Protective sheet for semiconductor processing and method for manufacturing semiconductor device
By using an intermediate layer without ethylenically unsaturated groups and an adhesive layer containing ethylenically unsaturated groups in the protective sheet for semiconductor processing, combined with photocuring technology, the existing protective sheet follows the concave and convex surface at high temperatures and The problem of insufficient peeling performance achieves efficient semiconductor processing protection.
Patent Information
- Application Number
- CN202380034007.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-15
- Filing Date
- 2023-07-21
- Publication Date
- 2024-11-26
AI Technical Summary
The existing protective sheet for semiconductor processing is insufficient in high temperature treatment, and the concave and convex surfaces of semiconductor chips or printed wiring boards with bumps cannot be correctly followed, and residual glue is easily generated when peeled off.
A protective sheet consisting of a base material, an intermediate layer and an adhesive layer is a resin composition containing a methacrylic resin without ethylenically unsaturated groups and a crosslinking agent, and the adhesive layer is an olefinic-containing The composition of an unsaturated methacrylic resin, a crosslinking agent and a photopolymerization initiator, forms a crosslinking structure through photocuring to improve heat resistance and peeling properties.
It is achieved to correctly follow the surface concave and convexity at high temperature without peeling off residual glue, which reduces the peel strength of the adhesive layer, and improves the heat resistance and peeling performance of the protective sheet.
Smart Images

Figure CN119032416A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a protective sheet for semiconductor processing and a method for manufacturing a semiconductor device. Background Art
[0002] Various protective sheets are used in the manufacturing process of semiconductors. Specifically, there are protective sheets (back grinding tapes) used to protect the semiconductor wafer during the back grinding (back grinding) step, and fixing sheets (dicing tapes) used in the step of cutting (slicing) the semiconductor wafer into component chips. These protective sheets are removable protective sheets that are attached to the semiconductor wafer as the adherend and are peeled off from the adherend after the specified processing steps are completed.
[0003] In recent years, as electronic equipment has become smaller and more dense, flip chip mounting has become the mainstream as a method that enables semiconductor components to be mounted in the smallest area. In flip chip mounting, in order to achieve inter-chip bonding, a semiconductor chip (e.g., Through Silicon Via (TSV) chip) with a protruding electrode (bump) at the top end formed by welding is used. The semiconductor chip with the bump is electrically bonded to other semiconductor chips or substrates through a reflow soldering step that is heated to a temperature above the melting temperature of the solder (usually above 200°C). However, when semiconductor chips are mounted on electronic equipment for communication, electromagnetic waves generated from the inside of the chip may sometimes cause communication problems. To prevent this, a sputtering step is sometimes performed to vapor-deposit (usually above 150°C) a metal film on the periphery of the semiconductor chip as an electromagnetic shielding cover. In the reflow soldering step and the sputtering step, a removable protective sheet is used to protect the surface of the bump.
[0004] For example, Patent Document 1 describes a method for producing an electronic device using an electronic component having a circuit-formed surface and an adhesive laminate film having a base layer, an unevenness-absorbing resin layer, and an adhesive resin layer in this order.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2021-163785 Summary of the invention
[0008] [Problems to be Solved by the Invention]
[0009] Semiconductor chips with bumps and printed wiring boards (PCBs) with bumps have large concave-convex shapes on their surfaces, so when the surface protection function is realized in the processing steps, the protection sheet is required to correctly follow the concave-convex shapes and adhere tightly. In addition, the protection sheet is required to have high heat resistance. When the heat resistance is insufficient, during high-temperature treatments such as reflow soldering steps and sputtering steps, exhaust gas is generated from the protection sheet and it floats from the adherend, or residual glue is generated on the adherend during peeling.
[0010] However, conventional protective sheets have not been able to fully satisfy the above conditions. For example, Patent Document 1 describes that insufficient heat resistance causes resin dissolution of the unevenness absorbent resin layer during the heating step, or that adhesive residue is generated on the semiconductor chip when the protective sheet is peeled off.
[0011] The present invention provides a protective sheet for semiconductor processing, which can accurately follow the surface unevenness of a semiconductor device having unevenness on a semiconductor chip with bumps or a PCB with bumps, and can be peeled off without residual adhesive after irradiation with active energy lines, even after undergoing various processing steps. In particular, a protective sheet for semiconductor processing is provided, which can accurately follow the surface unevenness and adhere even when the step difference (bump height) of the unevenness on the surface of the adherend is large and after undergoing high-temperature treatment such as 200°C, and can be peeled off without residual adhesive after irradiation with active energy lines. A method for manufacturing a semiconductor device using a protective sheet for semiconductor processing is further provided.
[0012] [Methods to solve the problem]
[0013] The content of the present invention includes the following aspects.
[0014] [1] A protective sheet for semiconductor processing, comprising a substrate, and an intermediate layer and an adhesive layer in this order on one main surface of the substrate,
[0015] The intermediate layer is a cured product of a resin composition containing a (meth) acrylic resin (A1) having no ethylenically unsaturated group and a crosslinking agent (B1).
[0016] The adhesive layer is a cured product of an adhesive composition containing a (meth)acrylic resin (A2) having an ethylenically unsaturated group, a crosslinking agent (B2) and a photopolymerization initiator (C).
[0017] The (meth)acrylic resin (A1) having no ethylenically unsaturated group has a plurality of functional groups that react with the functional groups of the crosslinking agent (B1).
[0018] The (meth)acrylic resin (A2) having an ethylenically unsaturated group has a plurality of functional groups that react with the functional groups of the crosslinking agent (B2).
[0019] The (meth) acrylic resin (A2) having an ethylenically unsaturated group is an addition product of an ethylenically unsaturated compound (a2-3) having an epoxy group to a copolymer of a monomer group (M2) containing a (meth) acrylic acid alkyl ester (a2-1) and an ethylenically unsaturated compound (a2-2) having a carboxyl group, and is a protective sheet for semiconductor processing.
[0020] [2] A protective sheet for semiconductor processing as described in [1], wherein the thickness of the intermediate layer is 30 to 600 μm, the thickness of the adhesive layer is 5 to 100 μm, and the ratio of the thickness of the intermediate layer to the adhesive layer (intermediate layer / adhesive layer) is 1 to 50.
[0021] [3] The protective sheet for semiconductor processing as described in [1] or [2], wherein the glass transition temperature (Tg) of the (meth)acrylic resin (A1) having no ethylenically unsaturated group is -80 to 0°C.
[0022] [4] A protective sheet for semiconductor processing as described in any one of [1] to [3], wherein the (meth)acrylic resin (A1) having no ethylenically unsaturated group is a copolymer of a monomer group (M1) containing an alkyl (meth)acrylate (a1-1) and a (meth)acrylate having a hydroxyl group (a1-2), and the crosslinking agent (B1) is an isocyanate crosslinking agent.
[0023] [5] The protective sheet for semiconductor processing as described in [4], wherein the monomer group (M1) further contains an ethylenically unsaturated compound (a1-3) having a carboxyl group.
[0024] [6] The protective sheet for semiconductor processing according to [4] or [5], wherein the monomer group (M1) further contains a (meth)acrylamide compound.
[0025] [7] The protective sheet for semiconductor processing as described in any one of [1] to [6], wherein the glass transition temperature (Tg) of the (meth)acrylic resin (A2) having an ethylenically unsaturated group is -80 to 0°C.
[0026] [8] The protective sheet for semiconductor processing as described in any one of [1] to [7], wherein the (meth)acrylic resin (A2) having an ethylenically unsaturated group has an ethylenically unsaturated group equivalent of 100 to 4000 g / mol.
[0027] [9]. The protective sheet for semiconductor processing as described in any one of [1] to [8], wherein the crosslinking agent (B2) is an epoxy crosslinking agent.
[0028]
[10] A method for manufacturing a semiconductor device having a bump electrode, comprising the steps of attaching the adhesive layer of the semiconductor processing protective sheet as described in any one of [1] to [9] to the surface of the semiconductor device having the bump electrode,
[0029] The semiconductor processing protective sheet is irradiated with active energy rays to photo-cure the adhesive layer;
[0030] A step of heating the semiconductor device to which the protective sheet for semiconductor processing is bonded, and a step of peeling the protective sheet for semiconductor processing from the surface with the bump electrodes.
[0031]
[11] . In the method for manufacturing a semiconductor device as described in
[10] , when the height of the bump electrode is H [μm] and the total thickness of the intermediate layer and the adhesive layer is d [μm], d / H is 0.40 to 110.
[0032]
[12] . The method for manufacturing a semiconductor device as described in
[10] or
[11] , wherein the maximum reaching temperature of the heating step is 100 to 230°C.
[0033] [Effects of the invention]
[0034] The present invention can provide a semiconductor processing protective sheet that can accurately follow the surface unevenness and adhere even when the unevenness (bump height) of the adherend surface is large and after a high temperature treatment step such as 200°C, and can be peeled off without residual adhesive after active energy ray irradiation. Further, a method for manufacturing a semiconductor device using the semiconductor processing protective sheet can be provided.
[0035] According to the present invention, the adhesive force of the adhesive layer of the semiconductor processing protective sheet can be reduced by irradiation with active energy rays. Specifically, the adhesive layer has sufficient adhesive force to the adherend before irradiation with active energy rays, and after irradiation with active energy rays, the unsaturated bonds in the resin form a three-dimensional cross-linked structure and solidify, thereby reducing the adhesive force and showing excellent peelability, and can fully prevent residual adhesive on the adherend after peeling. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic cross-sectional view showing a protective sheet for semiconductor processing in one embodiment. DETAILED DESCRIPTION
[0037] The embodiments of the present invention are described in detail below, but the present invention is not limited to the embodiments described below.
[0038] In the present specification, when "to" is used in a numerical range, the numerical values at both ends are the upper limit and the lower limit, respectively, and are included in the numerical range.
[0039] In the present invention, (meth)acrylic acid means "acrylic acid" or "methacrylic acid", (meth)acrylate means "acrylate" or "methacrylate", and (meth)acryloyloxy means "acryloyloxy" or "methacryloyloxy".
[0040] In the present invention, the “weight average molecular weight (Mw)” is a value determined by measuring at room temperature (23° C.) under the following conditions using gel permeation chromatography (GPC: gel permeation chromatography) and using a standard polystyrene calibration curve.
[0041] Device: Shodex (trademark) GPC-101 (Showa Denko K.K.)
[0042] Column: Shodex (trademark) LF-804 (Showa Denko K.K.)
[0043] Column temperature: 40℃
[0044] Sample: 0.2 mass% tetrahydrofuran solution of the sample
[0045] Flow rate: 1mL / min
[0046] Dissolution liquid: Tetrahydrofuran
[0047] Detector: RI detector
[0048] In the present invention, the glass transition temperature (Tg) of the (meth)acrylic resin refers to a value obtained by converting the glass transition temperature Tga at an absolute temperature obtained using the FOX formula (Fox, TG, Bull. Am. Phys. Soc., 1 (1956), p. 123) of the following formula (1) into Celsius degrees.
[0049] 1 / Tga=∑i(Wi / Tgi) …(1)
[0050] (In formula (1), Tga is the glass transition temperature (in absolute temperature) of the (meth)acrylic resin. Wi is the mass ratio of each monomer i in the (meth)acrylic resin. Tgi is the glass transition temperature (in absolute temperature) of a homopolymer formed only from each monomer i.)
[0051] In the present invention, the "acid value (mgKOH / g)" is a value measured in accordance with JIS K 0070:1992.
[0052] In the present invention, the "hydroxyl value (mgKOH / g)" is a value measured in accordance with JIS K 0070:1992.
[0053] In the present invention, the "ethylenically unsaturated group equivalent (g / mol)" is a value calculated from the iodine value measured in accordance with JIS K 0070:1992.
[0054] <Protective sheet for semiconductor processing>
[0055] A semiconductor processing protective sheet of one embodiment comprises a substrate, an intermediate layer and an adhesive layer sequentially arranged on one main surface of the substrate. The semiconductor processing protective sheet has an intermediate layer having an appropriate hardness and an adhesive layer that can be photocured, so that even when the step difference (bump height) of the concave and convex surface of the adherend is large and when a high temperature treatment step such as 200°C is performed, it can accurately follow the concave and convex surface and adhere tightly, and can be peeled off without residual adhesive after irradiation with active energy rays. Figure 1 FIG. 1 is a schematic cross-sectional view of a semiconductor processing protective sheet in one embodiment. The semiconductor processing protective sheet 10 comprises a substrate 12, a main surface (on the Figure 1 The semiconductor processing protective sheet 10 further comprises a release sheet (spacer) 18 disposed on the adhesive layer 16 as required. The release sheet is attached to the outer side of the adhesive layer for the purpose of protecting the surface of the adhesive layer (the surface attached to the adherend) before being used as the semiconductor processing protective sheet. The semiconductor processing protective sheet can be used, for example, as a back grinding tape and a dicing tape.
[0056] The semiconductor processing protective sheet can be used as a semiconductor processing protective sheet formed into a shape corresponding to the shape of the adherend by punching, etc. The semiconductor processing protective sheet can be used as a semiconductor processing protective sheet in a cylindrical shape by winding and cutting.
[0057] The thickness of the protective sheet for semiconductor processing depends on the uneven step difference (bump height) of the adherend surface, preferably 60 μm to 1600 μm, preferably 100 μm to 650 μm, and more preferably 120 μm to 550 μm. From the perspective of being able to more accurately follow the unevenness of the adherend surface and ensure the processing accuracy of the adherend in the processing step, it is preferred to set the thickness of the protective sheet for semiconductor processing to 1.5 to 3 times the uneven step difference of the adherend surface.
[0058] The peel strength of the protective sheet for semiconductor processing depends on the thickness of the protective sheet for semiconductor processing, the type of adherend, and the type and order of processing steps. For example, the peel strength before active energy ray irradiation is preferably 2.0 to 25 N / 25 mm, more preferably 3.0 to 20 N / 25 mm, and more preferably 5.0 to 15 N / 25 mm. If the peel strength before active energy ray irradiation is 2.0 N / 25 mm or more, the adhesion to the adherend before active energy ray irradiation is good. If the peel strength before active energy ray irradiation is 25 N / 25 mm or less, the peel strength during peeling can be sufficiently reduced, thereby reducing the residual glue on the adherend.
[0059] The semiconductor processing protective sheet of one embodiment can reduce the peel strength by irradiation with active energy rays, making it possible to easily peel off without residual adhesive from the adherend in the peeling step. The peel strength of the semiconductor processing protective sheet after irradiation with active energy rays depends on the thickness of the semiconductor processing protective sheet and the type of the adherend, as well as the type and order of the processing steps, for example, 0.001 to 1.0 N / 25 mm is preferred, 0.005 to 0.75 N / 25 mm is more preferred, and 0.01 to 0.5 N / 25 mm is more preferred.
[0060] The peel strength in the present invention refers to the peel strength (N / 25mm) of the semiconductor processing protective sheet to the adherend measured in a 180° extension test at a peeling speed of 300mm / min under an environment of 23°C and 50% humidity according to JIS Z 0237:2009.
[0061] [Base material]
[0062] As the substrate, a known sheet material can be appropriately selected. As the substrate, it is preferable to use a resin sheet produced using a transparent resin material.
[0063] As resin materials, polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), etc., polyetheretherketone (PEEK), polyamide (PA), polyimide (PI), polyphenylene sulfide (PPS), and polytetrafluoroethylene (PTFE) can be listed. Among these resin materials, in order to obtain a sheet with moderate flexibility and heat resistance, it is preferred to use PET, PEN, PEEK, PA, or PI, and it is further preferred to use PEN, PET, or PA, and PA is more preferred. When using these, the resin sheet is difficult to be damaged even when it is provided to a high temperature process such as a reflow step and a sputtering step. The resin material can be used alone or in combination of two or more.
[0064] When a resin sheet is used as a substrate, the resin sheet may be a single layer or a multilayer structure of two or more layers (eg, a three-layer structure). For a resin sheet having a multilayer structure, the resin materials constituting each layer may be one or more.
[0065] The thickness of the substrate can be appropriately selected according to the type of semiconductor processing, the material of the substrate, etc. The protective sheet for semiconductor processing is a sheet that protects a semiconductor chip with bumps or a flexible wiring circuit substrate (FPC) with bumps during a reflow soldering step or a sputtering process. When the substrate is a resin sheet, the thickness of the substrate is preferably 5 to 1000 μm, and more preferably 10 to 300 μm, more preferably 20 to 100 μm, and more preferably 25 to 50 μm. If the thickness of the substrate is 5 μm or more, the rigidity of the protective sheet for semiconductor processing is high (strong rigidity). Therefore, when the protective sheet for semiconductor processing is attached to an adherend such as a semiconductor chip, or when it is peeled off from an adherend, there is a tendency that wrinkles and floating are difficult to form on the protective sheet for semiconductor processing. In addition, if the thickness of the substrate is 5 μm or more, it is easy to peel off the protective sheet for semiconductor processing attached to the adherend from the adherend, and the workability (operability, handling) is good. When the thickness of the substrate is 1000 μm or less, the rigidity of the protective sheet for semiconductor processing will be appropriate and the workability will be good.
[0066] The thickness of the substrate is preferably 5 μm or more, more preferably 10 μm or more, more preferably 20 μm or more, and more preferably 25 μm or more, from the perspective of the ease of peeling off the semiconductor processing protective sheet attached to the adherend from the adherend. From the perspective of the rigidity of the semiconductor processing protective sheet, it is preferably 1000 μm or less, more preferably 300 μm or less, more preferably 100 μm or less, and more preferably 50 μm or less. The combination of these lower limits and upper limits may also be any combination.
[0067] When a resin sheet is used as the substrate, the substrate can be produced by using the above-mentioned resin material and appropriately adopting a conventionally known general sheet molding method (for example, extrusion molding, T-die molding, inflation molding, uniaxial or biaxial stretching molding, etc.).
[0068] The surface in contact with the substrate intermediate layer may be subjected to a surface treatment to improve adhesion between the substrate and the intermediate layer. Examples of the surface treatment include corona discharge treatment, acid treatment, ultraviolet irradiation treatment, plasma treatment, and primer coating.
[0069] [Middle layer]
[0070] The intermediate layer is a cured product of a resin composition containing a (meth) acrylic resin (A1) without an ethylenically unsaturated group and a crosslinking agent (B1). The cured product is a reaction product (crosslinked body) of a functional group possessed by the (meth) acrylic resin (A1) without an ethylenically unsaturated group and capable of reacting with a functional group possessed by the crosslinking agent (B1) and a functional group possessed by the crosslinking agent (B1). Since the protective sheet for semiconductor processing has an intermediate layer, it has good step tracking properties even when the step difference (bump height) on the surface of the adherend becomes larger.
[0071] The thickness of the intermediate layer is preferably 30 to 600 μm, more preferably 50 to 500 μm, more preferably 80 to 300 μm, and even more preferably 100 to 200 μm. When the thickness of the intermediate layer is 30 μm or more, the semiconductor processing protective sheet has good followability to the step difference on the surface of the adherend. When the thickness of the intermediate layer is 600 μm or less, the processing accuracy in the processing step of the adherend is good.
[0072] The thickness of the intermediate layer is preferably 30 μm or more, preferably 50 μm or more, more preferably 80 μm or more, and more preferably 100 μm or more, from the viewpoint of the followability of the step difference of the semiconductor processing protective sheet to the surface of the adherend. From the viewpoint of the processing accuracy in the processing step of the adherend, it is preferably 600 μm or less, preferably 500 μm or less, more preferably 300 μm or less, and more preferably 200 μm or less. The combination of these lower limits and upper limits can be any combination.
[0073] ((Meth)acrylic resin (A1) not having an ethylenically unsaturated group)
[0074] The (meth) acrylic resin (A1) without ethylenically unsaturated groups is a (meth) acrylic resin having an ethylenically unsaturated group equivalent weight exceeding 4000 g / mol or having no ethylenically unsaturated groups, and having multiple functional groups reactive to the functional groups possessed by the crosslinking agent (B1), and is not particularly limited. In one embodiment, the (meth) acrylic resin (A1) without ethylenically unsaturated groups does not have ethylenically unsaturated groups. As functional groups reactive to the functional groups possessed by the crosslinking agent (B1), for example, hydroxyl, carboxyl, isocyanate, glycidyl, amino and amido groups can be listed. The (meth) acrylic resin (A1) without ethylenically unsaturated groups can be used alone or in combination of two or more. By using a (meth) acrylic resin (A1) without an ethylenically unsaturated group to form an intermediate layer, the semiconductor processing protective sheet has high heat resistance and has high followability to the unevenness of the adherend from the step of laminating to the processing step and the peeling step, even when exposed to high temperature conditions. In addition, even when the step difference (bump height) on the surface of the adherend becomes large, it also has good step difference followability.
[0075] The glass transition temperature (Tg) of the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably -80°C or higher, more preferably -70°C or higher, and more preferably -60°C or higher. The glass transition temperature (Tg) of the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably 0°C or lower, more preferably -10°C or lower, and more preferably -20°C or lower. Any combination of these lower limits and upper limits may be used. The glass transition temperature (Tg) of the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably -80°C to 0°C, more preferably -70°C to -10°C, and more preferably -60°C to -20°C. When the glass transition temperature is -80°C or higher, an intermediate layer with high cohesive force can be obtained, so that the resin can be prevented from eluting during sheet molding. When the glass transition temperature is 0° C. or lower, the adhesion between the intermediate layer and the adhesive layer can be further improved.
[0076] The weight average molecular weight of the (meth)acrylic resin (A1) having no ethylenically unsaturated group is preferably 100,000 to 2,000,000, more preferably 150,000 to 1,500,000, and more preferably 200,000 to 1,000,000. When the weight average molecular weight is 100,000 or more, an intermediate layer with high cohesive force can be obtained, and resin elution can be prevented during sheet molding. When the weight average molecular weight is 2,000,000 or less, molding and processing become easy.
[0077] As described later, as the crosslinking agent (B1), for example, a crosslinking agent such as an isocyanate crosslinking agent and an epoxy crosslinking agent can be used.
[0078] In the embodiment where the crosslinking agent (B1) is an isocyanate crosslinking agent, the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably a copolymer of a monomer group (M1) containing an alkyl (meth)acrylate (a1-1) and a (meth)acrylate having a hydroxyl group (a1-2). The monomer group (M1) may further contain at least one selected from an ethylenically unsaturated compound (a1-3) having a carboxyl group and other monomers (a1-4) as needed.
[0079] In this embodiment, the hydroxyl value of the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably 0.5 to 100 mgKOH / g, more preferably 1 to 50 mgKOH / g, and more preferably 5 to 30 mgKOH / g. When the hydroxyl value is 0.5 mgKOH / g or more, it can fully react with the isocyanate crosslinking agent to obtain an intermediate layer with high cohesive force. When the hydroxyl value is 100 mgKOH / g or less, the obtained resin can be dissolved in widely used organic solvents such as ethyl acetate or toluene, so the workability is good.
[0080] In this embodiment, the content of the (meth)acrylic acid alkyl ester (a1-1) in the monomer group (M1) constituting the (meth)acrylic resin (A1) having no ethylenically unsaturated group is preferably 50 to 95 mol%, more preferably 60 to 90 mol%, and more preferably 70 to 90 mol%. When the content of the (meth)acrylic acid alkyl ester (a1-1) is 50 mol% or more, the adhesion to the substrate of the intermediate layer and the adhesive layer is good. When the content of the (meth)acrylic acid alkyl ester (a1-1) is 95 mol% or less, since the content of the (meth)acrylic acid ester (a1-2) having a hydroxyl group can be sufficiently ensured, the crosslinking amount with the crosslinking agent (B1) is sufficiently ensured, and the cohesive force of the intermediate layer is improved.
[0081] In this embodiment, the content of the (meth)acrylate (a1-2) having a hydroxyl group in the monomer group (M1) constituting the (meth)acrylic resin (A1) having no ethylenically unsaturated group is preferably 0.5 to 30 mol%, more preferably 1.0 to 20 mol%, and more preferably 1.5 to 10 mol%. When the content of the (meth)acrylate (a1-2) having a hydroxyl group is 0.5 mol% or more, the amount of crosslinking with the crosslinking agent (B1) can be sufficiently ensured to improve the cohesive force of the intermediate layer. When the content of the (meth)acrylate (a1-2) having a hydroxyl group is 30 mol% or less, the obtained resin can be dissolved in widely used organic solvents such as ethyl acetate or toluene, so the operability is good.
[0082] In this embodiment, when the monomer group (M1) constituting the (meth) acrylic resin (A1) having no ethylenically unsaturated group contains an ethylenically unsaturated compound (a1-3) having a carboxyl group, the content is preferably 0.01 to 10 mol%, more preferably 0.05 to 5 mol%, and more preferably 0.1 to 3 mol%. When the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group is 0.01 mol% or more, the cohesive force of the intermediate layer is good. When the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group is 10 mol% or less, the cohesive force of the obtained resin does not become too high, so the operability is good.
[0083] In this embodiment, when the monomer group (M1) constituting the (meth)acrylic resin (A1) having no ethylenically unsaturated group contains other monomers (a1-4), the content is preferably 0.5 to 30 mol %, more preferably 1.0 to 25 mol %, and more preferably 5 to 15 mol %.
[0084] The (meth)acrylic acid alkyl ester (a1-1) is a compound having no functional groups such as hydroxyl group and carboxyl group but having an alkyl group and a (meth)acryloyloxy group, and is not particularly limited. Specifically, examples thereof include linear or branched alkyl (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, n-hexyl (meth)acrylate, isooctyl (meth)acrylate, and lauryl (meth)acrylate; and (meth)acrylic acid esters containing cyclic alkyl groups such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentyloxyethyl (meth)acrylate. Among these, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and isooctyl (meth)acrylate are also preferred. From the viewpoint of ease of synthesis, it is preferred to use a linear or branched alkyl (meth)acrylate having an alkyl group with 1 to 20 carbon atoms, and it is further preferred to use a linear or branched alkyl (meth)acrylate having an alkyl group with 1 to 12 carbon atoms. From the viewpoint of heat resistance, a (meth)acrylate containing a cyclic alkyl group having 3 to 30 carbon atoms is preferred. The alkyl (meth)acrylate (a1-1) may be used alone or in combination of two or more.
[0085] As the (meth)acrylate (a1-2) having a hydroxyl group, it is a compound having a hydroxyl group and a (meth)acryloyloxy group, and there is no particular limitation. Specifically, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,3-butanediol (meth)acrylate, 1,4-butanediol (meth)acrylate, 1,6-hexanediol (meth)acrylate and 3-methylpentanediol (meth)acrylate can be listed. The (meth)acrylate (a1-2) having a hydroxyl group can be used alone or in combination of two or more.
[0086] As the ethylenically unsaturated compound (a1-3) having a carboxyl group, it is a compound that does not have a hydroxyl group but has a carboxyl group and a (meth) acryloyloxy group, and there is no particular limitation. When the monomer group (M1) constituting the (meth) acrylic resin (A1) without an ethylenically unsaturated group contains an ethylenically unsaturated compound (a1-3) having a carboxyl group, when the intermediate layer is formed, the carboxyl group from the ethylenically unsaturated compound (a1-3) having a carboxyl group will be cross-linked with the hydroxyl group from the (meth) acrylate (a1-2) having a hydroxyl group, etc. to improve the cohesive force. In addition, when the adhesive layer also has a carboxyl group, the interlayer adhesion of the adhesive layer and the intermediate layer can also be improved. Further, when the crosslinking agent (B2) of the adhesive layer is an epoxy crosslinking agent, at the interface between the adhesive layer and the intermediate layer, the carboxyl group from the ethylenically unsaturated compound (a1-3) having a carboxyl group is crosslinked by the epoxy crosslinking agent of the adhesive layer, and then a stronger interlayer adhesion can be obtained, so it is further preferred.
[0087] Specific examples of the ethylenically unsaturated compound (a1-3) having a carboxyl group include (meth)acrylic acid, carboxymethyl (meth)acrylate, and β-carboxyethyl (meth)acrylate. The ethylenically unsaturated compound (a1-3) having a carboxyl group may be used alone or in combination of two or more.
[0088] As other monomers (a1-4), it is a compound having an ethylenically unsaturated group that can be copolymerized with these other than (a1-1) to (a1-3), and there is no particular limitation. For example, alkoxyalkyl (meth)acrylates, alkoxy (poly)alkylene glycol (meth)acrylates, (meth)acrylates containing aromatic groups, fluorinated (meth)acrylates, dialkylamino (meth)acrylates, and (meth)acrylamide compounds can be listed. Other monomers (a1-4) can be used alone or in combination of two or more.
[0089] As an alkoxyalkyl (meth)acrylate, ethoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, and butoxyethyl (meth)acrylate are mentioned, for example.
[0090] Examples of the alkoxy(poly)alkylene glycol (meth)acrylate include methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, 2-methoxyethoxyethyl (meth)acrylate, and methoxydipropylene glycol (meth)acrylate.
[0091] Examples of the (meth)acrylate containing an aromatic group include benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, 3-phenoxyphenyl acrylate, 4-phenoxyphenyl acrylate, 2-biphenylyl acrylate, 4-biphenylyl acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypropyl (meth)acrylate, and phenoxypolypropylene glycol (meth)acrylate.
[0092] As a fluorinated alkyl (meth)acrylate, octafluoropentyl (meth)acrylate is mentioned, for example.
[0093] Examples of the dialkylamino(meth)acrylate alkyl ester include N,N-dimethylaminoethyl(meth)acrylate and N,N-diethylaminoethyl(meth)acrylate.
[0094] Examples of the (meth)acrylamide compound include (meth)acrylamide; N-alkyl (meth)acrylamide such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-isopropyl acrylamide, and N-hexyl (meth)acrylamide; N,N-dialkyl (meth)acrylamide such as N,N-dimethyl (meth)acrylamide and N,N-diethyl (meth)acrylamide; (meth)acryloyl morpholine and diacetone acrylamide.
[0095] Other specific examples of other monomers (a1-4) include acrylonitrile, methacrylonitrile, styrene, α-methylstyrene, vinyl acetate, vinyl propionate, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyltoluene, N-vinylpyridine, N-vinylpyrrolidone, dialkyl itaconate, dialkyl fumarate, allyl alcohol, hydroxybutyl vinyl ether, hydroxyethyl vinyl ether, 4-hydroxymethylcyclohexyl methyl vinyl ether, triethylene glycol monovinyl ether, diethylene glycol monovinyl ether, methyl vinyl ketone, allyltrimethylammonium chloride and dimethylallyl vinyl ketone.
[0096] Among them, from the viewpoint of improving the adhesion to the adherend, a (meth)acrylamide compound is preferred, N,N-dialkyl (meth)acrylamide is more preferred, and N,N-dimethyl (meth)acrylamide is more preferred.
[0097] In the embodiment where the crosslinking agent (B1) is an epoxy crosslinking agent, the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably a copolymer of a monomer group (M1) containing an alkyl (meth)acrylate (a1-1) and an ethylenically unsaturated compound (a1-3) having a carboxyl group. The monomer group (M1) may further contain at least one selected from a (meth)acrylate (a1-2) having a hydroxyl group and other monomers (a1-4) as required.
[0098] In this embodiment, the same ones as those described above can be used as (a1-1) to (a1-4).
[0099] In this embodiment, the content of the (meth)acrylic acid alkyl ester (a1-1) in the monomer group (M1) constituting the (meth)acrylic resin (A1) having no ethylenically unsaturated group is preferably 50 to 99.0 mol%, more preferably 60 to 99.0 mol%, and more preferably 70 to 99.0 mol%. When the content of the (meth)acrylic acid alkyl ester (a1-1) is 50 mol% or more, the adhesion to the substrate and the adhesive layer of the intermediate layer is good. When the content of the (meth)acrylic acid alkyl ester (a1-1) is 99.0 mol% or less, the content of the (meth)acrylic acid ester (a1-2) having a hydroxyl group or the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group can be sufficiently ensured, so the crosslinking amount with the crosslinking agent (B1) can be sufficiently ensured, so the cohesion of the intermediate layer is improved.
[0100] In this embodiment, the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group in the monomer group (M1) constituting the (meth) acrylic resin (A1) having no ethylenically unsaturated group is preferably 0.1 to 30 mol%, more preferably 0.1 to 20 mol%, and more preferably 0.1 to 10 mol%. When the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group is 0.1 mol% or more, the cohesive force of the intermediate layer is good. When the content of the ethylenically unsaturated compound (a1-3) having a carboxyl group is 30 mol% or less, the cohesive force of the resulting resin will not become too high, and the operability is good.
[0101] In this embodiment, when the monomer group (M1) constituting the (meth) acrylic resin (A1) having no ethylenically unsaturated group contains a (meth) acrylic acid ester (a1-2) having a hydroxyl group, the content is preferably 0.1 to 30 mol%, more preferably 0.1 to 20 mol%, and more preferably 0.1 to 10 mol%. When the content of the (meth) acrylic acid ester (a1-2) having a hydroxyl group is 0.1 mol% or more, the amount of crosslinking with the crosslinking agent (B1) can be fully ensured. When the content of the (meth) acrylic acid ester (a1-2) having a hydroxyl group is 30 mol% or less, the resulting resin can be dissolved in widely used organic solvents such as ethyl acetate or toluene, so the operability is good.
[0102] In this embodiment, the content of the other monomer (a1-4) in the monomer group (M1) constituting the (meth)acrylic resin (A1) having no ethylenically unsaturated group is preferably 0 to 45 mol %, more preferably 0 to 35 mol %, and more preferably 0.1 to 25 mol %.
[0103] (Crosslinking agent (B1))
[0104] As a crosslinking agent (B1), a compound having a plurality of functional groups that can react with any one of the plurality of functional groups possessed by the (meth) acrylic resin (A1) without ethylenically unsaturated groups can be obtained, and there is no particular limitation, and the functional groups possessed by the (meth) acrylic resin (A1) without ethylenically unsaturated groups can be combined and selected. For example, when the (meth) acrylic resin (A1) without ethylenically unsaturated groups has a hydroxyl group, it is preferred to use an isocyanate crosslinking agent or an epoxy crosslinking agent as a crosslinking agent (B1), and it is further preferred to use an isocyanate crosslinking agent. When the (meth) acrylic resin (A1) without ethylenically unsaturated groups has a carboxyl group, it is preferred to use an isocyanate crosslinking agent, an epoxy crosslinking agent or an aziridine crosslinking agent as a crosslinking agent (B1), and it is further preferred to use an epoxy crosslinking agent. Because the intermediate layer contains a crosslinking agent (B1), the cohesive force of the intermediate layer can be improved, and the residual glue when the semiconductor processing protective sheet is peeled off from the adherend can be reduced. The cross-linking agent (B1) may be used alone or in combination of two or more.
[0105] Further preferred combinations of the (meth)acrylic resin (A1) not having an ethylenically unsaturated group and the crosslinking agent (B1) include a combination of the (meth)acrylic resin (A1) not having an ethylenically unsaturated group having a hydroxyl group and an isocyanate crosslinking agent, a combination of the (meth)acrylic resin (A1) not having an ethylenically unsaturated group having a carboxyl group and an epoxy crosslinking agent, and a combination of the (meth)acrylic resin (A1) not having an ethylenically unsaturated group having a carboxyl group and an aziridine crosslinking agent. Further preferred is a combination of the (meth)acrylic resin (A1) not having an ethylenically unsaturated group having a hydroxyl group and an isocyanate crosslinking agent.
[0106] Isocyanate crosslinking agents are compounds having two or more isocyanate groups. Examples thereof include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hydrogenated toluene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, isocyanurate of hexamethylene diisocyanate, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, toluene diisocyanate adduct of trimethylolpropane, xylylene diisocyanate adduct of trimethylolpropane, triphenylmethane triisocyanate, methylenebis(4-phenylmethane) triisocyanate, etc. Among them, isocyanurate of hexamethylene diisocyanate and toluene diisocyanate adduct of trimethylolpropane are also preferred. The isocyanate cross-linking agent may be used alone or in combination of two or more.
[0107] Epoxy crosslinking agents are compounds having two or more epoxy groups. Examples thereof include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, bisphenol A·epichlorohydrin type epoxy resins, N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine], ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, and both-end epoxy-modified polydimethylsiloxane. Epoxy crosslinking agents may be used alone or in combination of two or more.
[0108] The aziridine crosslinking agent is a compound having two or more aziridine groups. Examples thereof include ethylene glycol-bis-[3-(2-aziridine) propionate], trimethylolpropane-tris[3-(2-aziridine) propionate], trimethylolpropane-tris[3-(1-aziridine) propionate], trimethylolpropane-tris[3-(2-methyl-1-aziridine) propionate], tetramethylolmethane-tris[3-(2-aziridine) propionate], pentaerythritol-tris[3-( [1-aziridine) propionate], N,N'-diphenylmethane-4,4'-bis(1-aziridine carboxylic acid amide), N,N'-hexamethylene-1,6-bis(1-aziridine carboxylic acid amide), tris-2,4,6-(1-aziridine)-1,3,5-triazine, tris(1-aziridine)phosphine oxide, 2,2-bis(hydroxymethyl)butanol-tris[3-(1-aziridine) propionate], etc. The aziridine crosslinking agent may be used alone or in combination of two or more.
[0109] The content of the crosslinking agent (B1) is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, and more preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the (meth) acrylic resin (A1) having no ethylenically unsaturated group. When the content of the crosslinking agent (B1) is 0.05 parts by mass or more, a three-dimensional crosslinked structure is fully formed in the middle layer, resulting in an intermediate layer with high heat resistance. When the content of the crosslinking agent (B1) is 30 parts by mass or less, a moderate gelation time during sheet molding can be ensured.
[0110] (Other ingredients)
[0111] The resin composition may contain other components other than the (meth)acrylic resin (A1) and the crosslinking agent (B1) as necessary. Examples of other components include tackifiers, solvents, and various additives.
[0112] Adhesive
[0113] As the adhesion imparting agent, any known adhesive may be used without particular limitation. As the adhesion imparting agent, for example, terpene-based resins imparting adhesion, phenol-based resins imparting adhesion, rosin-based resins imparting adhesion, aliphatic petroleum resins, aromatic petroleum resins, copolymerized petroleum resins, alicyclic petroleum resins, xylene resins, epoxy-based resins imparting adhesion, polyamide-based resins imparting adhesion, ketone-based resins imparting adhesion, and elastic-based resins imparting adhesion may be cited. The adhesion imparting agent may be used alone or in combination of two or more.
[0114] When the resin composition contains the tackifier, the content is preferably 30 parts by mass or less, more preferably 5 to 20 parts by mass, based on 100 parts by mass of the (meth)acrylic resin (A1) having no ethylenically unsaturated group.
[0115] Solvents
[0116] The solvent is used to dilute the resin composition for the purpose of adjusting the viscosity of the resin composition. For example, when applying the resin composition, the viscosity of the resin composition can be adjusted to an appropriate viscosity using the solvent. The solvent is removed when the intermediate layer is formed.
[0117] As the solvent, for example, organic solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, propyl acetate, tetrahydrofuran, dioxane, cyclohexanone, hexane, toluene, xylene, n-propanol, and isopropanol can be used. The solvent may be used alone or in combination of two or more.
[0118] "additive"
[0119] Examples of the additives include plasticizers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, benzotriazole-based light stabilizers, phosphate-based and other flame retardants, surfactants, and antistatic agents.
[0120] [Method for producing (meth)acrylic resin (A1) not having ethylenically unsaturated group]
[0121] The method for producing the (meth) acrylic resin (A1) without ethylenically unsaturated groups is not particularly limited. For example, the monomer group (M1) can be copolymerized by a known polymerization method to obtain the (meth) acrylic resin (A1) without ethylenically unsaturated groups. Specifically, as the polymerization method, solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, alternating copolymerization, etc. can be used. Among these polymerization methods, from the viewpoint of the ease of reaction, it is preferred to use solution polymerization.
[0122] When the (meth)acrylic resin (A1) having no ethylenically unsaturated group is produced by a solution polymerization method, a radical polymerization initiator is used as necessary.
[0123] The radical polymerization initiator is not particularly limited, and one appropriately selected from known radical polymerization initiators can be used. Examples of the radical polymerization initiator include azo-based polymerization initiators such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentane), and dimethyl-2,2'-azobis(2-methylpropionate); and oil-soluble polymerization initiators such as peroxide-based polymerization initiators such as benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxybenzoate, dicumyl peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(tert-butylperoxy)cyclododecane.
[0124] The radical polymerization initiator may be used alone or in combination of two or more.
[0125] The amount of the radical polymerization initiator used is preferably 0.01 to 5 parts by mass, more preferably 0.02 to 4 parts by mass, and even more preferably 0.03 to 3 parts by mass, based on 100 parts by mass of the monomer group (M1).
[0126] As the solvent used in the production of the (meth)acrylic resin (A1) having no ethylenically unsaturated group by solution polymerization, a general solvent can be used. Examples of the solvent include esters such as ethyl acetate, propyl acetate, and butyl acetate; aromatic hydrocarbons such as toluene, xylene, and benzene; aliphatic hydrocarbons such as hexane and heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone; glycols such as ethylene glycol, propylene glycol, and dipropylene glycol; glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether; and glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate.
[0127] The solvent may be used alone or in combination of two or more.
[0128] [Method for producing resin composition]
[0129] The resin composition can be produced by a conventionally known method, for example, by mixing and stirring a (meth)acrylic resin (A1) having no ethylenically unsaturated group and a crosslinking agent (B1) and other components such as a tackifier, a solvent, and various additives as required using a conventionally known method.
[0130] The method for mixing and stirring the components contained in the resin composition is not particularly limited. The mixing and stirring can be performed using, for example, a homodisper or a stirring device equipped with stirring blades such as a paddle.
[0131] [Method for producing intermediate layer]
[0132] The intermediate layer can be manufactured by the following method, for example. First, a resin composition is applied to a substrate. When the resin composition contains a solvent, the solvent is removed by heating and drying to form an intermediate layer before curing. Then, before laminating an adhesive layer or an adhesive layer before curing, a release sheet is attached to the intermediate layer before curing as required. The intermediate layer before curing can be cured by heating and aging the obtained sheet in an oven for a certain period of time to form a cross-linked structure. The curing reaction can also be carried out after attaching the intermediate layer before curing and the adhesive layer before curing.
[0133] The intermediate layer can be produced by the following method. A resin composition is applied to a release sheet. When the resin composition contains a solvent, the solvent can be removed by heating and drying to form a pre-cured intermediate layer. Then, the release sheet having the pre-cured intermediate layer is placed on a substrate in a manner that the pre-cured intermediate layer side faces the substrate, and the intermediate layer is transferred to the substrate. The resulting sheet can also be formed into a cross-linked structure as described above.
[0134] As a method for coating the resin composition on a substrate (or a release sheet), a known method can be used. As a specific example, a conventional coating machine can be used, and for example, a method for coating using a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a rod coater, a knife coater, a spray coater, a notch wheel coater, a direct coater, etc. can be listed.
[0135] There are no particular restrictions on the conditions for heating and drying the coated resin composition, but the temperature is usually 25 to 180°C, preferably 60 to 150°C, and the heating and drying is usually carried out for 1 to 20 minutes, preferably 1 to 10 minutes. By heating and drying under the above conditions, the solvent contained in the resin composition can be removed. There are no particular restrictions on the reaction conditions for curing the pre-curing intermediate layer after (cross-linking) heating and drying, but the temperature is usually 25 to 100°C, preferably 30 to 80°C, and the temperature is usually 1 to 14 days, preferably 1 to 7 days. By carrying out the curing reaction under the above conditions, the (meth) acrylic resin (A1) without an ethylenically unsaturated group can be cross-linked with the cross-linking agent (B1), and the gel fraction of the intermediate layer can be adjusted to the desired range.
[0136] (Peel Sheet (Separator))
[0137] As the release sheet, a known sheet-shaped material can be appropriately selected and used. As the release sheet, the same as the above-mentioned resin sheet used as the base material can be used.
[0138] The thickness of the release sheet can be appropriately selected in accordance with the material of the release sheet, etc. When a resin sheet is used as the release sheet, the thickness of the release sheet is preferably 5 to 300 μm, more preferably 10 to 200 μm, and even more preferably 25 to 100 μm.
[0139] The release surface (the surface disposed in contact with the intermediate layer) of the release sheet may be subjected to a release treatment using a conventionally known release agent such as a silicone-based, long-chain alkyl-based, or fluorine-based release agent as required.
[0140] [Adhesive layer]
[0141] The adhesive layer is a cured product of an adhesive composition containing a (meth) acrylic resin (A2) having an ethylenically unsaturated group, a crosslinking agent (B2) and a photopolymerization initiator (C). The cured product is a product (crosslinked body) of a functional group of the (meth) acrylic resin (A2) having an ethylenically unsaturated group that can react with a functional group of the crosslinking agent (B2), and a reaction with a functional group of the crosslinking agent (B2), and is not a photocured product of a photopolymerization initiator (C). On the adhesive layer, by irradiation with active energy rays such as ultraviolet rays, the ethylenically unsaturated group of the (meth) acrylic resin (A2) having an ethylenically unsaturated group begins free radical polymerization by means of the decomposition of the photopolymerization initiator (C), and further forms a (photocured) crosslinked structure. The protective sheet for semiconductor processing has an adhesive layer, so that even if it is attached to the adherend and undergoes various processing steps, it will not float up, and has good adhesion to the adherend. Furthermore, after the processing step is completed, the peel strength of the pressure-sensitive adhesive layer can be reduced by irradiation with active energy rays, and the pressure-sensitive adhesive layer can be peeled from the adherend without leaving any adhesive residue.
[0142] The thickness of the adhesive layer is preferably 5 μm or more, more preferably 10 μm or more, and more preferably 15 μm or more. The thickness of the adhesive layer is preferably 100 μm or less, more preferably 50 μm or less, and more preferably 30 μm or less. The combination of these lower limit values and upper limit values may be any combination. The thickness of the adhesive layer is preferably 5 to 100 μm, more preferably 10 to 50 μm, and more preferably 15 to 30 μm. When the thickness of the adhesive layer is 5 μm or more, the adhesion to the adherend is good. When the thickness of the adhesive layer is 100 μm or less, the generation of residual adhesive is suppressed.
[0143] The thickness ratio of the intermediate layer to the adhesive layer (intermediate layer / adhesive layer) is preferably 1 to 50, more preferably 1 to 40, more preferably 1 to 30, and even more preferably 1 to 10. When the thickness ratio is within the above range, both conformability to irregularities and heat resistance can be achieved.
[0144] ((Meth)acrylic resin (A2) having ethylenically unsaturated group)
[0145] The (meth) acrylic resin (A2) with ethylenically unsaturated groups is an adduct of an ethylenically unsaturated compound (a2-3) having an epoxy group to a copolymer containing a monomer group (M2) of an ethylenically unsaturated compound (a2-1) and an ethylenically unsaturated compound (a2-2) having a carboxyl group, and is not particularly limited. The (meth) acrylic resin (A2) with ethylenically unsaturated groups can be used alone or in combination with two or more. When an adhesive layer is formed by using a (meth) acrylic resin (A2) with an ethylenically unsaturated group as an adduct of an ethylenically unsaturated compound (a2-3) having an epoxy group to a (meth) acrylic copolymer having a carboxyl group, the protective sheet for semiconductor processing has high heat resistance, and from the step of being attached to the adherend to the processing step and the peeling step, even when exposed to high temperature conditions, it is possible to maintain high tracking properties to the concave and convex of the adherend. Furthermore, when the protective sheet for semiconductor processing is peeled off from an adherend after the processing step, good peeling properties can be obtained by irradiating the sheet with active energy rays.
[0146] The glass transition temperature (Tg) of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably -80°C or higher, more preferably -70°C or higher, and more preferably -60°C or higher. The glass transition temperature (Tg) of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 0°C or lower, more preferably -10°C or lower, and more preferably -20°C or lower. The combination of these lower limits and upper limits may be any combination. The glass transition temperature (Tg) of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably -80°C to 0°C, more preferably -70°C to -10°C, and more preferably -60°C to -20°C. When the glass transition temperature is -80°C or higher, a high cohesive adhesive layer can be obtained, so that the resin can be prevented from eluting during sheet molding. When the glass transition temperature is 0° C. or lower, the adhesion between the intermediate layer and the adhesive layer can be further improved.
[0147] The weight average molecular weight of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 100,000 to 2,000,000, more preferably 150,000 to 1,500,000, and more preferably 200,000 to 1,000,000. When the weight average molecular weight is 100,000 or more, a highly cohesive adhesive layer can be obtained, and the dissolution of the resin can be prevented during sheet molding. When the weight average molecular weight is 2,000,000 or less, molding and processing become easy.
[0148] The ethylenically unsaturated group equivalent of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 100 g / mol or more, more preferably 300 g / mol or more, and more preferably 500 g / mol or more. The ethylenically unsaturated group equivalent of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 4000 g / mol or less, more preferably 3000 g / mol or less, and more preferably 1500 g / mol or less. The combination of these lower limits and upper limits may be any combination. The ethylenically unsaturated group equivalent of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 100 to 4000 g / mol, more preferably 300 to 3000 g / mol, and more preferably 500 to 1500 g / mol. When the ethylenically unsaturated group equivalent is within the above range, sufficient curability can be imparted. In addition, the pick-up property after UV irradiation becomes good.
[0149] The acid value of the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 1 to 100 mgKOH / g, more preferably 5 to 75 mgKOH / g, and more preferably 10 to 50 mgKOH / g. When the acid value is 1 mgKOH / g or more, it can react sufficiently with the epoxy crosslinking agent to obtain an adhesive layer with high cohesive force. When the acid value is 100 mgKOH / g or less, the cohesive force of the obtained resin will not become too high, and the workability is easy.
[0150] The content of the (meth) alkyl acrylate (a2-1) in the monomer group (M2) constituting the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 50 to 95 mol%, more preferably 60 to 90 mol%, and more preferably 70 to 90 mol%. When the content of the (meth) alkyl acrylate (a2-1) is 50 mol% or more, the adhesion to the intermediate layer is good. When the content of the (meth) alkyl acrylate (a2-1) is 95 mol% or less, the content of the ethylenically unsaturated compound (a2-2) having a carboxyl group can be fully ensured, so the amount of crosslinking with the crosslinking agent (B2) can be fully ensured, thereby improving the cohesive force of the adhesive layer. In addition, since the amount of ethylenically unsaturated groups introduced can be fully ensured, the peel strength of the protective sheet for semiconductor processing can be fully reduced when the active energy line is irradiated.
[0151] The content of the ethylenically unsaturated compound (a2-2) having a carboxyl group in the monomer group (M2) constituting the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 1 to 50 mol%, more preferably 5 to 40 mol%, and more preferably 10 to 30 mol%. When the content of the ethylenically unsaturated compound (a2-2) having a carboxyl group is 1 mol% or more, the amount of crosslinking with the crosslinking agent (B2) can be fully ensured to improve the cohesive force of the adhesive layer. In addition, since the amount of introduction of the ethylenically unsaturated group can be fully ensured, the peel strength of the protective sheet for semiconductor processing can be fully reduced when the active energy line is irradiated.
[0152] The amount of the ethylenically unsaturated compound (a2-3) having an epoxy group is preferably 1 to 40 mol, more preferably 3 to 30 mol, and more preferably 8 to 25 mol relative to 100 mol of the monomer group (M2). The addition rate of the ethylenically unsaturated compound (a2-3) having an epoxy group to the carboxyl group from the ethylenically unsaturated compound (a2-2) having a carboxyl group is preferably 50 to 99%, more preferably 65 to 95%, and more preferably 70 to 85%. When set within the above range, the amount of crosslinking with the crosslinking agent (B2) can be ensured, and the amount of introduction of the ethylenically unsaturated group can be sufficiently ensured.
[0153] The monomer group (M2) may contain other monomers (a2-4) as required. The content of other monomers (a2-4) in the monomer group (M2) constituting the (meth) acrylic resin (A2) having an ethylenically unsaturated group is preferably 0 to 45 mol%, more preferably 0 to 30 mol%, and more preferably 0 to 10 mol%.
[0154] Specific examples and further preferred examples of (meth) alkyl acrylate (a2-1) are the same as those of (meth) alkyl acrylate (a1-1). (Meth) alkyl acrylate (a2-1) can be used alone or in combination of two or more thereof. Specific examples and further preferred examples of the ethylenically unsaturated compound (a2-2) having a carboxyl group are the same as those of the ethylenically unsaturated compound (a1-3) having a carboxyl group. The ethylenically unsaturated compound (a2-2) having a carboxyl group can be used alone or in combination of two or more thereof.
[0155] As the ethylenically unsaturated compound (a2-3) having an epoxy group, it is a compound that does not have a carboxyl group but has an epoxy group and an ethylenically unsaturated group, and there is no particular limitation. In the present invention, the so-called "ethylenically unsaturated compound having an epoxy group" also includes an ethylenically unsaturated compound containing an oxetane ring instead of an epoxy group. Specifically, glycidyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate glycidyl ether, 3,4-epoxycyclohexyl methyl (meth) acrylate, 3,4-epoxycyclohexane-1-carboxylic acid allyl, (3-ethyloxetane-3-yl) methyl (meth) acrylate, etc. can be listed. Among them, from the perspective of ease of synthesis, glycidyl (meth) acrylate is preferred, and from the perspective of heat resistance, 3,4-epoxycyclohexyl methyl (meth) acrylate is preferred. The ethylenically unsaturated compound (a2-3) having an epoxy group can be used alone or in combination of two or more.
[0156] As other monomers (a2-4) other than (a2-1) and (a2-2), the same compounds as the (meth)acrylates (a1-2) and other monomers (a1-4) having a hydroxyl group can be used. Other monomers (a2-4) can be used alone or in combination of two or more.
[0157] (Crosslinking agent (B2))
[0158] As a crosslinking agent (B2), a compound having a plurality of functional groups that can react with any one of the plurality of functional groups possessed by the (meth) acrylic resin (A2) having an ethylenically unsaturated group is not particularly limited. Because the (meth) acrylic resin (A2) having an ethylenically unsaturated group has a carboxyl group, as a crosslinking agent (B2) that can be used, for example, epoxy crosslinking agents and aziridine crosslinking agents can be cited. The adhesive layer contains a crosslinking agent (B2), so the cohesive force of the adhesive layer can be improved, and the residual glue when the semiconductor processing protective sheet is peeled off from the adherend can also be reduced. The crosslinking agent (B2) can be used alone or in combination with two or more.
[0159] As the epoxy crosslinking agent and the aziridine crosslinking agent, the same epoxy crosslinking agent and the aziridine crosslinking agent as the crosslinking agent (B1) can be used. The epoxy crosslinking agent can be used alone or in combination of two or more. The aziridine crosslinking agent can be used alone or in combination of two or more.
[0160] The content of the crosslinking agent (B2) is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, and more preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the (meth) acrylic resin (A2) having an ethylenically unsaturated group. When the content of the crosslinking agent (B2) is 0.05 parts by mass or more, a three-dimensional crosslinked structure is sufficiently formed in the adhesive layer, and as a result, an adhesive layer having sufficiently high cohesive force is obtained. When the content of the crosslinking agent (B2) is 30 parts by mass or less, a moderate gelation time can be ensured during sheet molding.
[0161] (Photopolymerization initiator (C))
[0162] Examples of the photopolymerization initiator (C) include benzophenone, benzil, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzoic acid methyl ether, benzoic acid isobutyl ether, benzoic acid n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, Carbonyl photopolymerization initiators such as methylbenzoylformate, 4'-dimethylaminoacetophenone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, etc.; sulfide photopolymerization initiators such as diphenyl disulfide, diphenylmethyl disulfide, tetraethylthiuram disulfide, tetramethylammonium monosulfide, etc.; acylphosphine oxide photopolymerization initiators such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide, etc.; quinone photopolymerization initiators such as benzoquinone and anthraquinone; sulfonyl chloride photopolymerization initiators and thioxanthone photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, etc.
[0163] Among these, it is preferable to use a carbonyl-based photopolymerization initiator or an acylphosphine oxide-based photopolymerization initiator from the viewpoint of high sensitivity to ultraviolet rays and heat resistance.
[0164] The photopolymerization initiator (C) may be used alone or in combination of two or more.
[0165] The content of the photopolymerization initiator (C) is preferably 0.1 to 5.0 parts by mass, and more preferably 0.5 to 2.0 parts by mass, relative to 100 parts by mass of the (meth) acrylic resin (A2) having an ethylenically unsaturated group. When the content of the photopolymerization initiator (C) is 0.1 parts by mass or more, the adhesive layer can be cured at a sufficiently fast curing speed by irradiating active energy rays, so that the peel strength of the adhesive layer after irradiation with active energy rays can be sufficiently reduced. When the content of the photopolymerization initiator (C) is 5.0 parts by mass or less, when the protective sheet for semiconductor processing is peeled off from the adherend, the adhesive layer becomes difficult to remain on the adherend. Even if the content of the photopolymerization initiator (C) exceeds 5.0 parts by mass, the effect of the content of the photopolymerization initiator (C) is not seen, so when the content is set to 5.0 parts by mass or less, the adhesive composition can be economically manufactured.
[0166] (Other ingredients)
[0167] The adhesive composition may contain other components other than the (meth) acrylic resin (A2) having an ethylenically unsaturated group, the crosslinking agent (B2) and the photopolymerization initiator (C) as required. Other components include, for example, adhesion imparting agents, solvents and various additives. As adhesion imparting agents, solvents and various additives, the same ones as those described for each resin composition can be used.
[0168] [Method for producing (meth)acrylic resin (A2) having ethylenically unsaturated group]
[0169] The method for producing the (meth)acrylic resin (A2) having an ethylenically unsaturated group is not particularly limited. The (meth)acrylic resin (A2) having an ethylenically unsaturated group is obtained, for example, by copolymerizing a monomer group (M2) by a known polymerization method and then adding an ethylenically unsaturated compound (a2-3) having an epoxy group to a part of the carboxyl groups of the copolymer.
[0170] The copolymer used in the production of the (meth)acrylic resin (A2) having an ethylenically unsaturated group can be obtained by the same method as the method for producing the (meth)acrylic resin (A1) having no ethylenically unsaturated group. Among them, the solution polymerization method is also preferred, and the types and amounts of the free radical polymerization initiator and solvent used are the same as those described in the production method of the (meth)acrylic resin (A1) having no ethylenically unsaturated group.
[0171] When a copolymer having a carboxyl group is produced as a copolymer for producing a (meth)acrylic resin (A2) having an ethylenically unsaturated group, and an ethylenically unsaturated compound (a2-3) having an epoxy group is added to a part of the carboxyl group, the temperature of the addition reaction is preferably 80 to 150° C., and particularly preferably 90 to 130° C. When the temperature of the addition reaction is 80° C. or higher, a sufficient reaction rate can be obtained. When the temperature of the addition reaction is 150° C. or lower, free radical polymerization proceeds by heat, and the double bond portion is crosslinked, thereby preventing the generation of gelled products.
[0172] In the addition reaction, a known catalyst can be used as needed. Examples of the catalyst include primary amines such as n-butylamine, n-hexylamine, benzylamine, diethylenetriamine, triethylenetetramine, and diethylaminopropylamine; tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, and 1,4-diazabicyclo[2.2.2]octane; aromatic amines such as aniline, toluidine, phenylenediamine, diaminodiphenylmethane, and 1,8-diaminonaphthalene; pyridine compounds such as pyridine, 2,6-lutidine, and 4-dimethylaminopyridine; imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole; tetramethylammonium chloride, tetramethylammonium bromide, and tetrabutylammonium bromide. Ammonium salts such as ammonium chloride, tetrabutylammonium bromide, tetrabutylammonium iodide, and tetrabutylammonium hydroxide; alkyl ureas such as tetramethyl urea; alkyl guanidines such as tetramethylguanidine; phosphine compounds such as triphenylphosphine, dimethylphenylphosphine, tricyclohexylphosphine, tributylphosphine, tri(4-methylphenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(2,6-dimethylphenyl)phosphine, tri(2,6-dimethoxyphenyl)phosphine, tri(2,4,6-trimethylphenyl)phosphine, and tri(2,4,6-trimethoxyphenyl)phosphine; and phosphonium salts such as tetraphenylphosphonium chloride, tetraphenylphosphonium bromide, tetraphenylphosphonium iodide, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetrapentafluorophenylborate, 4-hydroxyphenyl-2-(triphenylphosphonium)phenolate, and 4-hydroxyphenyl-2-{tri-(4-methylphenyl)phosphonium}phenolate. Among them, from the viewpoint of reactivity, it is preferable to use a pyridine compound, an imidazole compound, an ammonium salt, a phosphine compound or a phosphonium salt.
[0173] The amount of the catalyst used in the addition reaction is preferably 0.01 to 20 parts by mass, more preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the total of the copolymer and the ethylenically unsaturated compound (a2-3) having an epoxy group.
[0174] During the addition reaction, a gas having a polymerization inhibiting effect may be further introduced into the reaction system, or may be added to the polymerization inhibitor. By introducing a gas having a polymerization inhibiting effect into the reaction system, or adding a polymerization inhibitor, gelation during the addition reaction can be prevented.
[0175] Examples of the gas having a polymerization inhibiting effect include a gas containing oxygen to a degree that does not cause an explosion range of substances in the system, and examples thereof include air.
[0176] As the polymerization inhibitor, known ones can be used without particular limitation, and examples thereof include 4-methoxyphenol, hydroquinone, p-hydroxyanisole, 2,6-di-tert-butylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol) and phenothiazine. The polymerization inhibitor can be used alone or in combination of two or more.
[0177] The amount of the polymerization inhibitor used is preferably 0.005 to 5 parts by mass, preferably 0.03 to 3 parts by mass, and more preferably 0.05 to 1.5 parts by mass relative to a total of 100 parts by mass of the copolymer and the ethylenically unsaturated compound (a2-3) having an epoxy group. When the amount of the polymerization inhibitor used is 0.005 parts by mass or more, gelation during the addition reaction can be prevented. On the other hand, when the amount of the polymerization inhibitor used is 5 parts by mass or less, sufficient exposure sensitivity of the adhesive layer during active energy line irradiation can be obtained.
[0178] When a gas having a polymerization inhibitory effect is used in combination with a polymerization inhibitor, it is more preferable because the amount of the polymerization inhibitor to be used can be reduced or the polymerization inhibitory effect can be enhanced.
[0179] [Method for producing adhesive composition]
[0180] The adhesive composition can be produced by a conventionally known method. For example, the (meth) acrylic resin (A2) having an ethylenically unsaturated group, a crosslinking agent (B2), a photopolymerization initiator (C), and other components such as an adhesion-imparting agent, a solvent, and various additives as required can be mixed and stirred using a conventionally known method.
[0181] The method for mixing and stirring the components contained in the adhesive composition is not particularly limited. The mixing and stirring can be performed using, for example, a stirring device equipped with stirring blades such as a homodispersor and a paddle.
[0182] [Method for producing adhesive layer]
[0183] The adhesive layer can be manufactured by the following method, for example. First, an adhesive composition is applied to a release sheet, and when it contains a solvent, the adhesive composition is heated and dried to remove the solvent to form a pre-cured adhesive layer. Then, the release sheet can be attached to the intermediate layer of the pre-cured adhesive layer or the laminating surface of the pre-cured intermediate layer as required, until it is about to be laminated to the intermediate layer or the pre-cured intermediate layer. The pre-cured adhesive layer can also be subjected to a curing reaction by heating and aging the obtained sheet in an oven for a certain period of time to form a cross-linked structure. The curing reaction can also be carried out after the pre-cured intermediate layer and the pre-cured adhesive layer are attached.
[0184] The adhesive layer can be manufactured by the method shown below. The adhesive composition is directly applied to the intermediate layer of a sheet having an intermediate layer on one main surface of the substrate. When containing a solvent, the adhesive layer before curing is formed after the solvent is removed by heating and drying. Then, a release sheet is attached to the adhesive layer before curing as required. The resulting sheet is formed into a cross-linked structure as described above. In addition, the adhesive composition is directly applied to the intermediate layer before curing of a sheet having an intermediate layer before curing on one main surface of the substrate. When containing a solvent, the adhesive layer before curing can also be formed after the solvent is removed by heating and drying. Then, a release sheet is attached to the adhesive layer before curing as required. Then, the intermediate layer before curing and the adhesive layer before curing are cured simultaneously. In these methods, the step of attaching the intermediate layer and the adhesive layer to obtain a protective sheet for semiconductor processing can be omitted.
[0185] The method of coating the adhesive composition on a release sheet (or an intermediate layer or an intermediate layer before curing), the conditions and preferred ranges for heating and drying the coated adhesive composition, and the conditions and preferred ranges for aging the pre-cured adhesive layer after heating and drying in an oven for a certain period of time are the same as those described for the method for manufacturing the intermediate layer.
[0186] (Peel Sheet (Separator))
[0187] As the release sheet, a known sheet-like material can be appropriately selected. As the release sheet, the same resin sheet as that used as the substrate can be used.
[0188] The thickness of the release sheet can be appropriately selected according to the application of the semiconductor processing protective sheet, the material of the release sheet, etc. When a resin sheet is used as the release sheet, the thickness of the release sheet is preferably 5 to 300 μm, more preferably 10 to 200 μm, and more preferably 25 to 100 μm.
[0189] The release surface (surface disposed in contact with the pressure-sensitive adhesive layer) of the release sheet may be subjected to a release treatment using a conventionally known release agent such as a silicone-based, long-chain alkyl-based, or fluorine-based release agent, as required.
[0190] [Method for producing protective sheet for semiconductor processing]
[0191] An example of an embodiment of a method for manufacturing a protective sheet for semiconductor processing is shown below. A sheet having a pre-cured intermediate layer on one main surface of a substrate and a sheet having a pre-cured adhesive layer on a release sheet are prepared. When the release sheet is laminated on the bonding surfaces of the two sheets, the release sheet is peeled off and the bonding surface of the pre-cured intermediate layer (the opposite side of the substrate) and the bonding surface of the pre-cured adhesive layer (the opposite side of the release sheet) are bonded face to face.
[0192] Then, in a state where the pre-curing intermediate layer and the pre-curing adhesive layer are attached, heating is performed in an oven for a certain period of time (aging step) to thermally cure the pre-curing intermediate layer and the pre-curing adhesive layer to obtain a cured product of the two layers. Although there is no particular restriction on the conditions of the aging step, it is usually 30 to 100°C, and preferably 40 to 80°C, and is usually performed for 1 to 14 days, and preferably 1 to 7 days. By aging under the above conditions, the (meth) acrylic resin (A1) and the crosslinking agent (B1) without ethylenically unsaturated groups in the intermediate layer are crosslinked, and the (meth) acrylic resin (A2) and the crosslinking agent (B2) with ethylenically unsaturated groups in the adhesive layer are crosslinked, and the gel fraction of each layer can be adjusted to the desired range. By combining the components, it is also expected that crosslinking at the interface between the intermediate layer and the adhesive layer, that is, crosslinking of (A1) and (B2) and crosslinking of (A2) and (B1) can be performed, so by going through the aging step, it is expected that the interlayer adhesion between the intermediate layer and the adhesive layer can be improved.
[0193] In addition to the above method, there is also a method of first curing either the pre-cured intermediate layer or the pre-cured adhesive layer, and then bonding the other pre-cured layer to cure the pre-cured layer, and a method of bonding the intermediate layer (as a cured product) and the adhesive layer (as a cured product).
[0194] [Method for manufacturing semiconductor device having bump electrodes]
[0195] A method for manufacturing a semiconductor device having a bump electrode according to one embodiment includes:
[0196] A protective step of laminating the adhesive layer of the semiconductor processing protective sheet to the surface of the semiconductor device with the bump electrode,
[0197] an active energy ray irradiation step of irradiating the protective sheet for semiconductor processing with active energy rays to photo-cure the adhesive layer,
[0198] A step of heating the semiconductor device to which the protective sheet for semiconductor processing is bonded, and a step of peeling the protective sheet for semiconductor processing from the surface with the bump electrode.
[0199] Furthermore, a processing step may be performed between the protection step and the stripping step. The protection step may be performed first and the stripping step may be performed last. The order of other steps may be changed.
[0200] (Protection Steps)
[0201] In the protection step, the adhesive layer of the semiconductor processing protection sheet is attached to the surface of the semiconductor device with the bump electrode. In this way, the surface of the semiconductor device with the bump electrode is protected. As specific examples of semiconductor devices, semiconductor chips with bumps, printed wiring boards (PCBs) with bumps, flexible wiring circuit boards (FPCs) with bumps, etc., which are semiconductor devices with bumps on the surface, can be listed. In the manufacturing steps of these semiconductor devices, various steps can be performed up to the installation step of connecting the bump electrodes to other electronic devices. By protecting the surface with the bump electrode during the processing step, it is possible to prevent damage, breakage, contamination, etc. of the surface with the bump electrode. The semiconductor processing protection sheet can also have the function of temporarily fixing the semiconductor device for continuing the processing step.
[0202] When the height of the bump electrode is H [μm] and the total thickness of the intermediate layer and the adhesive layer is d [μm], d / H is preferably 0.40-110, more preferably 1.00-100, more preferably 1.10-20, and even more preferably 1.25-10.
[0203] When the height of the bump electrode is set to H [μm] and the total thickness of the intermediate layer and the adhesive layer is set to d [μm], d / H is preferably 0.40 or more, more preferably 1.00 or more, more preferably 1.10 or more, and more preferably 1.25 or more. d / H is preferably 110 or less, more preferably 100 or less, more preferably 20 or less, more preferably 10 or less, and particularly preferably 5.0 or less. Any combination of these lower limit values and upper limit values may be used.
[0204] When a release sheet is provided on the adhesive layer, the release sheet can protect the adhesive layer until it is used. When a release sheet is provided on the adhesive layer, the adhesive layer can be exposed by peeling off the release sheet, and the operation of pressing the adhesive layer (bonding surface) onto the surface of the semiconductor device with the bump electrode can be performed more efficiently.
[0205] When the semiconductor device has a plurality of surfaces with bump electrodes, a semiconductor processing protection sheet is attached to some or all of the surfaces with bump electrodes in the protection step. For example, when laminating semiconductor chips disclosed in Japanese Patent Publication No. 2014-225546, a semiconductor processing protection sheet may be attached to a non-mounting surface other than the mounting surface of the surface with bump electrodes.
[0206] (Processing steps)
[0207] The method for manufacturing a semiconductor device may include a processing step between the protection step and the peeling step described later.
[0208] As a processing step, a processing step used in the manufacture of semiconductor devices known in the past can be used without particular limitation. For example, when the semiconductor processing protection sheet used in the protection step is used as a dicing tape for the wafer, the protection step can be implemented, and after the semiconductor processing protection sheet is attached to the wafer forming a plurality of parts, the processing step is implemented, and the wafer is cut to separate (divide) the parts to obtain the component small pieces (chips). When the semiconductor chip lamination step is implemented as a processing step, only the non-mounting surface of the surface with the bump electrode is protected in the protection step, and the mounting surfaces to which the semiconductor processing protection sheet is not attached are brought into contact with each other and electrically connected under lamination.
[0209] (Heating step)
[0210] In the method for manufacturing a semiconductor device, a heating step is provided between the protection step and the stripping step described later. When the method for manufacturing a semiconductor device includes a processing step after the protection step, the order of the processing step and the heating step is not limited. From the perspective of the protection function and temporary fixing function of the semiconductor processing protection sheet, that is, the adhesion performance can be maximized, it is preferred to perform the processing step and the heating step at the same time, or to perform the processing step before the heating step.
[0211] As the heating step, a heating step used in the manufacture of semiconductor devices known in the past can be used without particular limitation. As the heating step, for example, a post-curing step of a PCB with bumps, a sputtering step of a semiconductor chip, and a reflow step when a semiconductor chip is connected can be cited.
[0212] The conditions of the heating step are not particularly limited. When a protection step is implemented before the heating step, for example, a high-temperature treatment of above 150°C, above 180°C or above 200°C is performed, the surface with the bump electrode can also be well protected. The maximum reaching temperature of the heating step is not particularly limited, for example, 100 to 230°C. Although the upper limit temperature of the heating step is not particularly limited, from the perspective of the heat resistance of the protective sheet for semiconductor processing, 300°C is preferred, and 270°C is more preferred. The heating time is not particularly limited, for example, 1 minute to 180 minutes, 1 minute to 120 minutes is preferred, and 1 minute to 60 minutes is more preferred.
[0213] (Active energy ray irradiation step)
[0214] In the active energy line irradiation step, active energy lines are usually irradiated from the substrate side of the semiconductor processing protection sheet. When the adherend has light transmittance, active energy lines can also be irradiated from the adherend side toward the semiconductor processing protection sheet. The adhesive layer can be cross-linked and cured by irradiation with active energy lines, which can improve the heat resistance of the semiconductor processing protection sheet, or can improve the peelability of the semiconductor processing protection sheet. The active energy line irradiation step can be performed between the protection step and the stripping step described later, and is not limited to the order of the processing step and the heating step.
[0215] The active energy ray irradiation step can also be divided into two steps. For example, the active energy ray irradiation step is performed between the protection step and the processing step, and the heat resistance of the semiconductor processing protective sheet can be improved by crosslinking and curing a part of the ethylenically unsaturated groups contained in the adhesive layer. And when the peeling step described later is about to be performed, the second active energy ray irradiation step is performed first, and the peel strength of the semiconductor processing protective sheet can be reduced by crosslinking (completely curing) the remaining ethylenically unsaturated groups, and the peelability from the adherend can be improved.
[0216] As active energy line, for example, gamma ray, ultraviolet (UV), visible light, infrared (heat line), radio wave, α ray, β ray, electron beam, plasma flow, electric offline, particle line etc. can be listed, and ultraviolet (UV) is also preferred. As the light source used when the semiconductor processing protective sheet before peeling that is attached to the adherend is UV irradiated, for example, LED lamp, high pressure mercury lamp, ultra-high pressure mercury lamp, carbon arc lamp, xenon lamp, metal halide lamp, chemical lamp and black light lamp can be listed. In active energy line irradiation, it is preferred to use LED lamp, high pressure mercury lamp or metal halide lamp.
[0217] The active energy ray irradiation dose to the semiconductor processing protective sheet is 50 to 3000 mJ / cm 2 Preferably, 100 to 1500 mJ / cm 2 The active energy ray irradiation dose irradiated to the semiconductor processing protective sheet is 50 mJ / cm 2 When the active energy ray irradiation is above 3000 mJ / cm, the adhesive layer can be cured at a sufficiently fast curing speed, so the adhesive force of the adhesive layer after the active energy ray irradiation can be sufficiently reduced. 2 , the corresponding effect cannot be obtained, so the active energy ray irradiation dose irradiated to the semiconductor processing protective sheet is set at 3000mJ / cm 2 When the viscosity is less than 50%, the influence of the active energy ray irradiation on the adherend can be reduced, and the ethylenically unsaturated group contained in the pressure-sensitive adhesive layer can be cross-linked economically.
[0218] (Peeling step)
[0219] In the stripping step, the semiconductor processing protective sheet is stripped from the surface with the bump electrode and removed. The stripping step is performed after the adhesive layer is cured by irradiation with active energy rays. By irradiation with active energy rays, the ethylenically unsaturated bonds contained in the adhesive layer form a three-dimensional crosslinked structure and solidify. As a result, the peel strength of the adhesive layer is reduced. Thereafter, the semiconductor processing protective sheet is stripped from the semiconductor device.
[0220] According to one embodiment of a method for manufacturing a semiconductor device with a bump electrode, even when a heating step is performed, a semiconductor device can be obtained without generating exhaust gas and without residual glue on the surface of an adherend with bumps, so the installation step can be continued without causing any problems with the obtained semiconductor device.
[0221] Example
[0222] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0223] The raw materials used are shown below.
[0224] (Meth)acrylic acid alkyl ester (a1-1) or (a2-1):
[0225] Methyl methacrylate, Nippon Shokubai Co., Ltd.,
[0226] n-Butyl acrylate, Osaka Organic Chemical Industry Co., Ltd.
[0227] 2-Ethylhexyl acrylate, Osaka Organic Chemical Industry Co., Ltd.
[0228] 2-Ethylhexyl acrylate, Osaka Organic Chemical Industry Co., Ltd.
[0229] (Meth)acrylate (a1-2) or other monomer (a2-4) having a hydroxyl group:
[0230] 2-hydroxyethyl acrylate, Nippon Shokubai Co., Ltd.
[0231] Ethylenically unsaturated compound (a1-3) or (a2-2) having a carboxyl group:
[0232] Acrylic, Nippon Shokubai Co., Ltd.,
[0233] Methacrylic acid, Nippon Shokubai Co., Ltd.
[0234] Other monomers (a1-4):
[0235] N,N-Dimethylacrylamide
[0236] Free Radical Polymerization Initiator:
[0237] 2,2'-Azobis(isobutyronitrile), Fujifilm Wako Pure Chemical Industries, Ltd.
[0238] Ethylenically unsaturated compound having an epoxy group (a2-3):
[0239] 3,4-Epoxycyclohexylmethyl methacrylate, Daicel Corporation,
[0240] Glycidyl methacrylate, NOF Corporation
[0241] Ethylenically unsaturated compounds having isocyanate groups:
[0242] Karens (trademark) MOI (2-isocyanate ethyl methacrylate), Showa Denko K.K.,
[0243] Crosslinking agent (B1):
[0244] HX (isocyanurate of hexamethylene diisocyanate), Tosoh Corporation, trade name: Coronate HX,
[0245] L-45E (trimethylolpropane toluene diisocyanate adduct), Tosoh Corporation, trade name: Coronate L-45E
[0246] Crosslinking agent (B2):
[0247] KF-105 (epoxy-modified polydimethylsiloxane at both ends), Shin-Etsu Chemical Co., Ltd., trade name KF-105,
[0248] TetradX (N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine]), Mitsubishi Gas Chemical Co., Ltd., trade name: TETRAD-X
[0249] Photopolymerization initiator (C):
[0250] TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide), BASF, trade name: L-TPO
[0251] [Synthesis Example 1: Production of (meth)acrylic resin (A1-1) not having an ethylenically unsaturated group]
[0252] A mixed solution was prepared having a monomer group (M1) containing 7 parts by mass (9.07 mol) of methyl methacrylate, 50 parts by mass (50.61 mol) of n-butyl acrylate, 35 parts by mass (24.64 mol) of 2-ethylhexyl acrylate, 10 parts by mass (13.09 mol) of N,N-dimethylacrylamide, 1.5 parts by mass (1.68 mol) of 2-hydroxyethyl acrylate and 0.5 parts by mass (0.90 mol) of acrylic acid, and 0.1 parts by mass of 2,2'-azobis(isobutyronitrile) as a polymerization initiator relative to 100 parts by mass of the monomer group (M1).
[0253] In a four-necked flask equipped with a stirrer, a dropping funnel, a cooling tube and a nitrogen inlet tube, 175.6 parts by mass of butyl acetate as a solvent was placed, and the temperature was raised to 80° C. in a nitrogen atmosphere. The reaction temperature was maintained at 80° C.±2° C., and the mixed solution was uniformly dripped into the four-necked flask over 4 hours. After the dripping was completed, the mixture was further stirred at 80° C.±2° C. for 6 hours to perform polymerization, thereby obtaining a reaction solution containing a (meth)acrylic resin (A1-1) having no ethylenically unsaturated group (weight average molecular weight (Mw): 300,000, glass transition temperature (Tg): −42° C., acid value: 3.74 mgKOH / g, hydroxyl value: 6.97 mgKOH / g).
[0254] [Synthesis Example 2: Production of (meth)acrylic resin (A2-1) having an ethylenically unsaturated group]
[0255] A first mixed solution containing a monomer group (M2) consisting of 60 parts by mass (45.82 mol) of 2-ethylhexyl acrylate, 28 parts by mass (30.74 mol) of n-butyl acrylate, and 12 parts by mass (23.44 mol) of acrylic acid, and 0.1 parts by mass of 2,2'-azobis(isobutyronitrile) as a radical polymerization initiator was prepared.
[0256] Next, a second mixed solution containing 1.5 parts by mass of tri(4-methylphenyl)phosphine (TPTP) as a catalyst, 100.0 parts by mass of butyl acetate as a solvent, and 91.1 parts by mass of toluene was prepared relative to 25 parts by mass (17.93 mol) of 3,4-epoxycyclohexylmethyl methacrylate and 100 parts by mass of the total of the monomer group (M2) and 3,4-epoxycyclohexylmethyl methacrylate used in the first mixed solution.
[0257] In a four-necked flask with a stirrer, a dropping funnel, a cooling tube and a nitrogen inlet tube, 175.6 parts by mass of butyl acetate as a solvent was placed and heated to 80°C under a nitrogen environment. The reaction temperature was maintained at 80°C±2°C, and the first mixed solution was uniformly dripped in the four-necked flask over 4 hours. After the dripping was completed, the polymerization was further carried out by stirring at a temperature of 80°C±2°C for 6 hours to obtain a copolymer having a carboxyl group. Then, in the reaction system, 0.15 parts by mass of 4-methoxyphenol as a polymerization inhibitor was added to a total of 100 parts by mass of the monomer group (M2) and 3,4-epoxycyclohexylmethyl methacrylate.
[0258] The reaction system to which 4-methoxyphenol was added was heated to 100°C, and the above-mentioned second mixed solution was added dropwise over a period of 0.5 hours. The mixture was then stirred at 100°C for 8 hours and cooled to room temperature (23°C) to obtain a reaction solution of a (meth)acrylic resin (A2-1) having an ethylenically unsaturated group (weight average molecular weight (Mw): 350,000, glass transition temperature (Tg): -50°C, acid value: 17.55 mgKOH / g, hydroxyl value: 57.13 mgKOH / g, ethylenically unsaturated group equivalent: 981.98 g / mol).
[0259] [Synthesis Example 3: Production of (meth)acrylic resin (A2-2) having an ethylenically unsaturated group]
[0260] A first mixed solution containing a monomer group (M2) consisting of 10 parts by mass (14.66 mol) of methyl methacrylate, 45 parts by mass (35.85 mol) of 2-ethylhexyl acrylate, 30 parts by mass (29.90 mol) of isooctyl acrylate, and 15 parts by mass (25.58 mol) of methacrylic acid, and 0.1 parts by mass of 2,2'-azobis(isobutyronitrile) as a radical polymerization initiator was prepared.
[0261] Next, a second mixed solution was prepared containing 1.5 parts by mass of tri(4-methylphenyl)phosphine (TPTP) as a catalyst, 100 parts by mass of butyl acetate and 91.1 parts by mass of toluene as a solvent, relative to 20 parts by mass (20.66 mol) of glycidyl methacrylate and 100 parts by mass of the total of the monomer group (M2) and glycidyl methacrylate used in the first mixed solution.
[0262] In a four-necked flask equipped with a stirrer, a dropping funnel, a cooling tube and a nitrogen inlet tube, 175.6 parts by mass of butyl acetate as a solvent was placed and heated to 80°C under a nitrogen atmosphere. The reaction temperature was maintained at 80°C±2°C, and the first mixed solution was uniformly dripped into the four-necked flask over 4 hours. After the dripping was completed, the mixture was further stirred for 6 hours at a temperature of 80°C±2°C to polymerize to obtain a copolymer having a carboxyl group. Then, 0.15 parts by mass of 4-methoxyphenol as a polymerization inhibitor was added to the reaction system relative to a total of 100 parts by mass of the monomer group (M2) and glycidyl methacrylate.
[0263] The reaction system to which 4-methoxyphenol was added was heated to 100°C, and the second mixed solution was added dropwise over a period of 0.5 hours. The mixture was then stirred at 100°C for 8 hours and cooled to room temperature (23°C) to obtain a reaction solution of a (meth)acrylic resin (A2-2) having an ethylenically unsaturated group (weight average molecular weight (Mw): 400,000, glass transition temperature (Tg): -35°C, acid value: 15.67 mgKOH / g, hydroxyl value: 65.72 mgKOH / g, ethylenically unsaturated group equivalent: 853.61 g / mol).
[0264] [Comparative Synthesis Example 1: Production of (meth)acrylic Resin (cA2-1) Having Ethylenically Unsaturated Group]
[0265] A mixed solution containing a monomer group (M1) consisting of 5 parts by mass (6.63 mol) of methyl methacrylate, 50 parts by mass (51.79 mol) of n-butyl acrylate, 25 parts by mass (18.01 mol) of 2-ethylhexyl acrylate, 19 parts by mass (21.73 mol) of 2-hydroxyethyl acrylate and 1 part by mass (1.84 mol) of acrylic acid, and 0.1 parts by mass of 2,2'-azobis(isobutyronitrile) as a radical polymerization initiator was prepared.
[0266] In a four-necked flask equipped with a stirrer, a dropping funnel, a cooling tube and a nitrogen inlet tube, 175.6 parts by mass of butyl acetate as a solvent was placed, and the temperature was raised to 80°C under a nitrogen atmosphere. The reaction temperature was maintained at 80°C±2°C, and the mixed solution was uniformly dripped in the four-necked flask over 4 hours. After the dripping was completed, the polymerization was further carried out by stirring at 80°C±2°C for 6 hours. Next, the temperature of the reactant was lowered to 60°C, and a mixed solution of 20 parts by mass (17.12 mol) of 2-isocyanate ethyl methacrylate, 0.1 parts by mass of dibutyltin laurate as a urethanization catalyst, and 200 parts by mass of ethyl acetate was dripped through a dropping funnel. After the addition is completed, the reaction system is maintained at 70°C for 4 hours to eliminate the isocyanate group, thereby obtaining a reaction solution of a (methyl) acrylic resin (cA2-1) having an ethylenically unsaturated group (weight average molecular weight (Mw): 400,000, glass transition temperature (Tg): -25°C, acid value: 6.48 mgKOH / g, hydroxyl value: 16.22 mgKOH / g, ethylenically unsaturated group equivalent: 931.68 g / mol).
[0267] Table 1
[0268]
[0269] *1 Parts by mass relative to 100 parts by mass of monomer
[0270] Table 2
[0271] *3 Parts by mass relative to 100 parts by mass of monomer
[0272] *2 Number of moles relative to 100 moles of monomer
[0273] (Production of Intermediate Layer (X1-1) Before Curing)
[0274] Ethyl acetate was added as a diluent to a reaction solution containing a (meth) acrylic resin (A1-1) having no ethylenically unsaturated group obtained in Synthesis Example 1 (referred to simply as resin (A1-1)) to obtain a resin (A1-1) solution having a content of 30% by mass of the resin (A1-1). The resin (A1-1) solution was used to obtain a resin composition (X1) for an intermediate layer according to the method shown below.
[0275] In a room shielded from active lines, a (meth) acrylic resin (A1-1) not having an ethylenically unsaturated group and HX as a crosslinking agent (B1) were added in a plastic container in the amounts (parts by mass) shown in Table 3 and stirred to obtain a resin composition (X1) for an intermediate layer. The numerical value of the (meth) acrylic resin (A1) not having an ethylenically unsaturated group (also referred to as resin (A1)) in Table 3 is the solid content of the resin (A1) solution when the content of the resin (A1) is 30% by mass, that is, the amount (parts by mass) of the resin (A1). The numerical value of the crosslinking agent (B1) is the amount (parts by mass) of the resin (A1) relative to 100 parts by mass.
[0276] The resin composition (X1) is directly applied to the substrate so that the film thickness after thermal curing can be 125 μm, and the intermediate layer (X1-1) before curing is formed by heating and drying at 100°C for 5 minutes. Then, a release sheet is attached to the intermediate layer (X1-1) before curing. A polyamide (PA) film (EX-25, Unitika Co., Ltd.) with a thickness of 25 μm is used as a substrate. A polyethylene terephthalate (PET) film (E5100, Higashiyama Film Co., Ltd.) with a thickness of 25 μm is used as a release sheet. In addition, the film thickness after thermal curing is measured by curing the intermediate layer (X1-1) before curing in an oven at 40°C for 3 days.
[0277] (Production of Intermediate Layer (X1-2) Before Curing)
[0278] The film thickness after thermal curing was set at 35 μm, and a polyethylene terephthalate (PET) film (E5107, Higashiyama Film Co., Ltd.) with a thickness of 25 μm was used as the substrate. In addition, the pre-curing intermediate layer (X1-2) bonded with a peeling sheet was obtained in the same manner as the preparation of the pre-curing intermediate layer (X1-1), and the film thickness after thermal curing was further measured.
[0279] (Production of Intermediate Layer (X2-1) Before Curing)
[0280] Resin composition (X2) was obtained in the same manner as in the manufacture of resin composition (X1) except that the raw materials and blending amounts described in Table 3 were used. A pre-cured intermediate layer (X2-1) to which a release sheet was attached was obtained in the same manner as in the manufacture of pre-cured intermediate layer (X1-1) except that resin composition (X2) was used instead of resin composition (X1), and the film thickness after thermal curing was further measured.
[0281] (Production of Intermediate Layer (X2-2) Before Curing)
[0282] The pre-curing intermediate layer (X2-2) with a bonded peeling sheet was obtained in the same manner as the pre-curing intermediate layer (X2-1), except that the film thickness after thermal curing was set to 90 μm and a polyethylene terephthalate (PET) film (E5107, Higashiyama Film Co., Ltd.) with a thickness of 25 μm was used as the substrate, and the film thickness after thermal curing was further measured.
[0283] (Production of Intermediate Layer (X2-3) Before Curing)
[0284] The pre-curing intermediate layer (X2-3) with a bonded release sheet was obtained in the same manner as the pre-curing intermediate layer (X2-1), except that the film thickness after thermal curing was set to 80 μm and a polyethylene naphthalate (PEN) film (TheonexQ51, Toyobo Co., Ltd.) with a thickness of 25 μm was used as the substrate, and the film thickness after thermal curing was further measured.
[0285] (Manufacturing of the middle layer (X3))
[0286] On a polyamide (PA) film (EX-25, Unitika Co., Ltd.) having a thickness of 25 μm, an ethylene / vinyl acetate copolymer (melting point 70°C, product name: Evaflex (trademark) EV150, Mitsui Dow Polychemical Co., Ltd.) was extruded and film-formed to a thickness of 125 μm using a uniaxial extruder (uniaxial extruder, Technovel Co., Ltd.) to form an intermediate layer (X3). A release sheet (a 25 μm polyethylene terephthalate (PET) film (E7006, Higashiyama Film Co., Ltd.)) was attached to the intermediate layer (X3) thus formed.
[0287] Table 3 (values are in parts by mass)
[0288]
[0289] (Manufacturing of Adhesive Layer (Y1-1) Before Curing)
[0290] Ethyl acetate was added as a diluent solvent to a reaction solution containing the (meth) acrylic resin (A2-1) having an ethylenically unsaturated group obtained in Synthesis Example 2 (sometimes simply referred to as resin (A2-1)), thereby obtaining a resin (A2-1) solution having a content of 30% by mass of the resin (A2-1). The resin (A2-1) solution was used to obtain an adhesive composition (Y1) for an adhesive layer by the method shown below.
[0291] In a plastic container in a room shielded from active lines, a (meth) acrylic resin (A2-1) having an ethylenically unsaturated group, KF-105 as a crosslinking agent (B2), and TPO as a photopolymerization initiator (C) are added in the amounts (parts by mass) shown in Table 4 and stirred to obtain an adhesive composition (Y1) for an adhesive layer.
[0292] The numerical values of the (meth)acrylic resin (A2) having an ethylenically unsaturated group (sometimes simply referred to as resin (A2)) in Table 4 are the solid content of the resin (A2) solution having a content of 30% by mass of the resin (A2), that is, the amount (parts by mass) of the resin (A2) used. The numerical values of the crosslinking agent (B2) and the photopolymerization initiator (C) are the amounts (parts by mass) blended per 100 parts by mass of the resin (A2).
[0293] The adhesive composition (Y1) is directly applied to the release sheet until the film thickness after thermal curing can become 25 μm, and the adhesive layer (Y1-1) before curing is formed by heating and drying at 100°C for 2 minutes. Then, a release sheet is attached to the adhesive layer (Y1-1) before curing. A polyethylene terephthalate (PET) film (E7006, Higashiyama Film Co., Ltd.) with a thickness of 25 μm is used as the release sheet. In addition, the film thickness after thermal curing is measured by curing the adhesive layer (Y1-1) before curing in an oven at 40°C for 3 days.
[0294] (Manufacturing of Adhesive Layer (Y1-2) Before Curing)
[0295] A pre-cured adhesive layer (Y1-2) to which a release sheet was bonded was obtained in the same manner as in the preparation of the pre-cured adhesive layer (Y1-1) except that the film thickness after thermal curing was set to 15 μm, and the film thickness after thermal curing was further measured.
[0296] (Manufacturing of Adhesive Layer (Y1-3) Before Curing)
[0297] A pre-cured adhesive layer (Y1-3) to which a release sheet was bonded was obtained in the same manner as in the production of the pre-cured adhesive layer (Y1-1) except that the film thickness after thermal curing was set to 10 μm, and the film thickness after thermal curing was further measured.
[0298] (Manufacturing of Adhesive Layer (Y1-4) Before Curing)
[0299] The adhesive composition (Y1) obtained by manufacturing the adhesive layer (Y1-1) before curing is directly applied to a polyamide (PA) film (EX-25, Unitika Co., Ltd.) with a thickness of 25 μm, so that the film thickness after thermal curing can be 150 μm, and the adhesive layer (Y1-4) before curing is formed by heating and drying at 100°C for 2 minutes. Then, a release sheet is attached to the adhesive layer (Y1-4) before curing. A polyethylene terephthalate (PET) film (E7006, Higashiyama Film Co., Ltd.) with a thickness of 25 μm is used as a release sheet. In addition, the film thickness after thermal curing is measured by curing the adhesive layer (Y1-4) before curing in an oven at 40°C for 3 days.
[0300] (Manufacturing of Adhesive Layer (Y2-1) Before Curing)
[0301] An adhesive composition (Y2) was obtained in the same manner as the adhesive composition (Y1) except that the raw materials and the blending amounts described in Table 4 were used. A pre-cured adhesive layer (Y2-1) to which a release sheet was attached was obtained in the same manner as the pre-cured adhesive layer (Y1-1) except that the adhesive composition (Y2) was used instead of the adhesive composition (Y1), and the film thickness after thermal curing was further measured.
[0302] (Manufacturing of Adhesive Layer (Y2-2) Before Curing)
[0303] A pre-cured adhesive layer (Y2-2) to which a release sheet was bonded was obtained in the same manner as in the production of the pre-cured adhesive layer (Y2-1) except that the film thickness after thermal curing was set to 20 μm, and the film thickness after thermal curing was further measured.
[0304] (Manufacturing of Adhesive Layer (Y2-3) Before Curing)
[0305] A pre-cured adhesive layer (Y2-3) to which a release sheet is bonded is obtained in the same manner as the pre-cured adhesive layer (Y1-4), except that the adhesive composition (Y2) obtained in the production of the pre-cured adhesive layer (Y2-1) is used in place of the adhesive composition (Y1), and the film thickness after thermal curing is further measured.
[0306] (Manufacturing of Adhesive Layer (Y3) Before Curing)
[0307] An adhesive composition (Y3) was obtained in the same manner as the production of the adhesive composition (Y1) except that the raw materials and the blending amounts described in Table 4 were used. A pre-cured adhesive layer (Y3) to which a release sheet was attached was obtained in the same manner as the production of the pre-cured adhesive layer (Y1-1) except that the adhesive composition (Y3) was used instead of the adhesive composition (Y1), and the film thickness after thermal curing was further measured.
[0308] Table 4 (values are in parts by mass)
[0309]
[0310] [Example 1] (Manufacturing of protective sheet for semiconductor processing)
[0311] The release sheet was peeled off from the pre-curing intermediate layer (X1-1) to which the release sheet was attached, and the release sheet was peeled off from one side of the pre-curing adhesive layer (Y1-1) to which the release sheet was attached, and the exposed surfaces were attached face to face. Then, the pre-curing intermediate layer (X1-1) and the pre-curing adhesive layer (Y1-1) were cured in an oven at 40° C. for 3 days, and the semiconductor processing protective sheet of Example 1 was obtained by cross-linking and curing.
[0312] [Examples 2 to 7, Comparative Example 4]
[0313] A protective sheet for semiconductor processing was obtained in the same manner as in Example 1 except that the pre-curing intermediate layer and the pre-curing adhesive layer described in Table 5 were used.
[0314] [Comparative Example 1]
[0315] The uncured adhesive layer (Y1-4) was aged in an oven at 40° C. for 3 days to crosslink and cure the uncured adhesive layer (Y1-4), thereby obtaining a semiconductor processing protective sheet of Comparative Example 1.
[0316] [Comparative Example 2]
[0317] The pre-cured adhesive layer (Y2-3) was cured by crosslinking the pre-cured adhesive layer (Y2-3) in an oven at 40° C. for 3 days, thereby obtaining a semiconductor processing protective sheet of Comparative Example 2.
[0318] [Comparative Example 3]
[0319] The release sheet was peeled off from the intermediate layer (X3) of the release sheet, and the release sheet was peeled off from one side of the pre-curing adhesive layer (Y1-1) of the release sheet, and the exposed surfaces were bonded to face each other. Thereafter, the pre-curing adhesive layer (Y1-1) was cross-linked and cured in an oven at 40°C for 3 days to obtain a semiconductor processing protective sheet of Comparative Example 3.
[0320] The obtained semiconductor processing protective sheet was evaluated for the following items by the following methods. The results are shown in Table 5.
[0321] [Peel strength before UV irradiation]
[0322] The semiconductor processing protective sheet was cut into a size of 25 mm in length and 100 mm in width, and the adhesive layer was exposed after peeling off the release sheet. Next, the semiconductor processing protective sheet was attached to a glass plate so that the exposed adhesive layer (measurement surface) was in contact with the glass plate, and a 2 kg coating roller (width: about 50 mm) was moved back and forth once to obtain a sample for measuring the peel strength before UV irradiation.
[0323] The obtained test sample was placed in an environment of temperature 23°C and humidity 50% for 24 hours. Thereafter, a tensile test was performed in a 180° direction at a peeling speed of 300 mm / min in an environment of temperature 23°C and humidity 50% using a tensile tester (texture analyzer, Eiko Seiki Co., Ltd.) in accordance with JIS Z0237:2009 to measure the peel strength (N / 25 mm) of the adhesive sheet to the glass plate.
[0324] [Peel strength after UV irradiation]
[0325] A sample similar to the sample for measuring the peel strength before UV irradiation was prepared and irradiated from the side of the semiconductor processing protective sheet at a dose of 1000 mJ / cm 2 The samples were irradiated with ultraviolet light (UV) under the conditions of , and the peel strength after UV irradiation was measured. For UV irradiation, a conveyor type ultraviolet irradiation device (iGraphics Co., Ltd., 2KW lamp, 80W / cm) was used.
[0326] The peel strength (N / 25 mm) of the pressure-sensitive adhesive sheet with respect to the glass plate was measured for the obtained measurement sample in the same manner as in the "peel strength before UV irradiation".
[0327] [Step filling ability: Installation steps]
[0328] The peeling sheet of the protective sheet for semiconductor processing is peeled off to expose the adhesive layer. Next, the exposed adhesive layer is bonded to a PCB with bumps (bump diameter φ = 20 μm, distance between bumps 30 μm, bump height 45, 80, 100 or 120 μm) using a chip mounter (Hugle Electronic Products Co., Ltd., HS7800) at 40°C for 5 minutes to obtain a sample for the step test. The sample is observed with an optical microscope from the side of the protective sheet for semiconductor processing, and the area of mixed bubbles is evaluated as "excellent" when it is less than 1% of the entire PCB with bumps, "good" when it is greater than 1% and less than 10%, and "poor" when it is more than 10%, thereby evaluating the step burying property (installation step).
[0329] [Step Burying: Cutting Steps]
[0330] The step test sample obtained in the installation step was cut with a blade (SDC200 R100NMR, kerf width: 0.3mm, blade rotation number: 28000rpm, cutting speed: 30mm / sec, cutting depth: 100μm, Tokyo Seimitsu Co., Ltd.) to obtain a small piece of step test sample. 2 UV is irradiated under the conditions of , so that the adhesive layer is partially cured. As UV irradiation, a conveyor type ultraviolet irradiation device (iGraphics Co., Ltd., 2KW lamp, 80W / cm) is used. The sample after UV irradiation is observed with an optical microscope from the side of the protective sheet for semiconductor processing. When the area mixed with bubbles is less than 1% of the entire PCB with bumps, it is evaluated as "excellent", when it is greater than 1% and less than 10%, it is evaluated as "good", and when it is more than 10%, it is evaluated as "poor", thereby evaluating the step burying property (cutting step).
[0331] [Step Burying Properties: Heating Steps]
[0332] The small-piece test sample obtained in the dicing step was heat treated for 2 hours at 200°C. After cooling the sample, it was observed with an optical microscope from the side of the semiconductor processing protective sheet. When the area mixed with bubbles was less than 1% of the entire PCB with bumps, it was evaluated as "excellent", when it was greater than 1% and less than 10%, it was evaluated as "good", and when it was more than 10%, it was evaluated as "poor", thereby evaluating the step embedding property (heating step).
[0333] [Glue residue]
[0334] The step test sample that was heat-treated in the heating step and was cut into small pieces was heated from the side of the semiconductor processing protective sheet at 1000 mJ / cm2 UV was irradiated under the conditions of , so that the adhesive layer was completely cured. As UV irradiation, a conveyor type ultraviolet irradiation device (iGraphics Co., Ltd., 2KW lamp, 80W / cm) was used. Then, the protective sheet for semiconductor processing was peeled off, and the surface of the sheet with the PCB with bumps attached was observed with an optical microscope. When no residual glue was seen at all, it was evaluated as "excellent", when less than 10% of the total area of the paste was attached, it was evaluated as "good", and when more than 10% of the paste was attached, it was evaluated as "poor", and the residual glue was evaluated in this way.
[0335] [Substrate damage]
[0336] The step test samples obtained in the dicing step were subjected to a heat treatment at 200° C. for 2 hours. The condition of the substrate after the heat treatment was confirmed, and when no damage (cracks, holes, and warping) of the substrate was observed, it was evaluated as "excellent", when less than 5% of the entire area of the substrate was observed, it was evaluated as "good", and when more than 5% of the substrate was observed, it was evaluated as "poor", and the substrate damage was evaluated in this way.
[0337]
[0338]
[0339] In Examples 1 to 7, for bumps of all heights, the step-difference burying property was excellent or good, and the residual adhesive was excellent. On the other hand, in Comparative Examples 1 and 2 without an intermediate layer, the step-difference burying property deteriorated as the bump height increased. In Comparative Examples 3 and 4, the step-difference burying property was excellent or good, but the residual adhesive was all poor.
[0340] Industrial Availability
[0341] The present disclosure provides a semiconductor processing protective sheet that can accurately follow the surface irregularities and adhere even when the unevenness (bump height) of the adherend surface is large or when the adherend undergoes a high temperature treatment step such as 200°C.
[0342] Description of the accompanying drawings
[0343] 12: Base material
[0344] 14: Middle layer
[0345] 16: Adhesive layer
[0346] 18: Peel sheet
[0347] 10: Protective sheet for semiconductor processing
Claims
1. A protective sheet for semiconductor processing, comprising a substrate, and an intermediate layer and an adhesive layer sequentially provided on one main surface of the substrate, The intermediate layer is a cured product of a resin composition containing a (meth)acrylic resin (A1) having no ethylenically unsaturated group and a crosslinking agent (B1). The adhesive layer is a cured product of an adhesive composition containing a (meth)acrylic resin (A2) having an ethylenically unsaturated group, a crosslinking agent (B2) and a photopolymerization initiator (C). The (meth)acrylic resin (A1) having no ethylenically unsaturated group has a plurality of functional groups that react with the functional groups of the crosslinking agent (B1). The (meth)acrylic resin (A2) having an ethylenically unsaturated group has a plurality of functional groups that react with the functional groups of the crosslinking agent (B2). The (meth)acrylic resin (A2) having an ethylenically unsaturated group is an adduct of an ethylenically unsaturated compound (a2-3) having an epoxy group to a copolymer of a monomer group (M2) containing an alkyl (meth)acrylate (a2-1) and an ethylenically unsaturated compound (a2-2) having a carboxyl group.
2. The protective sheet for semiconductor processing according to claim 1, wherein the thickness of the intermediate layer is 30 to 600 μm, the thickness of the adhesive layer is 5 to 100 μm, and the ratio of the thickness of the intermediate layer to the adhesive layer, i.e., intermediate layer / adhesive layer, is 1 to 50. 3 . The protective sheet for semiconductor processing according to claim 1 , wherein the (meth)acrylic resin (A1) having no ethylenically unsaturated group has a glass transition temperature (Tg) of −80 to 0° C.
4. The protective sheet for semiconductor processing according to claim 1 or 2, wherein the (meth)acrylic resin (A1) having no ethylenically unsaturated group is a copolymer of a monomer group (M1) containing an alkyl (meth)acrylate (a1-1) and a (meth)acrylate having a hydroxyl group (a1-2), The crosslinking agent (B1) is an isocyanate crosslinking agent. 5 . The protective sheet for semiconductor processing according to claim 4 , wherein the monomer group (M1) further comprises an ethylenically unsaturated compound (a1-3) having a carboxyl group. 6 . The protective sheet for semiconductor processing according to claim 4 , wherein the monomer group (M1) further comprises a (meth)acrylamide compound.
7. The protective sheet for semiconductor processing according to claim 1 or 2, wherein the glass transition temperature (Tg) of the (meth)acrylic resin (A2) having an ethylenically unsaturated group is -80 to 0°C. 8 . The protective sheet for semiconductor processing according to claim 1 , wherein the (meth)acrylic resin (A2) having an ethylenically unsaturated group has an ethylenically unsaturated group equivalent of 100 to 4000 g / mol. 9 . The protective sheet for semiconductor processing according to claim 1 , wherein the crosslinking agent (B2) is an epoxy crosslinking agent.
10. A method for manufacturing a semiconductor device having a bump electrode, comprising the following steps: A protective step of laminating the adhesive layer of the semiconductor processing protective sheet according to claim 1 or 2 to a surface of a semiconductor device having bump electrodes, an active energy ray irradiation step of irradiating the semiconductor processing protective sheet with active energy rays to photocure the adhesive layer, A step of heating a semiconductor device to which the protective sheet for semiconductor processing is attached, and The step of peeling off the semiconductor processing protection sheet from the surface with the bump electrodes. 11 . The method for manufacturing a semiconductor device according to claim 10 , wherein, when a height of the bump electrode in μm is denoted as H and a total thickness of the intermediate layer and the adhesive layer in μm is denoted as d, d / H is 0.40 to 110.
12. The method for manufacturing a semiconductor device according to claim 10, wherein the highest reaching temperature in the heating step is 100 to 230°C.