Floating sealing material and manufacturing method thereof

By adjusting the element ratio and process conditions in the floating sealing material, an excellent carbide structure is formed, which solves the problem of insufficient formability and sintering resistance of Ni hard cast iron under high load, and achieves high hardness, excellent formability and resistance. Sintering.

CN119032190APending Publication Date: 2024-11-26EAGLE INDS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033394.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-11
Filing Date
2023-05-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing Ni hard cast iron floating sealing materials cannot meet the requirements of high hardness, formability and sintering resistance under high loads, and are prone to oxide generation and casting defects, resulting in low formability.

Method used

By adjusting the element ratio in the floating sealing material, the content is ensured to be within a specific range, including Fe, C, Si, Mn, Cr and Mo, to form excellent carbide structure and dispersed phases, and centrifugal casting and cooling processes are used to improve forming. properties and hardness.

Benefits of technology

High hardness, excellent formability and sintering resistance are achieved, oxide generation and casting defects are reduced, and the overall performance of floating sealing materials is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032190A_ABST
    Figure CN119032190A_ABST
Patent Text Reader

Abstract

The floating seal material contains at least Fe, C, Si, Mn, Cr, and Mo, the content of C being 2.3% by weight or more and 3.8% by weight or less, the content of Si being 0.7% by weight or more and 2.5% by weight or less, the content of Mn being 0.3% by weight or more and 1.3% by weight or less, the content of Cr being 3% by weight or more and 13% by weight or less, and the content of Mo being 1.8% by weight or more and 15% by weight or less, with the remainder being Fe and unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a floating sealing material and a manufacturing method thereof. Background Art

[0002] The floating seal device is used as a seal for track rollers of construction machinery or vehicles, etc., and its purpose is to prevent mud, water, sand, etc. from invading the inside of the wheel, and to prevent the lubricating oil filled in the wheel from leaking to the outside. The floating seal device is composed of a pair of fixed side floating seal rings and a rotating side floating seal ring, and is arranged on the outer periphery of the shaft in a state of not contacting the shaft, that is, in a state of floating from the shaft. In addition, each of the floating seal rings on the fixed side and the rotating side has a sliding surface that can slide in contact with each other as an opposing surface, and is used in a state of facing each other via the sliding surface.

[0003] The floating seal rings on the fixed side and the rotating side are assembled to the fixed side structure and the rotating side structure via O-rings, and the two floating seal rings are pressed together via sliding surfaces using the elastic force of the O-rings. Therefore, whether rotating or not, the fixed side structure and the rotating side structure can be sealed, and muddy water, sand and soil can be prevented from intruding into the wheel and lubricating oil can be prevented from leaking to the outside.

[0004] The material constituting such a floating seal ring is required to have various properties. For example, Patent Document 1 discloses a cast iron material and a floating seal material composed of the cast iron material. The cast iron material contains carbon, silicon, manganese, nickel and chromium as essential components and the content of each element is controlled within a specific range. As a result, the cast iron material has high hardness and excellent wear resistance and abrasive wear resistance.

[0005] (Prior art literature)

[0006] (Patent Document)

[0007] Patent Document 1: Japanese Patent Application Publication No. 2005-240065 Summary of the invention

[0008] (Problems to be solved by the invention)

[0009] As mentioned above, the floating seal material is required to have various characteristics, and it is expected to develop a material that not only has the excellent characteristics required by patent document 1, but also maintains high hardness and excellent formability and sintering resistance. According to the research of the inventor, it is known that in the Ni (nickel) hard cast iron disclosed in patent document 1, sintering occurs in high-load applications, and it is impossible to obtain a material that meets these characteristics. Specifically, in the Ni hard cast iron of patent document 1, due to poor chemical stability and low hardness, the sintering resistance is low. In addition, since it contains a few percent of residual austenite, this also causes the sintering resistance to become low. Furthermore, martensite will also flow plastically and sinter under a relatively high load. In addition, in order to suppress sintering, it is known to use high Cr (chromium) cast iron, but since it contains a large amount of Cr, the generation of oxides in the atmospheric melting in the manufacturing stage is intense. Therefore, the oxygen content in the molten metal also becomes more, and casting defects such as oxide inclusion or pinholes are prone to occur in the final formed body, and the formability becomes low.

[0010] Therefore, an object of the present invention is to provide a floating seal material having excellent moldability and seizure resistance while maintaining high hardness, and a method for producing the floating seal material.

[0011] (Measures taken to solve the problem)

[0012] The present inventors have conducted studies to solve the above-mentioned problems and have found that the above-mentioned problems can be solved by adjusting the ratio of elements in the material constituting the floating seal material to a specific range, thereby completing the present invention.

[0013] That is, the gist of the present invention is as follows.

[0014] [1] A floating sealing material, wherein:

[0015] Contains at least Fe, C, Si, Mn, Cr and Mo,

[0016] The C content is greater than 2.3 wt% and less than 3.8 wt%, the Si content is greater than 0.7 wt% and less than 2.5 wt%, the Mn content is greater than 0.3 wt% and less than 1.3 wt%, the Cr content is greater than 3 wt% and less than 13 wt%, the Mo content is greater than 1.8 wt% and less than 15 wt%, and the balance is Fe and unavoidable impurities.

[0017] [2] The floating sealing material according to [1], wherein:

[0018] Contains at least one of carbides represented by M3C and M7C3 (M is Fe, Si, Mn, Cr or Mo) composed of at least a part of the Fe, Si, Mn, Cr or Mo and at least a part of the C.

[0019] [3] The floating seal material according to [1] or [2], comprising a carbide represented by M6C (M is Fe, Si, Cr or Mo) composed of at least a part of the Fe, Si, Cr or Mo and at least a part of the C.

[0020] [4] The floating sealing material according to [2] or [3], wherein:

[0021] having a phase-separated structure containing at least one dispersed phase in a matrix phase,

[0022] The dispersed phase includes a granular phase having an average particle size of 1 μm or less and composed of at least one of the carbides represented by M3C, M7C3, and M6C.

[0023] [5] A floating seal device, wherein:

[0024] A floating sealing material including any one of [1] to [4].

[0025] [6] A method for manufacturing a floating sealing material, comprising:

[0026] a molten metal preparing step of preparing a molten metal, the molten metal containing at least Fe, C, Si, Mn, Cr and Mo, wherein a C content is 2.3 wt% to 3.8 wt% inclusive, a Si content is 0.7 wt% to 2.5 wt% inclusive, a Mn content is 0.3 wt% to 1.3 wt% inclusive, a Cr content is 3 wt% to 13 wt% inclusive, a Mo content is 1.8 wt% to 15 wt% inclusive, and the balance is Fe and unavoidable impurities; and

[0027] A casting process of pouring the molten metal into a mold.

[0028] [7] The method for manufacturing a floating sealing material according to [6], wherein:

[0029] In the casting step, the molten metal is cast into the mold by centrifugal casting.

[0030] [8] The method for manufacturing a floating seal material according to [6] or [7], wherein:

[0031] The method includes cooling the mold after the casting step to cool and solidify the molten metal.

[0032] (Effects of the Invention)

[0033] According to the present invention, it is possible to provide a floating seal material having excellent moldability and seizure resistance (particularly seizure resistance under high load) while maintaining high hardness, and a method for producing the floating seal material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a cross-sectional view of a floating seal device according to an embodiment.

[0035] Figure 2 This is an electron microscope photograph (a photograph replacing a drawing) showing an example of the structure of a floating seal material.

[0036] Figure 3 This is a diagram for explaining the structure of a floating seal material.

[0037] Figure 4 The electron microscope photographs of the floating seal materials according to Examples 1 to 4 (photographs replacing drawings) are shown.

[0038] Figure 5 The electron microscope photographs of the floating seal materials according to Examples 5 to 7 (photographs replacing drawings) are shown. DETAILED DESCRIPTION

[0039] The present invention will be described in detail below, but the description of the constituent elements described below is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and the present invention can be implemented by making various modifications within the scope of the gist thereof.

[0040] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit, and "A to B" means A or more and B or less.

[0041] In addition, although a plurality of embodiments are described in this specification, various conditions in the respective embodiments can be mutually applied within the applicable range.

[0042] <Structure of floating seal>

[0043] A floating seal material (hereinafter also referred to as "floating seal material") as one embodiment of the present invention contains at least Fe, C, Si, Mn, Cr and Mo.

[0044] The C content is greater than 2.3 wt% and less than 3.8 wt%, the Si content is greater than 0.7 wt% and less than 2.5 wt%, the Mn content is greater than 0.3 wt% and less than 1.3 wt%, the Cr content is greater than 3 wt% and less than 13 wt%, the Mo content is greater than 1.8 wt% and less than 15 wt%, and the balance is Fe and unavoidable impurities.

[0045] The floating seal material contains C (carbon). By changing the content of C, the amount of carbides constituting the chill structure can be controlled. In addition, C has the effect of promoting the dendritic crystallization of crystal grains and adjusting the matrix structure.

[0046] The content of C in the floating seal material is not particularly limited as long as it is 2.3% by weight or more and 3.8% by weight or less, but is preferably 2.5% by weight or more, more preferably 2.7% by weight or more, and further preferably 2.9% by weight or more. In addition, it is preferably 3.6% by weight or less, more preferably 3.5% by weight or less, and further preferably 3.4% or less. If the content of C is lower than the above range, there is a tendency that excellent formability cannot be obtained. In addition, when it exists as a crystal of carbide, there is a tendency that the content of the carbide in the microstructure decreases, and the wear resistance and machinability of the base material deteriorate. As the crystal of the carbide, for example, M3C, M7C3 or M6C can be cited, and it is preferably composed of at least one of the carbides represented by M3C, M7C3 and M6C (M is, for example, Fe, Cr, Si, Mn or Mo). On the other hand, if the C content exceeds the above range, excellent formability tends not to be obtained. In addition, carbide cementite in the cold hardened structure coarsens, pores caused by remelting are easily generated in the refined structure, and further, the amount of graphite increases, and the strength of the cast iron tends to decrease.

[0047] The floating seal material contains Si (silicon). Si has the effect of releasing carbon from pig iron and promoting graphitization of cast iron after casting, and also has the effect of making crystal grains dendritic or columnar.

[0048] The content of Si in the floating seal material is not particularly limited as long as it is 0.7% by weight or more and 2.5% by weight or less, but is preferably 1.0% by weight or more, more preferably 1.5% by weight or more, further preferably 1.7% by weight or more, particularly preferably 1.9% by weight or more, and preferably 2.4% by weight or less, more preferably 2.3% by weight or less, and further preferably 2.2% by weight or less. If the content of Si is lower than the above range, there is a tendency that excellent formability cannot be obtained, and there is also a tendency that the hardening of the base material cannot be promoted, the base material itself is miniaturized, and the cutting processability is significantly reduced. On the other hand, if the amount of Si exceeds the above range, there is a tendency that excellent hardness, formability and sintering resistance cannot be obtained, and there is also a tendency that excessive carbon liberation proceeds and toughness is reduced.

[0049] The floating seal material contains Mn (manganese). When S (sulfur) is contained as an impurity, Mn combines with S to form manganese sulfide, which has the effect of suppressing the adverse effects caused by S mixing into cast iron, the effect of making the structure finer, and the effect of suppressing graphitization that may be generated by adding Ni when Ni is contained, thereby improving the matrix.

[0050] The content of Mn in the floating seal material is not particularly limited as long as it is 0.3% by weight or more and 1.3% by weight or less, but is preferably 0.5% by weight or more, more preferably 0.7% by weight or more, and further preferably 0.9% by weight or more. In addition, it is preferably 1.25% by weight or less, more preferably 1.20% by weight or less, and further preferably 1.15% by weight or less. If the content of Mn is lower than the above range, there is a tendency that excellent hardness, formability and sintering resistance cannot be obtained. On the other hand, if the content of Mn exceeds the above range, there is a tendency that excellent formability and sintering resistance cannot be obtained, and there is a tendency that the microstructure is significantly refined, the cast iron is embrittled, or the machinability is reduced.

[0051] The floating seal material contains Cr (chromium). Cr forms high-hardness and fine carbides, which has the effect of improving wear resistance and matrix strength.

[0052] The content of Cr in the floating seal material is not particularly limited as long as it is 3% by weight or more and 13% by weight or less, but is preferably 6.5% by weight or more, more preferably 7.0% by weight or more, further preferably 7.5% by weight or more, particularly preferably 8.0% by weight or more, and preferably 9.8% by weight or less, more preferably 9.6% by weight or less, and further preferably 9.4% by weight or less. By setting it to this range, the Cr concentration in the main carbide increases to become a harder carbide. If the Cr content is lower than the above range, there is a tendency that excellent hardness and sintering resistance cannot be obtained. On the other hand, if the Cr content exceeds the above range, there is a tendency that excellent formability cannot be obtained. In addition, the generation of oxides in atmospheric melting is intense, and the oxygen content in the molten metal also increases, and there is a tendency that casting defects such as pinholes and oxide inclusions are easily generated.

[0053] The floating seal material contains Mo (molybdenum). Mo can form carbides (M6C) and the like in cast iron, and also dissolves in the matrix to increase hardness. Cr also forms carbides, but if the Cr content exceeds 10% by weight, it forms oxides during atmospheric melting and deteriorates the formability, so it cannot be too much. When Cr is less than 10% by weight, the sintering resistance is insufficient. In order to compensate for this deficiency, Mo is added to form M6C without deteriorating the formability and increasing the sintering resistance.

[0054] As described above, Mo is dissolved in the matrix, preferably in the metal portion (martensite). When Mo is dissolved in martensite, the crystal lattice is distorted, so-called solid solution strengthening is performed, and the hardness is increased.

[0055] The content of Mo in the floating seal material is not particularly limited as long as it is 1.8% by weight or more and 15% by weight or less, but is preferably 2.0% by weight or more, more preferably 3.0% by weight or more, further preferably 4.0% by weight or more, particularly preferably 5.0% by weight or more, and preferably 14.95% by weight or less. If the content of Mo is lower than the above range, there is a tendency that excellent hardness, formability and sintering resistance cannot be obtained. In addition, if the content of Mo is lower than the above range, the amount of Mo carbide decreases, and the hardness and wear resistance decrease. In addition, if the content of Mo exceeds the above range, the cost becomes high and it is easy to break.

[0056] The floating seal material contains Fe. Fe is contained as a main constituent element, and constitutes the balance other than the above-mentioned C, Si, Mn, Cr and Mo and each element other than C, Si, Mn, Cr and Mo that can be present in an amount of 1 weight % or less. Preferably, Fe constitutes the balance other than C, Si, Mn, Cr and Mo and inevitable impurities.

[0057] The floating seal material may contain inevitable impurities. The types of inevitable impurities are not particularly limited, and may be elements other than the above-mentioned Fe, C, Si, Mn, Cr and Mo and specific arbitrary components, such as P (phosphorus) or S (sulfur). The content of each inevitable impurity in the floating seal material is preferably small, preferably 0 weight % (less than the detection limit), but within the range that can obtain the effect of the present invention, it can be 0 weight %, 0.001 weight %, 0.005 weight %, or 0.01 weight %, and in addition, it is 1 weight % or less, preferably 0.5 weight % or less, more preferably 0.3 weight % or less, further preferably 0.1 weight % or less, particularly preferably 0.05 weight % or less, and even more preferably 0.02 weight % or less.

[0058] In particular, P combines with iron to form steadite (Fe3P), which tends to reduce the machinability of cast iron or make cast iron brittle, so it is preferably as small as possible. Therefore, the P content in the floating seal material is preferably 0.5% by weight or less, more preferably 0.3% by weight or less, and preferably 0% by weight (less than the detection limit), but may be 0% by weight or more within the range in which the effect of the present invention can be obtained.

[0059] In addition, S tends to increase the solidification point of cast iron and deteriorate the fluidity of the molten metal bath or make the cast iron after casting brittle, so it is preferably less. Therefore, the content of P in the floating seal material is preferably 0.1% by weight or less, more preferably 0.05% by weight or less, and further preferably 0.02% by weight or less. In addition, it is preferably 0% by weight (less than the detection limit), but it may be 0% by weight or more within the range that the effect of the present invention can be obtained.

[0060] The floating seal material may further contain at least one selected from the group consisting of V and W as an arbitrary component (also referred to as a "specific arbitrary component") within the scope of being able to obtain the effect of the present invention. These components may contain only one type, or may contain two or more types, but preferably contain only one type. In this specification, "arbitrary component (arbitrary element)" is a component (element) that may or may not be contained. The arbitrary component may be contained as an inevitable impurity, or may be contained as an arbitrary additional component other than this.

[0061] From the viewpoint of ensuring excellent hardness, formability and sintering resistance, the content of each specific arbitrary component in the floating sealing material is preferably less than 1 weight %, or less than 0.9 weight %. In addition, it can be 0 weight % (less than the detection limit), or more than 0 weight % (less than the detection limit), or even more than 0 weight % (less than the detection limit).

[0062] When the above-mentioned optional components and inevitable impurities are separated and the content of each component is 1 weight % or less, the floating seal material involved in this embodiment contains at least Fe, C, Si, Mn, Cr and Mo.

[0063] The C content is greater than 2.3 wt% and less than 3.8 wt%, the Si content is greater than 0.7 wt% and less than 2.5 wt%, the Mn content is greater than 0.3 wt% and less than 1.3 wt%, the Cr content is greater than 6 wt% and less than 10 wt%, the Mo content is greater than 1.8 wt% and less than 15 wt%, the V and W contents are both less than 1 wt%, and the balance is Fe and unavoidable impurities.

[0064] At least a portion of the above-mentioned Fe, Si, Mn, Cr or Mo may also constitute at least one of the carbides represented by M3C and M7C3 (M is Fe, Si, Mn, Cr or Mo, especially Fe or Cr) together with at least a portion of the above-mentioned C.

[0065] At least a part of the above-mentioned Fe, Si, Cr or Mo may also constitute a carbide represented by M6C (M is Fe, Si, Cr or Mo) together with at least a part of the above-mentioned C. The crystal system of this carbide is a cubic system, and it is harder than the carbide represented by the above-mentioned M3C or M7C3, and has excellent wear resistance and excellent thermal conductivity.

[0066] In addition, the above-mentioned M in the floating seal material may form M6C carbide, but may also be present in the above-mentioned M3C or M7C3 carbide or / and martensite in the form of solid solution.

[0067] The floating seal material preferably has a phase separation structure containing at least one dispersed phase in a matrix phase (matrix phase) (main phase, metal matrix), and as the dispersed material, it is preferred to contain a phase composed of at least one of the carbides represented by M3C, M7C3 and M6C. In addition, the dispersed phase is preferably granular, with an average particle size of 1 μm or less. Specifically, for example, when manufacturing the floating seal material in the shape of a floating seal ring described in the floating seal device described later, it is preferred that the sliding surfaces 5 and 10 (see Figure 1 ) is dispersed to form a microstructure. From the viewpoint of improving the hardness of the matrix, as such a microstructure, dendritic cementite and fine carbides mainly composed of Cr are dispersed, and the matrix structure is preferably a structure selected from pearlite, bainite and martensite or a mixed structure thereof, more preferably a mixed structure composed of pearlite, bainite and martensite with martensite as the main body, and further preferably a mixed structure composed of pearlite and martensite with martensite as the main body.

[0068] Normally, the metal part (martensite) plastically flows and is sintered. However, if fine carbides are dispersed in the martensite, the strength of the martensite increases and the sintering resistance improves.

[0069] In addition, Figure 1 In the embodiment, the above-mentioned fine structure can be formed on the sliding surface by making the component composition of the cast iron the composition of this embodiment. In particular, by controlling the addition amount of Cr, the cold hardening depth of the cold hardened structure forming the fine structure can be stabilized.

[0070] The average particle size of the dispersed phase can be determined, for example, by observing the floating seal material using an electron microscope, randomly selecting 100 dispersed phases, measuring the particle size of each dispersed phase, and then calculating the average value thereof.

[0071] The method of dispersing the carbide represented by M3C or M7C3 and / or M6C carbide in the material is not particularly limited, and an example thereof is a method of dispersing the carbide represented by M3C or M7C3 and / or M6C carbide by heat treatment.

[0072] The content of each element constituting the above-mentioned floating seal material can be controlled by adjusting the amount of each element in the raw material when manufacturing the floating seal material.

[0073] Furthermore, the constituent elements of the above-mentioned floating seal material can be analyzed by atomic emission spectrometry.

[0074] Furthermore, the structure of martensite or the like in the above-mentioned floating seal material is determined by structure observation (for example, structure observation using a scanning electron microscope (SEM)) and hardness measurement.

[0075] Figure 2 An example of a photograph of the structure of a floating seal material observed using a scanning electron microscope is shown. Figure 2 In the structure, any one of fine M3C, M7C3, and M6C is dispersed in the main metal matrix phase (martensite) in a manner with an average particle size of less than 1 μm. Figure 3 Shown to illustrate the Figure 2 The composition of each phase in such a structure ( Figure 3 M in is the same as M above). In addition, Figure 3 The organization is not Figure 2 The organization corresponds to the organization recorded. Figure 3 In FIG. 1 , it is shown that there are a phase of "M3C (or M7C3)" and a phase of "M7C3 (or M3C)", which means that one of the phases is M3C and the other is M7C3. In addition, Figure 3 The types of M in each phase can be the same or different. Figure 3 As shown in FIG. 1 , if fine carbides are dispersed in martensite, the strength of the martensite increases and the sintering resistance improves. Figure 2 This is a photograph obtained by observing the structure of a floating seal material according to Example 1 described later using a scanning electron microscope.

[0076] In addition, when the observation object is not circular, the above-mentioned average particle size may be set to the diameter of a circle having the same area (including substantially the same area) as the observation object.

[0077] The shape of the floating seal material is not particularly limited, and a known shape can be adopted, for example, a ring shape that can be used as a known floating seal ring. The size of the floating seal material can be appropriately changed according to the purpose. In the case of a ring shape, the thickness of the innermost diameter portion of the ring can also be appropriately changed according to the purpose.

[0078] The floating seal material according to the present embodiment may also be described as a floating seal material composed of a cast iron material satisfying the above-mentioned conditions of the constituent elements. In this case, the "floating seal material" in the description of the above-mentioned constituent elements can be replaced by "cast iron material".

[0079] <Characteristics of floating seal materials>

[0080] [hardness]

[0081] The hardness of the floating seal material is not particularly limited, but the Rockwell hardness HRC is usually 64 HRC or higher, preferably 65 HRC or higher, more preferably 67 HRC or higher, and further preferably 68 HRC or higher.

[0082] The hardness of the floating seal material can be measured by a Rockwell hardness tester.

[0083] The material constituting the above-mentioned floating seal material (cast iron material) can be used not only for floating seal applications but also can be appropriately used for other applications requiring hardness, formability, and seizure resistance.

[0084] <Method for manufacturing floating seal material>

[0085] The method for producing the above-mentioned floating seal material is not particularly limited, and a known method can be applied.

[0086] As an example of a method for manufacturing a floating seal material, a method for manufacturing a floating seal material as another embodiment of the present invention (also referred to as a "method for manufacturing a floating seal material") includes:

[0087] a molten metal preparing step of preparing a molten metal, the molten metal containing at least Fe, C, Si, Mn, Cr and Mo, wherein a C content is 2.3 wt% to 3.8 wt% inclusive, a Si content is 0.7 wt% to 2.5 wt% inclusive, a Mn content is 0.3 wt% to 1.3 wt% inclusive, a Cr content is 3 wt% to 13 wt% inclusive, a Mo content is 1.8 wt% to 15 wt% inclusive, and the balance is Fe and unavoidable impurities; and

[0088] A casting process of pouring the molten metal into a mold.

[0089] The conditions such as the content of each component constituting the molten metal can be similarly applied to the conditions such as the content of each component including the specific arbitrary component in the description of the composition of the above-mentioned floating seal material.

[0090] Hereinafter, an example of the production method will be described in detail.

[0091] [Molten metal preparation process]

[0092] The method for manufacturing the floating seal material includes a molten metal preparation step of preparing the above-mentioned molten metal. The method for preparing the molten metal is not particularly limited, and for example, raw materials may be prepared in such a manner that the above-mentioned elements are within the above-mentioned content ranges, and these raw materials may be put into a melting furnace, etc., and heated to a temperature at which the raw materials melt, thereby obtaining a molten metal bath (molten metal). The form of the raw materials is not particularly limited, and for example, it may be coke, pig iron, or an iron alloy.

[0093] The heating temperature is not particularly limited as long as it is a temperature at which the raw material can be melted.

[0094] The heating time is not particularly limited.

[0095] The heating atmosphere is not particularly limited and may be air, but is preferably an inert gas such as argon or nitrogen.

[0096] In addition, by using a molten metal having the component composition in the present embodiment, in particular, by using a molten metal having a smaller amount of Cr than a molten metal of a high Cr casting (about 13 weight % or more) commonly used to produce Cr, the melting point of the material can be lowered, thereby improving the formability and fluidity of the molten metal.

[0097] [Casting process]

[0098] The method for producing a floating seal material includes a casting step of casting the molten metal obtained in the above-mentioned molten metal preparation step into a mold. The method of casting the molten metal into the mold is not particularly limited, and for example, a centrifugal casting method can be used.

[0099] The method of casting the molten metal into the mold (casting die) by centrifugal casting is not particularly limited, and a known method can be applied. In addition, the rotation speed of centrifugal casting is not particularly limited.

[0100] The shape of the mold is not particularly limited, and the size can be selected according to the size of the target floating seal material. Also, the material can be a known material.

[0101] In addition, when the floating seal material is manufactured as a floating seal ring, if there is an attachment similar to the molten metal slag composition containing a large amount of Si, Cr and Mn on the inner diameter of the ring, it can be inferred that it was cast by centrifugal casting. In addition, if the particle size of carbides in the finally obtained floating seal material is small and dispersed throughout the structure, it can be inferred that it was cast by centrifugal casting.

[0102] [Cooling process]

[0103] The method for manufacturing the floating seal material may also include a cooling step of cooling the mold after the above-mentioned casting step to cool and solidify the molten metal cast into the mold. The cooling method is not particularly limited, and examples thereof include cooling by leaving it alone, cooling using a blower or a cooler, or cooling by immersing it in a liquid such as water.

[0104] During cooling, for example, when manufacturing a floating seal material in the shape of a floating seal ring described in the floating seal device described later, it is preferable to use a material having a cooling rate faster than other parts to force and preferentially cool the sliding surfaces 5 and 10 (see Figure 1 ) is cooled, preferably the sliding surface is cooled preferentially compared to other parts. In the above mold, as a method of forcibly and preferentially cooling the sliding surface, for example, a method of cooling by passing a refrigerant near the sliding surface, or a method of configuring the mold in a casting method such as a centrifugal casting method so as to preferentially cool the sliding surface, etc. can be cited. In addition, by using such a mold, the sliding surfaces 5 and 10 are forcibly and preferentially cooled at a faster cooling rate than other parts, and a micronized structure can be formed on the sliding surface of the floating seal ring. The micronized structure is the same as the micronized structure described in the above-mentioned floating seal material structure.

[0105] A mold with molten metal (preferably the material in the mold, further, in the above Figure 1 The cooling rate of the sliding surfaces 5 and 10 is not particularly limited, but is preferably 300°C / min or more, more preferably 500°C / min or more, and preferably 700°C / min or less. Whether the cooling rate is too slow or too fast, it is difficult to form the above-mentioned microstructure, so the cooling rate is preferably within the above range.

[0106] In addition, Figure 1 In the method, it is important to utilize the above-mentioned cooling conditions to form the above-mentioned microstructure on the sliding surfaces 5 and 10. Therefore, the cooling performed under the above-mentioned conditions only needs to be performed to about 400 to 500°C, which is the temperature for forming the microstructure. That is, the cooling conditions after the microstructure is formed on the sliding surfaces 5 and 10 are not particularly limited and can be appropriately determined. In addition, by utilizing the above-mentioned cooling conditions, by forming a microstructure in which dendritic cementite and microcarbides mainly composed of Cr are dispersed on the sliding surfaces, the strength and hardness of the cast iron can be improved. In particular, since fine cementite and microcarbides mainly composed of Cr are formed, the shedding of coarse cementite visible in white pig iron, for example, and ablation wear caused by brittle structures can be effectively prevented.

[0107] In addition, as the cooling rate during cooling and solidification, it is possible to Figure 1 The cooling rate (°C / min) of the sliding surface of the floating seal material in the R 1. Set the cooling rate (℃ / min) of the parts other than the sliding surface to C R 2, preferably 1≤C R 1 / C R 2≤2.5, more preferably 1≤C R 1 / C R 2≤2.0, more preferably 1<C R 1 / C R The relationship is 2≤2.0.

[0108] <Floating seal device>

[0109] A floating seal device (also referred to as "floating seal device" for short) according to another embodiment of the present invention is a floating seal device including (having) the above-mentioned floating seal material, in particular, a floating seal ring. The form of the floating seal device is not particularly limited. As an example, the following floating seal device can be cited, which has an annular fixed side housing fixed to a fixed shaft and an annular rotating side housing rotating concentrically with respect to the fixed shaft, and has a pair of floating seal rings, the pair of floating seal rings are arranged on the inner sides of the fixed side housing and the rotating side housing with an annular gap relative to the fixed shaft and slide against each other (hereinafter, the floating seal ring arranged on the fixed housing side is also referred to as a "fixed side floating seal ring", and the floating seal ring arranged on the rotating side housing side is also referred to as a "rotating side floating seal ring"), and the floating seal ring of one of the pair of floating seal rings is the above-mentioned floating seal material, in particular, a floating seal ring.

[0110] Below, use Figure 1 The structure of a floating seal device will be described as an example thereof, but the floating seal device according to the present embodiment is not limited to this structure.

[0111] Figure 1 The floating seal device shown has a pair of fixed-side floating seal rings 2 and a rotating-side floating seal ring 7 , each of which is provided on the outer periphery of the shaft 20 in a state of not contacting the shaft 20 , that is, in a state of floating from the shaft 20 .

[0112] The stationary-side floating seal ring 2 is combined with the stationary housing 12 via an O-ring 18 , while the rotating-side floating seal ring 7 is combined with the rotating housing 15 via an O-ring 19 .

[0113] The stationary floating seal ring 2 has an annular structure with an inner diameter larger than the outer diameter of the shaft 20 and a groove 3 of a predetermined depth is provided on the outer peripheral surface. The bottom surface of the groove 3 is formed with a tapered surface 4 which gradually approaches the shaft 20 as it moves away from the rotating floating seal ring 7.

[0114] Similarly, the rotating side floating seal ring 7 also has an annular structure whose inner diameter is larger than the outer diameter of the shaft 20 , and a groove 8 of a predetermined depth is provided on the outer peripheral surface, and a tapered surface 9 is formed in the groove 8 .

[0115] The stationary floating seal ring 2 and the rotating floating seal ring 7 have sliding surfaces 5 and 10 on the outer circumferential sides of their respective facing surfaces, and the two floating seal rings face each other via the sliding surfaces 5 and 10 .

[0116] In addition, a tapered surface 6 which gradually moves away from the rotating floating sheet as it approaches the shaft 20 is formed on the inner peripheral portion of the surface of the stationary floating seal ring 2 facing the rotating floating seal ring 7 and continuous with the sliding surface 5 .

[0117] Similarly, a tapered surface 11 is formed on a portion of the inner circumference of the surface of the rotating-side floating seal ring 7 that faces the fixed-side floating seal ring 2 and that is continuous with the sliding surface 10 .

[0118] The stationary housing 12 is fixed to one end of the shaft 20, and its inner circumference surrounds the outer circumference of the stationary floating seal ring 2. A groove 13 of a predetermined depth is provided on the inner circumference of the stationary housing 12, and the groove 13 is formed with a tapered surface 14 inclined in the same direction as the bottom surface of the groove 3 on the outer circumference of the stationary floating seal ring 2.

[0119] The rotating housing 15 is rotatably provided at the other end of the shaft 20 via a bearing (not shown), and its inner peripheral surface surrounds the outer peripheral surface of the rotating side floating seal ring 7. A groove 16 of a predetermined depth is provided on the entire inner peripheral surface of the rotating housing 15, and the groove 16 is formed with a tapered surface 17 inclined in the same direction as the bottom surface of the groove 8 on the outer peripheral surface of the rotating side floating seal ring 7.

[0120] Furthermore, the fixed side floating seal ring 2 and the fixed housing 12, and the rotating side floating seal ring 7 and the rotating housing 15 are respectively combined via an O-ring 18 and an O-ring 19, and the O-rings 18 and 19 are made of a material having elastic force. Furthermore, by utilizing the elastic force of the O-rings 18 and 19, the fixed side floating seal ring 2 and the rotating side floating seal ring 7 are configured to be pressed via the sliding surface 5 and the sliding surface 10, and the two sliding surfaces 5 and 10 are sealed regardless of whether the rotating housing 15 is rotating or not rotating.

[0121] The floating seal device 1 including the fixed-side and rotating-side floating seal rings 2 and 7 described above can be suitably used as a seal for a track wheel of a construction machine or a vehicle, for example.

[0122] In the measurement of each characteristic in this specification, unless otherwise specified, the measurement sample is kept in the same environment as the measurement environment for more than 48 hours before the measurement. In addition, the measurement temperature, measurement humidity and measurement pressure are set to normal temperature (22±2°C), normal humidity (60±5%RH) and normal pressure (atmospheric pressure) unless otherwise specified.

[0123] Example

[0124] The present invention will be described in more detail below with reference to Examples. However, the present invention is not limited to the following Examples.

[0125] [Manufacture of floating seal materials]

[0126] First, raw materials were prepared to have the composition shown in Table 1, and these raw materials were heated (heated and melted) at a temperature of 1560°C to obtain molten metal. Thereafter, centrifugal casting was performed and cooling was performed at a cooling rate of 300 to 700°C / min to produce floating seal materials of Examples 1 to 7 and Comparative Examples 1 to 16. The components other than the components shown in Table 1 in the floating seal material are Fe and inevitable impurities (P and S, etc., any element is less than 0.1% by weight).

[0127] The [formability]

[0128] For each of the above floating seal materials, materials that could be formed into a sealing shape were evaluated as "A", and materials that could not be formed, or materials that could be formed but had cracks and were difficult to use as a sealing material were evaluated as "B".

[0129] [hardness]

[0130] The Rockwell hardness of each of the above floating seal materials was measured, and materials with a hardness of 65 HRC or higher, which is a desired hardness for floating seal materials, were evaluated as "A", and materials with a hardness of less than 65 HRC were evaluated as "B". The evaluation results are shown in Table 1.

[0131] [Sintering resistance]

[0132] For each of the above floating seal materials, prepare A fixed test piece with the same sealing size and shape, and a rotating test piece of the same shape, are produced. Figure 1 The floating seal device shown in the figure was used to evaluate the seizure resistance. The fixed test piece and the rotating test piece are equivalent to Figure 1 The fixed side floating seal ring and the rotating side floating seal ring.

[0133] The test atmosphere was lubricating oil on the inner circumference of the fixed test piece and the rotating test piece, and air on the outer circumference.

[0134] The rotating test pieces were rotated at a rotation speed of 1 to 5 m / s, and the test pieces without seizure (sudden increase in torque, rapid temperature rise) were evaluated as "A", and the test pieces with seizure were evaluated as "B". The evaluation results are shown in Table 1.

[0135] [Evaluation of Carbides]

[0136] The above-mentioned atomic emission spectrometry and structural observation (structural observation using a scanning electron microscope (SEM)) were performed using the floating seal materials of Examples 1 to 7. The results of structural observation using SEM are shown in FIG. Figure 4 as well as Figure 5 . Through these atomic emission spectrometry and structural observation, it was confirmed that granular carbides were formed. Specifically, it was confirmed that at least one carbide represented by the group consisting of M3C and M7C3 (M is Fe, Si, Mn, Cr or Mo) selected from at least a part of Fe, Si, Mn, Cr or Mo and at least a part of C was formed, and a carbide represented by M6C (M is Fe, Si, Cr or Mo) consisting of at least a part of Fe, Si, Cr or Mo and at least a part of C was formed. Furthermore, it was confirmed that there was a phase separation structure containing at least one dispersed phase in the matrix phase, and as a dispersed phase, it contained a granular phase composed of any one of M3C, M7C3, and M6C with an average particle size of less than 1 μm. Specifically, as shown in Table 2, the presence of three carbide phases and a matrix was confirmed. In Table 2, "fine phase" refers to a granular phase with an average particle size of less than 1 μm. In addition, according to the examples, there is also a case where phase 1 satisfies the condition of an average grain size of 1 μm or less. In addition, in Example 5, both phase 2 and phase 3 become M3C, which means that there are two M3Cs with different compositions. The inventors speculate that the absence of M7C3 in Example 5 is due to the small amount of Cr.

[0137] [Table 1]

[0138]

[0139]

[0140] [Table 2]

[0141] Phase 1 Phase 2 Phase 3 (fine phase) Matrix Example 1 <![CDATA[M6C]]> <![CDATA[M3C]]> <![CDATA[M7C3]]> Martensite Example 2 <![CDATA[M6C]]> <![CDATA[M7C3]]> <![CDATA[M7C3、M3C]]> Martensite Example 3 <![CDATA[M6C]]> <![CDATA[M3C]]> <![CDATA[M7C3]]> Martensite Example 4 <![CDATA[M6C]]> <![CDATA[M7C3]]> <![CDATA[M7C3、M3C]]> Martensite Example 5 <![CDATA[M6C]]> <![CDATA[M3C]]> <![CDATA[M3C]]> Martensite Example 6 <![CDATA[M6C]]> <![CDATA[M7C3]]> <![CDATA[M7C3、M3C]]> Martensite Example 7 <![CDATA[M6C]]> <![CDATA[M3C]]> <![CDATA[M7C3]]> Martensite

[0142] As can be seen from Table 1, the floating seal material corresponding to the present embodiment is excellent in all of the properties of moldability, hardness, and seizure resistance.

[0143] From Comparative Examples 4, 5, and 11, it is understood that when the C content is too small, the formability is poor, and when the C content is too large, the formability is poor.

[0144] As can be seen from Comparative Examples 6 and 7, when the Si content is too small, the formability is poor, and when it is too large, the formability, hardness, and seizure resistance are poor.

[0145] From Comparative Examples 8 and 9, it is understood that when the Mn content is too small, the formability, hardness, and seizure resistance are poor, and when the Mn content is too large, the formability and seizure resistance are poor.

[0146] As can be seen from Comparative Examples 1 and 2, if the Cr content is too small, the hardness and seizure resistance are poor, and if it is too large, the formability is poor.

[0147] As can be seen from Comparative Example 3, when the Mo content is too small, the formability, hardness, and seizure resistance are poor.

[0148] It can be seen from Comparative Examples 7 and 10 to 16 that, when the content of each component other than Fe, C, Si, Mn, Cr and Mo is less than 1 wt %, the formability, hardness and sintering resistance are excellent, but when it exceeds 1 wt %, at least one of these characteristics is poor.

[0149] (Explanation of Reference Numerals)

[0150] 1: floating seal device; 2: fixed side floating seal ring; 3, 8, 13, 16: groove;

[0151] 4, 6, 9, 11, 14, 17: conical surface; 5, 10: sliding surface; 7: floating seal ring on the rotating side;

[0152] 12: fixed housing; 15: rotating housing; 18, 19: O-rings; 20: shaft.

Claims

1. A floating sealing material, wherein: Contains at least Fe, C, Si, Mn, Cr and Mo, The C content is greater than 2.3 wt% and less than 3.8 wt%, the Si content is greater than 0.7 wt% and less than 2.5 wt%, the Mn content is greater than 0.3 wt% and less than 1.3 wt%, the Cr content is greater than 3 wt% and less than 13 wt%, the Mo content is greater than 1.8 wt% and less than 15 wt%, and the balance is Fe and unavoidable impurities.

2. The floating sealing material according to claim 1, wherein: Contains at least one of carbides represented by M3C and M7C3 (M is Fe, Si, Mn, Cr or Mo) composed of at least a part of the Fe, Si, Mn, Cr or Mo and at least a part of the C.

3. The floating sealing material according to claim 1 or 2, wherein: Contains a carbide represented by M6C (M is Fe, Si, Cr or Mo) composed of at least a part of the Fe, Si, Cr or Mo and at least a part of the C.

4. The floating sealing material according to claim 2 or 3, wherein: having a phase-separated structure containing at least one dispersed phase in a matrix phase, The dispersed phase includes a granular phase having an average particle size of 1 μm or less and composed of at least one of the carbides represented by M3C, M7C3, and M6C.

5. A floating seal device, wherein: The floating sealing material comprises the floating sealing material according to any one of claims 1 to 4.

6. A method for manufacturing a floating sealing material, wherein: include: a molten metal preparing step of preparing a molten metal, the molten metal containing at least Fe, C, Si, Mn, Cr and Mo, wherein a C content is 2.3 wt% to 3.8 wt% inclusive, a Si content is 0.7 wt% to 2.5 wt% inclusive, a Mn content is 0.3 wt% to 1.3 wt% inclusive, a Cr content is 3 wt% to 13 wt% inclusive, a Mo content is 1.8 wt% to 15 wt% inclusive, and the balance is Fe and unavoidable impurities; and A casting process of pouring the molten metal into a mold.

7. The method for manufacturing a floating sealing material according to claim 6, wherein: In the casting step, the molten metal is cast into the mold by centrifugal casting.

8. The method for manufacturing a floating sealing material according to claim 6 or 7, wherein: The method includes cooling the mold after the casting step to cool and solidify the molten metal.