[0415] Use OECD 301F manometric respirometry to test the biodegradation of polymer in wastewater in triplicate.30mg / mL test substance is inoculated into the wastewater extracted from Mannheim wastewater treatment plant, and incubated 28 days at 25 ℃ in airtight flask.During this time, oxygen consumption is measured as the change of pressure in the flask using OxiTop C (WTW).NaOH solution is used to absorb the CO2 that escapes.After using blank correction, the amount of oxygen consumed by microbial population during the biodegradation of test substance is expressed as % of ThOD (theoretical oxygen demand).

[0416] Table 16

[0417] Examples 28 days (%) 56 days (%) 1 37 73 2 29 68 3 23 41 4 18 41 5 48 82 6 22 41 7 41 not applicable 8 22 46 9 39 not applicable 10 28 32 11 27 not applicable 12 20 22 13 22 not applicable 15 38 not applicable 16 53 56 17 46 not applicable

[0418] The test results indicate that the carboxymethylated lysine-based polymer according to the present invention shows acceptable biodegradability.

[0419] Example 18

[0420] 82.5g of L-Lysine, 9.4g of tartaric acid and 90g of water were loaded into a 500ml four-necked flask equipped with an agitator, an internal thermometer, a gas inlet pipe, a condenser with a reduced pressure connection and a Dean-Stark receiver. The mixture was heated to an internal temperature of 160°C under stirring. After a reaction time of 2h 25min, water was further distilled off under reduced pressure (670 mbar). Finally, 94g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The K-value was measured to be 11.6. The molar ratio of the lysine structural unit and the tartaric acid structural unit is 95:05, as shown by 1 Determined by H NMR.

[0421] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 50 g of a polylysine copolymer, 29.0 g of acrylic acid, and 80 g of DI water. The pH of the mixture was close to 3. The pH could be slightly adjusted to exactly 3 by adding a small amount of HCl (1 mol / L) or NaOH solution (1 mol / L). The mixture was then heated to an internal temperature of 70°C for 24 h under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 h to obtain the final product. The solid content was 100% and the active substance content was 96.4 wt%, as determined by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 29%, and the molecular weights as determined were Mn = 1,047 g / mol and Mw = 1,590 g / mol.

[0422] Example 19

[0423] 250g of L-Lysine, 30g of tartaric acid and 120g of water were loaded into a 500ml four-necked flask equipped with an agitator, an internal thermometer, a gas inlet pipe, a condenser with a reduced pressure connection and a Dean-Stark receiver. The mixture was heated to an internal temperature of 160°C under stirring. After a reaction time of 2h 25min, water was further distilled off under reduced pressure (670 mbar). Finally, 127g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The K-value was measured to be 10.9. The molar ratio of the lysine structural unit to the tartaric acid structural unit is 95:05, as shown by 1 Determined by H NMR.

[0424] A 250 ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser was charged with 50 g of a polylysine copolymer, 29.0 g of acrylic acid, and 80 g of DI water. The pH of the mixture was close to 3. The pH could be slightly adjusted to exactly 3 by adding a small amount of HCl (1 mol / L) or NaOH solution (1 mol / L). The mixture was then heated to an internal temperature of 70°C for 24 h under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48 h to obtain the final product. The solid content was 100% and the active substance content was 96.1 wt %, as determined by1 As determined by H NMR. 1 The degree of modification (DM) of the polymer determined by H NMR was 33%, and the molecular weights as determined were Mn = 995 g / mol and Mw = 1,425 g / mol.

[0425] Example 20

[0426] 250g of L-Lysine, 30g of tartaric acid and 120g of water are loaded into a 500ml four-necked flask equipped with agitator, internal thermometer, gas inlet pipe, condenser with decompression connection and Dean-Stark receiver. The mixture is heated to an internal temperature of 160°C under stirring. Finally, 125g of water distillate is collected, and the highly viscous polymer is discharged into a silicone container as quickly as possible while it is still hot and flowable. The K-value is measured to be 10.3. The molar ratio of lysine structural unit and tartaric acid structural unit is 92:08, as determined by1H NMR.

[0427] 80g polylysine copolymer, 56.7g acrylic acid and 135g DI water were loaded into a 500ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. The pH of the mixture was close to 3. The pH could be slightly adjusted to exactly 3 by adding a small amount of HCl (1mol / L) or NaOH solution (1mol / L). The mixture was then heated to an internal temperature of 70°C for 24h under stirring. After the reaction mixture was cooled to 25°C, the modified polymer was precipitated with an excess of acetone (1:10 by weight). After three consecutive precipitation steps, the supernatant was transparent and colorless, and the precipitate was dried in a vacuum oven at 40°C for more than 48h to obtain the final product. The solid content was 100% and the active substance content was 99.3wt%, as determined by 1H NMR. The degree of modification (DM) of the polymer as determined by 1H NMR was 51%, and the molecular weights as determined were Mn = 1,060 g / mol and Mw = 1,481 g / mol.

[0428] Comparative Example 1

[0429] 200g of lysine, 22.82g of tartaric acid and 108g of DI water were loaded into a 500ml four-necked flask equipped with an agitator, an internal thermometer, a gas inlet pipe, a condenser with a reduced pressure connection and a receiver. The mixture was heated to an internal temperature of 160°C for 2h 50min under stirring, with continuous water separation. When 108g of distilled water was collected, an additional 28.52g of tartaric acid was introduced into the reactor. After the total reaction time of 3h 50min, water was further distilled off under reduced pressure (900 mbar). Finally, 131g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of lysine was determined to be 12.1. The molar ratio of lysine structural unit and tartaric acid structural unit is 83:17, as shown by 1 Determined by H NMR.

[0430] 145.6g sodium chloroacetate, 175g polylysine copolymer and 480g DI water were charged into a 2000ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. Then, the solution was heated until 70°C for 5h. At the same time, the pH was maintained at 10 by controlling the addition of 48%wt. of NaOH aqueous solution using the control unit of the Systag FlexyPat automated laboratory reactor equipped with a membrane pump and a pH probe with a high-temperature electrolyte. After the reaction mixture was cooled to 30°C, the modified polymer was precipitated with excess methanol (1:10 by weight) and filtered. After three consecutive precipitation steps, the product was dried in a vacuum oven at 40°C for more than 16 hours to obtain a final product having a solid content of 100% and an active substance content of 96.8wt%, as obtained by 1 As determined by H NMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 45%, and the molecular weights as determined were Mn = 1,045 g / mol and Mw = 1,820 g / mol.

[0431] Comparative Example 2

[0432] 82.5g of L-Lysine, 9.4g of tartaric acid and 90g of water were loaded into a 500ml four-necked flask equipped with an agitator, an internal thermometer, a gas inlet pipe, a condenser with a reduced pressure connection and a Dean-Stark receiver. The mixture was heated to an internal temperature of 160°C under stirring. After a reaction time of 2h 25min, water was further distilled off under reduced pressure (670 mbar). Finally, 94g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The K-value was measured to be 11.6. The molar ratio of the lysine structural unit to the tartaric acid structural unit is 91:9, as shown by 1 Determined by H NMR.

[0433] 18.08g of sodium chloroacetate, 27.5g of lysine copolymer and 70g of DI water were charged into a 250ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. Then, the solution was heated until 70°C for 5 hours. At the same time, the pH was maintained at 10 by controlling the addition of 48wt% of NaOH aqueous solution using the control unit of a Systag FlexyCube automated laboratory reactor equipped with a peristaltic pump and a pH probe with a high-temperature electrolyte. After the reaction mixture was cooled to 30°C, the modified polymer was precipitated with excess methanol (1:10 by weight) and filtered. After three consecutive precipitation steps, the product was dried in a vacuum oven at 40°C for more than 16 hours to obtain a final product having a solid content of 100% and an active substance content of 97.6%. As obtained by 1 The degree of modification (DM) of the polymer as determined by H NMR was 32%, and the molecular weights as determined were Mn = 1,018 g / mol and Mw = 1,547 g / mol.

[0434] Comparative Example 3

[0435] Into a 500ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet pipe, a condenser with a reduced pressure connection and a Dean-Stark receiver, an aqueous solution of 100g of L-Lysine (50wt%) was loaded. The mixture was heated to an internal temperature of 160°C for 45 minutes under stirring. Then, an aqueous solution of 400g of L-Lysine (50wt%) was continuously metered in over 3.5 hours with continuous water separation. After a reaction time of 1 hour, water was further distilled off under reduced pressure (670 mbar). Finally, 259g of water distillate was collected, and the highly viscous polymer was discharged as quickly as possible into a silicone container while it was still hot and flowable. The k-value of the lysine homopolymer was determined to be 10.6.

[0436] 3.93g of sodium chloroacetate, 18.75g of lysine homopolymer and 56.25g of DI water were charged into a 250ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. Then, the solution was heated until 70°C for 5 hours. During the first 1.5 hours, 15.72g of sodium chloroacetate and 13.5g of sodium hydroxide (50wt%) were added to the flask in 3 portions (every 0.5 hour). After the reaction mixture was cooled to 30°C, the modified polymer was precipitated with excess methanol (1:10 by weight) and filtered. After three consecutive precipitation steps, the product was dried in a vacuum oven at 40°C for more than 16 hours to obtain a final product with a solid content of 100% and an active substance content of 94wt%, as obtained by 1 As determined by HNMR. 1 The degree of modification (DM) of the polymer as determined by H NMR was 45%, and the molecular weights as determined were Mn = 1,067 g / mol and Mw = 1,619 g / mol.

[0437] Comparative Example 4

[0438] 104.65g of sodium chloroacetate, 50g of linear ε-polylysine and 154.65g of DI water were loaded into a 1000ml four-necked flask equipped with a stirrer, an internal thermometer, a gas inlet tube, and a condenser. Then, the solution was heated until 70°C for 5 hours. At the same time, the control unit of a Systag FlexyCube automated laboratory reactor equipped with a peristaltic pump and a pH probe with a high-temperature electrolyte was used to maintain the pH at 10 by controlling the addition of 48wt% of an aqueous NaOH solution. After the reaction mixture was cooled to 30°C, the pH of the solution was adjusted to 4 using an aqueous HCl solution. Then, the modified polymer was precipitated with an excess of methanol (1:10 by weight) and filtered. After three consecutive precipitation steps, the product was dried in a vacuum oven at 40°C for more than 16 hours to obtain a final product with a solid content of 100% and an active substance content of 84%. The degree of modification (DM) of the polymer as determined by 1H NMR was 86%, and the molecular weights as determined were Mn = 10,864 g / mol and Mw = 11,384 g / mol.

[0439] Application Testing

[0440] IV. Anti-ashing test

[0441] Test 1:

[0442] A Terg-o-meter (RHLG-IV, from Shanghai Banking Equipment Co., Ltd., China) comprising 12 drums with corresponding rotor blades as washing units was used to simulate the laundry process in the laboratory, generally following GBT 13174-2008. The washing units were operated at the same stirring speed of 120 revolutions per minute (rpm), and each was filled with 1 L of washing liquid. The white test fabric was washed in the same drum at 30° C. with 10 g of a yellow clay and oil mixture in a washing liquid containing a detergent formulation as shown in Table 17. After washing, the fabric was removed from the washing unit, drained and rinsed twice in 10 L of tap water for 30 seconds each time, and dried in air. The details of the washing cycle are summarized in Table 18.

[0443] The anti-greying properties of the fabrics were measured by measuring the fabrics before washing (R 之前 ) and after washing (R 之后 ) to characterize the difference in relief.

[0444] The remission difference (ΔR) was calculated according to the following equation:

[0445] ΔR=R 之前 -R 之后 .

[0446] The smaller the ΔR value, the better the performance.

[0447] Table 17

[0448]

[0449] a) Based on the active substance content of all ingredients

[0450] b)C 12 -C 14 Fatty alcohol ethoxylate (7EO), commercially available from BASF.

[0451] Table 18

[0452]

[0453]

[0454] Table 19

[0455] additive ΔR, total for all fabrics blank 44.87 Modified PEI-2 34.27 <![CDATA[Polyacrylic acid a) > 38.46 Example 15 35.55 Example 16 33.74 Example 17 38.53

[0456] a) Acrylic acid homopolymer (partially neutralized), available from BASF.

[0457] Test 2:

[0458] Generally follow ASTM D4008-16 using Terg-o-meter (Testfabrics, West Pittston, Pennsylvania, the United States) to simulate the washing process in the laboratory. Several white test samples are washed at 30 ° C in a washing solution containing a liquid detergent formulation detailed in Table 20 and a selected polymer together with 0.5g Georgia red clay. After washing, the test fabric is rinsed and wrung out by hand. The wash cycle is repeated three times (four times in total) with fresh Georgia red clay and new washing solution. After the fourth wash, the test fabric is rinsed, spin dried in a wringer and dried for 30 minutes in a dryer at a medium temperature setting. The details of the wash cycle are summarized in Table 21.

[0459] The anti-redeposition performance was determined by measuring the L, a and b values ​​of the white test fabric before and after washing using a Konica Minolta spectrophotometer. The ΔE value was then calculated from the obtained values ​​according to the following equation:

[0460] ΔE=(ΔL *2 +Δa *2 +Δb *2 ) 1 / 2

[0461] Where ΔL*=L* 洗涤 -L* 初始 ; Δa*=a* 洗涤 -a* 初始 ; and Δb* = b* 洗涤 -b* 初始 .

[0462] The smaller the ΔE value, the better the performance.

[0463] Table 20

[0464]

[0465] a) Based on the active substance content of all ingredients

[0466] b) Fatty alcohol ether sulfates, commercially available from BASF

[0467] c) Lauryl alcohol ethoxylate, commercially available from BASF

[0468] Table 21

[0469]

[0470]

[0471] Table 22

[0472]

[0473]

[0474] Test 3:

[0475] The washing process was simulated with a Launder-o-meter (LP2 Typ, SDL Atlas Inc., USA). The details of the washing cycle are summarized in Table 23. The white test fabric was washed in the same beaker with 2.5 g EMPA101 and 2.5 g SBL 2004 and 20 steel balls at 30°C in a wash liquor containing a detergent having a formulation as shown in Table 24, and then rinsed and spin-dried to complete the wash cycle. The wash cycle was repeated twice with a new clay dispersion and a new wash liquor. After rinsing in the third wash cycle, the test fabric was dried in air instead.

[0476] The anti-greying performance was characterized by the relief R value of the soiled fabric before and after washing, by measuring the fabric with a spectrophotometer Elrepho 2000 from Datacolor at 460 nm. The higher the relief R value, the better the performance. The results are summarized in Table 25.

[0477] Table 23

[0478]

[0479]

[0480] Table 24

[0481]

[0482] a) Active substance content based on all ingredients / solid content based on polymer components b) Linear alkylbenzene sulfonate Maranil DBS / LC (BASF)

[0483] Table 25

[0484] additive R, the sum of all fabrics blank 540.2 Example 12 567.0

[0485] Detergency performance

[0486] Test 1:

[0487] The primary detergency performance of protease-related stains is determined as follows. A Terg-o-meter (Testfabrics, West Pittston, Pennsylvania, USA) is used to simulate the washing process in the laboratory. A mixture of fabrics soiled with standardized stains is washed with 30 g of unsoiled ballast fabric at 30°C in a wash liquor containing the liquid detergent formulation of Table 26 in the presence or absence of enzymes. After the wash cycle, the test fabric and ballast are rinsed and spin-dried in a wringer. The stain sample is then separated from the ballast fabric, shaded and hung to dry. The details of the washing process are summarized in Table 27.

[0488] The primary detergency was determined by measuring the L, a and b values ​​of the soiled test fabrics before and after washing using a Mach5+ ColourConsult spectrophotometer from the Center for Testmaterials. The ΔE value was then calculated from the obtained pre- and post-wash values ​​according to the following equation:

[0489] ΔE=(ΔL *2 +Δa *2 +Δb *2 ) 1 / 2

[0490] Where ΔL*=L* 洗涤 -L* 初始 ; Δa*=a* 洗涤 -a* 初始 ; and Δb* = b* 洗涤 -b* 初始 .

[0491] The higher the ΔE value, the better the performance. Table 28 shows the detergency performance of different polymer additives in the absence and presence of laundry proteases.

[0492] Table 26

[0493]

[0494] a) Based on the active substance content of all ingredients

[0495] Table 27

[0496]

[0497] Table 28

[0498]

[0499]

[0500] Test 2:

[0501] A Launder-o-meter (LP2 Typ, Slide Atlas, USA) was used to simulate the washing process using the liquid laundry formulations in Table 29 and according to the protocol as described in Table 30. A soil monitor was used to evaluate the detergency of outdoor and fat stains.

[0502] Table 29

[0503]

[0504] a) Active substance content based on non-polymer components and solid content based on polymer components

[0505] Table 30

[0506]

[0507]

[0508] The primary detergency is characterized by the ΔE value calculated according to DIN EN ISO 11664-4 (June 2012) according to the following equation:

[0509] ΔE=(ΔL *2 +Δa *2 +Δb *2 ) 1 / 2 ,

[0510] in

[0511] ΔL*=L* 洗涤 -L* 初始 ; Δa * =a* 洗涤 -a* 初始 ; and Δb * =b* 洗涤 -b* 初始 .

[0512] The spectrophotometer MACH 5 from Colour Consult, supplied by CFT, NL-Vlaardingen, was used to measure L on stained fabrics before and after washing. * 、a * 、b * The higher the ΔE value, the better the performance.

[0513] The characterization by ΔE was performed twice, and the average value was given as the test result. The higher the ΔE value, the better the performance. The test results are summarized in Table 31.

[0514] Table 31

[0515]

[0516] VBiodegradability

[0517] The biodegradability was measured by using the above method. The results are listed in Table 32.

[0518] Table 32

[0519] 28 days (%) 56 days (%) Example 7 41 52 Example 16 53 56 Example 17 46 - Example 18 9 25 Example 19 13 25 Example 20 29 68

Claims

1. A modified lysine-based polymer obtainable or obtained by a process comprising subjecting at least a portion of the free amino groups in the lysine-based polymer to Michael addition with a Michael acceptor selected from at least one of an unsaturated carboxylic acid and an unsaturated carboxylic acid ester.

2. The modified lysine-based polymer according to claim 1, wherein The Michael acceptor is at least one selected from the group consisting of: α,β-ethylenically unsaturated monocarboxylic acids having 3 to 10 carbon atoms, α,β-ethylenically unsaturated dicarboxylic acids having 4 to 8 carbon atoms, α,β-ethylenically unsaturated tricarboxylic acids having 4 to 8 carbon atoms, α,β-ethylenically unsaturated carboxylic acids having more carboxylic acid groups, and any esters thereof.

3. The modified lysine-based polymer according to claim 2, wherein The Michael acceptor is at least one selected from the group consisting of acrylic acid, methacrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, aconitic acid, and any esters thereof.

4. The modified lysine-based polymer according to claim 3, wherein The Michael acceptor is at least one selected from the group consisting of acrylic acid, maleic acid, itaconic acid and any esters thereof.

5. The modified lysine-based polymer according to any one of the preceding claims, wherein The ester is selected from polyoxyalkylene esters or blocked polyoxyalkylene esters of the unsaturated carboxylic acid, preferably blocked polyethylene oxide esters, blocked polypropylene oxide esters or blocked polybutylene oxide esters, or a combination thereof.

6. A modified lysine-based polymer according to any one of the preceding claims, wherein The capped polyethylene oxide ester contains a capping group selected from C1-C4-alkyl or C1-C4-hydroxyalkyl.

7. The modified lysine-based polymer according to claim 5 or 6, wherein The polyalkylene oxide or capped polyalkylene oxide portion has a number average molecular weight of 100 to 2,000, preferably 200 to 1,200, and more preferably 400 to 800.

8. A modified lysine-based polymer comprising structural units derived from a lysine monomer represented by: in R2 and R3 are independently H or R4, provided that at least one of R2 and R3 is R4, * indicates the position at which this structural unit is attached to any other structural unit via an amide linkage, R4 is a moiety represented by formula (II) in R5 and R6 are independently H, C1-C6-alkyl, carboxyl (-COOH), -COOM, -(C1-C4-alkylene)-COOH or -(C1-C4-alkylene)-COOM, R7 is H, C1-C6-alkyl, -(CH2CH2O) n -R8 or M, R8 is C1-C4-alkyl, M is a cation selected from alkali metal cations, alkaline earth metal cations, ammonium and amine cations, n is a number in the range of 2 to 40, and ** indicates the position where the moiety is attached to the N atom carrying R4.

9. The modified lysine-based polymer according to claim 8, wherein R5 and R6 are independently H, C1-C4-alkyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM, R7 is H, -(CH2CH2O) n -R8 or M, R8 is C1-C2-alkyl, and n is a number in the range of 4 to 25.

10. The modified lysine-based polymer according to claim 9, wherein R5 is H, methyl, carboxyl (-COOH), or -COOM, R6 is H, methyl, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM, R7 is H, -(CH2CH2O) n -R8 or M, R8 is C1-C2-alkyl, and n is a number in the range of 8 to 15.

11. The modified lysine-based polymer according to claim 10, wherein R5 is H, carboxyl (-COOH), or -COOM, R6 is H, carboxyl (-COOH), -COOM, -(C1-C2-alkylene)-COOH or -(C1-C2-alkylene)-COOM, R7 is H, -(CH2CH2O) n -R8 or M, and R8 is methyl.

12. The modified lysine-based polymer according to any one of the preceding claims, which is a modified lysine homopolymer.

13. The modified lysine-based polymer according to any one of the preceding claims 1 to 11, which is a modified lysine copolymer comprising more than 50 mol% of structural units derived from lysine monomers and less than 50 mol% of structural units derived from at least one dicarboxylic acid or an amide-forming derivative thereof.

14. The modified lysine-based polymer according to claim 13, comprising (A) 60 to 99 mol % of structural units derived from lysine monomers, (B) 1 to 40 mol % of structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof HOOC-R1-COOH(I) in R1 is a direct bond or an aliphatic straight-chain alkylene group, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted alkyl, unsubstituted or substituted alkoxy, unsubstituted or substituted alkylthio, unsubstituted or substituted alkylamino, di(alkyl)amino, alkylene, hydroxyl, mercapto, amino and halogen.

15. The modified lysine-based polymer according to claim 14, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 24 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 18 -alkyl, unsubstituted or substituted C1-C 18 -alkoxy, unsubstituted or substituted C1-C 18 -alkylthio, unsubstituted or substituted C1-C 18 -alkylamino, di(C1-C 18 -alkyl)amino, C1-C6-alkylene, hydroxy, mercapto, amino and halogen.

16. The modified lysine-based polymer according to claim 15, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 18 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C 12 -alkyl, unsubstituted or substituted C1-C 12 -alkoxy, unsubstituted or substituted C1-C 12 -alkylthio, unsubstituted or substituted C1-C 12 -alkylamino, di(C1-C 12 -alkyl)amino, C1-C4-alkylene, hydroxy, mercapto, amino and halogen.

17. The modified lysine-based polymer according to claim 16, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond or an aliphatic straight chain C1-C 12 -alkylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C8-alkyl, unsubstituted or substituted C1-C8-alkoxy, unsubstituted or substituted C1-C8-alkylthio, unsubstituted or substituted C1-C8-alkylamino, di(C1-C8-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

18. The modified lysine-based polymer according to claim 17, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene, which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, unsubstituted or substituted C1-C4-alkoxy, unsubstituted or substituted C1-C4-alkylthio, unsubstituted or substituted C1-C4-alkylamino, di(C1-C4-alkyl)amino, C1-C4-alkylene, hydroxyl, mercapto, amino and halogen.

19. The modified lysine-based polymer according to claim 18, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, a C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C4-alkylene, hydroxy, mercapto and amino.

20. The modified lysine-based polymer according to claim 19, comprising (B) structural units derived from at least one dicarboxylic acid of formula (I) or an amide-forming derivative thereof, wherein R1 is a direct bond, C1-C 12 -alkylene or C2-C 12 -alkenylene which is unsubstituted or substituted by at least one group selected from the group consisting of unsubstituted or substituted C1-C4-alkyl, C1-C2-alkylene, hydroxyl and amino, preferably at least one of oxalic acid, malonic acid, succinic acid, maleic acid and fumaric acid, tartaric acid, aspartic acid, glutaric acid, itaconic acid, glutamic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid and dodecanedioic acid.

21. The modified lysine-based polymer according to any one of the preceding claims 14 to 20, comprising (A) 70 to 97 mol% of structural units derived from lysine monomers; and (B) 3 to 30 mol % of structural units derived from at least one dicarboxylic acid of the formula (I) or an amide-forming derivative thereof.

22. The modified lysine-based polymer according to claim 21, comprising (A) 75 to 97 mol% of structural units derived from lysine monomers; and (B) 4 to 25 mol % of structural units derived from at least one dicarboxylic acid of the formula (I) or an amide-forming derivative thereof.

23. The modified lysine-based polymer according to claim 22, comprising (A) 75 to 95 mol% of the lysine structural unit; and (B) 5 to 25 mol% of the dicarboxylic acid structural unit.

24. A modified lysine-based polymer according to any one of the preceding claims, having a degree of modification via Michael addition of at least 10%, such as at least 20%.

25. The modified lysine-based polymer according to any one of the preceding claims, having a weight average molecular weight (Mw) in the range of 600 to 20,000 g / mol, and / or having a number average molecular weight (Mn) in the range of 500 to 20,000 g / mol.

26. A detergent composition, preferably a laundry detergent composition, comprising the modified lysine-based polymer according to any one of the preceding claims 1 to 25.

27. The detergent composition according to claim 26, wherein The detergent composition comprises the modified lysine-based polymer in an amount of 0.5 to 30%, preferably 1 to 25% and more preferably 1 to 15% by weight based on the total solid content of the detergent composition.

28. A detergent composition according to claim 25 or 26, comprising 2-phenoxyethanol, preferably in an amount of 2 ppm to 5%, more preferably 0.1% to 2% by weight based on the total weight of the detergent composition.

29. The detergent composition according to claim 25 or 26, comprising 4,4'-dichloro-2-hydroxydiphenyl ether, preferably in an amount of 0.001% to 3%, preferably 0.002% to 1%, more preferably 0.01% to 0.6%, based on the total weight of the detergent composition.

30. A detergent composition according to any one of the preceding claims 26 to 29, comprising at least one enzyme, preferably at least one enzyme selected from the group consisting of proteases, amylases, lipases, cellulases, mannanases, xylanases, deoxyribonucleases, dispases, pectinases, oxidoreductases and cutinases.

31. Use of a modified lysine-based polymer according to any one of claims 1 to 25 in a detergent composition, especially a laundry detergent composition.

32. Use of the modified lysine-based polymer according to any one of claims 1 to 25 as a dispersant.

33. A method of preserving an aqueous detergent composition comprising a modified lysine-based polymer according to any one of the preceding claims 1 to 25 from microbial contamination or growth, comprising adding 2-phenoxyethanol to the detergent composition.

34. A method of laundering fabrics or cleaning hard surfaces comprising treating the fabrics or hard surfaces antimicrobially with a detergent composition comprising the modified lysine-based polymer according to any one of the preceding claims 1 to 25 and 4,4'-dichloro-2-hydroxydiphenyl ether.