Light-emitting element and manufacturing method thereof
By adopting a linearly symmetric hexagonal shape with a symmetry axis and the use of bonding materials, the problems of high installation cost and low space utilization of micro LEDs are solved, and higher wafer yields and lower Production cost.
Patent Information
- Application Number
- CN202380036487.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the installation cost of micro LEDs is high and the space utilization rate of rectangular grains is not high, resulting in a high unit price per LED, making it difficult to effectively improve the component yield of the wafer.
Using a linearly symmetric hexagonal shape light emitting element design with a symmetry axis, by forming isolation grooves on the light emitting layer and bonding the translucent substrate to the epitaxial layer with bonding materials, the starting substrate is removed and each crystal is improved. Round light emitting element yield.
Through this design, the yield of light emitting elements per wafer is improved, and short circuits caused by position shift are suppressed during installation, reducing the overall area of the light emitting elements, thereby reducing production costs.
Smart Images

Figure CN119032430A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light emitting element and a method for manufacturing the same. Background Art
[0002] There are two types of displays using tiny light-emitting diodes (micro-LEDs): a monochrome display achieved by microfabrication of a single-color micro-LED, and a full-color display achieved by separately shifting RGB LEDs from a donor substrate.
[0003] In the past, the cost of relocating RGB chips to achieve full-color display was high, which has become the reason for the increase in manufacturing costs of micro LED displays.
[0004] In recent years, the EZ-PETAMP series, SQDP series, SQDP-G series, and SQRP series manufactured by Shin-Etsu Chemical Co., Ltd. have been developed, which can significantly reduce installation costs by adhering the chip to a donor substrate having a silicone film formed on synthetic quartz, and irradiating the interface between the starting substrate and the epitaxial layer with ultraviolet laser to sublimate the interface, thereby transferring the micro-LED from the starting substrate to the donor substrate for installation.
[0005] However, although this method is effective for, for example, a GaN-based LED formed on a sapphire substrate, it cannot be applied to, for example, an AlGaInP-based LED formed on a GaAs substrate.
[0006] In order to achieve displacement by the above-mentioned EZ-PETAMP, a technique is required in which the starting substrate is removed after the epitaxial functional layer is bonded to the permanent substrate to achieve displacement.
[0007] Patent Document 1 discloses a technique of thermally pressing a semiconductor epitaxial substrate and a temporary supporting substrate via a dielectric layer, and a technique of separating a temporary supporting substrate from an epitaxial functional layer by wet etching.
[0008] By bonding the sapphire substrate and the LED device portion with a bonding material (adhesive) such as benzocyclobutene (BCB), it is possible to implement the same process as the structure in which a GaN-based LED is formed on a sapphire substrate (EZ-PETAMP).
[0009] By combining GaN LEDs and AlGaInP LEDs, pixels capable of RGB color display can be formed. When using RGB light-emitting elements to form a display device, multiple LEDs need to be installed. In order to suppress the overall cost, it is crucial to minimize the material cost per die.
[0010] Although as mentioned above, Patent Document 1 discloses a technology for hot pressing a semiconductor epitaxial substrate and a temporary supporting substrate through a dielectric layer, and a technology for separating the temporary supporting substrate from the epitaxial functional layer by wet etching, it does not involve a technology for the optimal device form of a micro-LED joined by a BCB layer, etc., and the prior art does not disclose a technology for reducing the material cost of the LED itself.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2021-27301
[0014] Patent Document 2: Japanese Patent Application Publication No. 2017-17163
[0015] Patent Document 3: Japanese Patent Application Publication No. 2000-164930
[0016] Patent Document 4: Japanese Patent Application Publication No. 2006-135309
[0017] Patent Document 5: Japanese Patent Application Publication No. 2016-164970
[0018] Patent Document 6: Japanese Patent Application Publication No. 2016-207870 Summary of the invention
[0019] 1. Technical issues to be resolved
[0020] Although the installation cost of micro-LEDs can be reduced through the above-mentioned EZ-PETAMP process, the unit price of each micro-LED still needs to be reduced. However, the space utilization rate of conventional rectangular grains is not high. As long as a rectangular grain shape is selected, when the light-emitting area is defined as fixed, the theoretical number of grains obtained from the wafer is uniquely determined. The reason is that when forming an LED for installation accompanied by a displacement process, the component will move in the vertical direction during displacement, so a gap (isolation width between components) that matches the tolerance of the movement is required between the LED components. The area including the isolation width between components is the area required for the actual component. As long as the isolation width between components cannot be set to zero, the area of the LED component itself and the area including the isolation width between components become the area required to form the component.
[0021] As a technique for minimizing the isolation width between elements, a technique using a close-packed structure based on a regular hexagon is disclosed as shown in Patent Document 2. However, the regular hexagonal shape is not sufficient as a crystal shape of a micro LED that is moved and mounted.
[0022] In particular, when transferring micro-LEDs, since the grain size is small (e.g., less than 100 μm), component connection techniques based on wire bonding are not used. Although bumps are sometimes used, flip-chip mounting is usually implemented, in which electrodes formed on the LED element are directly electrically coupled to electrodes on the mounting substrate.
[0023] In the case of flip-chip mounting, the form of forming two electrodes with different polarities on the top surface is the easiest to mount, so it is a commonly used form. However, since the mounting position tolerance cannot be zero during displacement, a μm-level mounting tolerance is required. Since electrodes with different polarities are formed on the same surface, the greater the distance between them, the greater the mounting tolerance that can be achieved. Based on the above requirements, as shown in Patent Document 3, a rectangular shape is required for micro-LEDs.
[0024] However, in the case of a circle, square, regular hexagon, or other regular polygon, it is impossible to obtain a spacing distance greater than the size of the outer edge of the grain. As shown in Patent Document 4, Patent Document 5, Patent Document 6, etc., in order to obtain the greatest possible spacing distance, a technology is disclosed in which the electrode is configured close to the outer edge. However, compared to the grain size, the pad electrode portion is too small. In order to obtain ohmic contact, when the resistance in the electrode / interface is fixed, if the area is not greater than a certain level, the ohmic resistance will not drop to an operational level. The electrode area disclosed in the prior art is significantly smaller. If directly applied to micro-LEDs, the ohmic contact resistance will become too large, and the micro-LEDs formed according to the prior art will not function properly.
[0025] From the above perspectives, for micro LEDs, it is believed that the best design is to adopt a rectangular grain shape as shown in Patent Document 3 and to provide electrodes at the ends in the long axis direction.
[0026] However, for this design, when the element area is determined, there is no other method to improve the yield of the number of grains that can be manufactured from one wafer except reducing the isolation width between the elements. If the isolation width between the elements is reduced, the yield during movement and installation will decrease. Therefore, the method of improving the yield by reducing the isolation width between the elements required for movement and displacement is limited, and the prior art does not disclose a method for further improving the yield.
[0027] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a method for manufacturing a light emitting element that does not reduce the yield during movement and mounting, thereby improving the yield of elements per wafer.
[0028] (II) Technical solution
[0029] The present invention is completed in order to achieve the above-mentioned purpose. The present invention provides a method for manufacturing a light-emitting element, which is a method for manufacturing a light-emitting element for manufacturing a plurality of light-emitting elements, and comprises: a step of growing an epitaxial layer including a light-emitting layer on a starting substrate, and a step of forming an isolation groove for forming an element on the light-emitting layer. The method for manufacturing a light-emitting element is characterized in that the top view shape of each of the plurality of light-emitting elements to be manufactured is set to a line-symmetric hexagon having an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°, the plurality of light-emitting elements to be manufactured are isolated by the isolation groove of a specified width, and the isolation groove is formed in a manner in which the plurality of light-emitting elements are arranged without gaps across the isolation groove.
[0030] By using the above-mentioned method for manufacturing a light-emitting element, a light-emitting element can be manufactured, wherein the top view shape of the light-emitting element is a line-symmetrical hexagon, wherein the hexagon has a side parallel to the axis of symmetry, the length of the parallel side is longer than the other sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°. Thus, compared with a light-emitting element having a rectangular top view shape, the yield of the light-emitting element per wafer can be further improved.
[0031] In this case, after the step of growing the epitaxial layer, the method may further include the step of bonding a light-transmitting substrate to the epitaxial layer via a bonding material and removing the starting substrate.
[0032] In particular, when the starting substrate is not a light-transmitting substrate, by transferring the epitaxial layer to the light-transmitting substrate in the above manner, it is applicable to a technology based on the premise that the technology is implemented on a substrate having a light-emitting element formed on a light-transmitting substrate.
[0033] Furthermore, the two vertex angles can be set to be greater than or equal to 90° and less than or equal to 120°.
[0034] By setting the vertex angle to be within the above range, the yield of light-emitting elements per wafer can be further improved.
[0035] Furthermore, the distance between the two sides parallel to the symmetry axis can be set to 1 μm or more and 100 μm or less.
[0036] The present invention is particularly effective when manufacturing such a micro-LED having parallel sides with a distance between the sides being 1 to 100 μm.
[0037] Furthermore, the isolation trench is preferably formed by an inductively coupled plasma dry etching method.
[0038] The formation of the isolation trenches by the inductively coupled plasma dry etching method can be easily performed with good accuracy.
[0039] Furthermore, it is preferable that the light-transmitting substrate be any one of sapphire, quartz and glass.
[0040] In addition, as the light-transmitting substrate, any of these substrates can be appropriately used, and in particular, a substrate having high transmittance to laser light can be selected.
[0041] Furthermore, the bonding material may be at least any one of benzocyclobutene, fluororesin, and epoxy resin.
[0042] As the bonding material, these bonding materials can be used appropriately.
[0043] In addition, the present invention provides a light-emitting element, characterized in that its top view shape is a line-symmetrical hexagon having an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°.
[0044] This light-emitting element can increase the area ratio of the light-emitting layer, that is, the ratio of the area of the light-emitting layer to the overall area of the element, by forming the electrode in the triangular portion of the hexagon that includes the top through which the axis of symmetry passes. By making the length of the parallel sides longer than the other sides, short circuits caused by positional displacement during installation can be suppressed.
[0045] In this case, the light emitting element may be bonded to the light-transmitting substrate via a bonding material.
[0046] As described above, if the light-emitting element is bonded to the light-transmitting substrate via a bonding material, it can be applied to a technology based on a substrate in which the light-emitting element is formed on the light-transmitting substrate.
[0047] Furthermore, it is preferable that the two vertex angles are not less than 90° and not more than 120°.
[0048] By setting the vertex angle within the above range, the area ratio of the light-emitting layer, that is, the ratio of the area of the light-emitting layer to the entire area of the element can be further increased.
[0049] Furthermore, the distance between the two sides parallel to the symmetry axis can be set to be greater than or equal to 1 μm and less than or equal to 100 μm.
[0050] The present invention is particularly effective when applied to a micro-LED having parallel sides with a distance of 1 to 100 μm.
[0051] Preferably, the light-transmitting substrate is any one of sapphire, quartz and glass.
[0052] As the light-transmitting substrate, any of these substrates can be appropriately used, and in particular, a substrate can be selected so as to increase the transmittance to laser light.
[0053] Furthermore, it is preferable that the bonding material is at least any one of benzocyclobutene, fluororesin, and epoxy resin.
[0054] As the bonding material, these bonding materials can be used appropriately.
[0055] (III) Beneficial effects
[0056] By the manufacturing method of the light-emitting element of the present invention, a light-emitting element can be manufactured, and its top view shape is a line-symmetrical hexagon, wherein the hexagon has a side parallel to the axis of symmetry, the length of the parallel side is longer than the other sides, and the two vertex angles through which the axis of symmetry passes are 90° or more and less than 180°. Thus, compared with the case of a rectangle, the yield of the light-emitting element per wafer can be further improved. In addition, by making the length of the parallel side longer than the other sides, the short circuit caused by positional offset can be suppressed during installation. In addition, as long as the vertex angle is more than 90°, the mechanical strength of the top of the triangular shape can be prevented from weakening, and cracking in the triangular portion can be suppressed.
[0057] In addition, the light-emitting element of the present invention can increase the area ratio of the light-emitting layer, that is, the ratio of the area of the light-emitting layer to the overall area of the element, by forming the electrode in the triangular portion of the hexagon that includes the top through which the symmetry axis passes. By making the length of the parallel sides longer than the other sides, short circuits caused by positional deviations can be suppressed during installation. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 It is a schematic cross-sectional view showing a part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0059] Figure 2 It is a schematic cross-sectional view showing another part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0060] Figure 3 It is a schematic cross-sectional view showing another part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0061] Figure 4 It is a schematic cross-sectional view showing another part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0062] Figure 5 1 is a schematic plan view showing the shape of one light-emitting layer in the first embodiment of the method for producing a light-emitting element of the present invention.
[0063] Figure 6It is a schematic plan view showing various parts of one light-emitting layer in the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0064] Figure 7 It is a schematic plan view showing a state where a plurality of light-emitting layers are arranged in the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0065] Figure 8 1 is a schematic plan view showing the arrangement position of a contact pad in the shape of one light-emitting layer in the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0066] Fig. 9 It is a schematic cross-sectional view showing another part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0067] Fig.10 It is a schematic cross-sectional view showing another part of the first embodiment of the method for manufacturing a light-emitting element of the present invention.
[0068] Fig.11 Schematic diagram showing a state where a plurality of light emitting elements of the present invention are displaced.
[0069] Fig.12 1 is a schematic plan view showing the shape of a light emitting element used in a comparative example.
[0070] Fig.13 1 is a schematic plan view showing the arrangement positions of contact pads in the shape of a light emitting element used in a comparative example. DETAILED DESCRIPTION
[0071] Hereinafter, the present invention will be described in detail, but the present invention is not limited to these descriptions.
[0072] As described above, a method for manufacturing a light emitting element that can improve the yield of elements per wafer without reducing the yield during movement and mounting is required.
[0073] The inventors of the present invention have repeatedly conducted in-depth research on the above-mentioned problems, and as a result, found that the shape of the light-emitting element is formed into a specific hexagonal shape, thereby completing the present invention. The present invention is a method for manufacturing a light-emitting element, which is a method for manufacturing a light-emitting element for manufacturing a plurality of light-emitting elements, and has: a step of growing an epitaxial layer including a light-emitting layer on a starting substrate, and a step of forming an isolation groove for forming an element on the light-emitting layer, wherein the top view shape of each of the plurality of light-emitting elements to be manufactured is set to: a line-symmetric hexagon having a symmetry axis, wherein the hexagon has two sides parallel to the symmetry axis, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the symmetry axis passes are greater than 90° and less than 180°, the plurality of light-emitting elements to be manufactured are isolated by the isolation groove of a specified width, and the isolation groove is formed in a manner that the plurality of light-emitting elements are arranged without gaps across the isolation groove.
[0074] In addition, the light-emitting element of the present invention is the following light-emitting element: a light-emitting element, characterized in that its top view shape is a line-symmetrical hexagon having an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°.
[0075] Below, while referring to the attached Figure 1 The present invention is described in detail, but the present invention is not limited to these descriptions. Below, the first embodiment and the second embodiment are exemplified to illustrate the scheme of the present invention. For similar components in each embodiment, the same symbols are marked in the drawings for description. In addition, some repeated descriptions are omitted.
[0076] (First embodiment)
[0077] First, the first embodiment is described. The first embodiment is an embodiment including the steps of growing an epitaxial layer on a starting substrate, bonding a light-transmitting substrate to the epitaxial layer via a bonding material, and removing the starting substrate.
[0078] First, if Figure 1 As shown, an epitaxial layer 18 including a light emitting layer is grown on a starting substrate 11. More specifically, it is as follows.
[0079] First, if Figure 1As shown, an etch stop layer 12 is epitaxially grown on a starting substrate 11 of a first conductivity type, for example, made of GaAs. The etch stop layer 12 can be formed by, for example, growing a first etch stop layer of GaInP of a first conductivity type, for example, to a thickness of 0.1 μm, and growing a second etch stop layer of GaAs of a first conductivity type, for example, to a thickness of 0.1 μm, after stacking a GaAs buffer layer of a first conductivity type. Further, on the etch stop layer 12, for example, a first cladding layer 13 of AlGaInP of a first conductivity type, for example, to a thickness of 1.0 μm, an active layer 14 of AlGaInP of an undoped type, for example, a second cladding layer 15 of AlGaInP of a second conductivity type, for example, to a thickness of 1.0 μm, a GaInP intermediate layer (not shown) of a second conductivity type, for example, to a thickness of 0.1 μm, and a GaP window layer 16 of a second conductivity type, for example, to a thickness of 6 μm, are sequentially grown, thereby preparing an epitaxial wafer 20 including an epitaxial layer 18. Here, the first cladding layer 13 to the second cladding layer 15 are referred to as a double heterogeneous (DH) structure ( Figure 1 ), which corresponds to the light-emitting layer. That is, the epitaxial layer 18 has a light-emitting layer. In addition, the material of the epitaxial layer 18 is not limited to these materials, as long as it is set to have the light-emitting layer (light-emitting element structure) as described above.
[0080] In the present invention, after the step of growing the epitaxial layer 18, Figure 2 , 3 The process shown further includes the following steps: bonding the light-transmitting substrate 30 to the epitaxial layer 18 via the bonding material 25, and removing the starting substrate 11. More specifically, it is as follows.
[0081] First, if Figure 2 As shown, benzocyclobutene (BCB), which is a thermosetting bonding material, is spin-coated on the epitaxial wafer 20 as the bonding material 25, and overlapped with a sapphire wafer (translucent substrate 30) as a bonding wafer to be bonded in a facing manner, and thermocompression bonding is performed, thereby manufacturing a first epitaxial bonding substrate in which the epitaxial wafer 20 and the sapphire wafer (translucent substrate 30) are bonded via BCB (bonding material 25). When BCB is applied by spin coating, the film thickness can be set to 0.6 μm, for example, but is not limited to this thickness, and can also be greater than this thickness, and the same effect can be obtained when it is thinner.
[0082] The bonding conditions at this time may be, for example, a temperature of 200° C. to 400° C., a force of 1.2 N / cm 2 The above pressure is applied and joined.
[0083] In addition, the material of the substrate to be bonded as the light-transmitting substrate 30 is not limited to sapphire, and any material can be selected as long as flatness can be ensured. In addition to sapphire, quartz, glass, etc. can also be selected.
[0084] The bonding material 25 is not limited to BCB, and fluorine resin, epoxy resin, etc. can be used. In addition, BCB is not limited to the case of coating in a layer, and photosensitive BCB can be patterned into isolated islands, lines, or other shapes and then the bonding process can be performed.
[0085] Then, if Figure 3 As shown, the starting substrate 11 (for example, a GaAs starting substrate) is removed by wet etching, and then the etch stop layer 12 is also removed. Regarding the removal of the etch stop layer 12, when there are a first etch stop layer and a second etch stop layer as described above, first, the first etch stop layer can be exposed by etching, and the etchant is switched to remove the second etch stop layer, thereby exposing the epitaxial layer 18 (the first cladding layer 13 in the epitaxial layer 18). In this way, a second epitaxial bonded substrate (DH) that only retains the double heterogeneous (DH) structure (the first cladding layer 13, the active layer 14, the second cladding layer 15) and the window layer 16 can be produced. Figure 3 ).
[0086] Next, an isolation groove 47 for forming an element is formed on the light emitting layer (see Figure 4 ). The formation of the isolation trench 47 is preferably performed by inductively coupled plasma dry etching, because it is simpler and more accurate. Figures 4 to 8 A more specific method will be described.
[0087] In this process, first, Figure 4 As shown, a pattern is formed by photolithography, and an element isolation process is performed by ICP (inductively coupled plasma). The gas used for ICP can be set to chlorine gas and argon gas. The ICP process can be performed twice: an element isolation process for exposing the layer (BCB layer) of the bonding material 25 and an exposure process for exposing the window layer 16 (GaP window layer). In addition, the formation of this isolation groove 47 is not limited to the case where the window layer 16 (GaP window layer) is exposed in the above manner ( Figure 4 ), as long as at least the active layer 14 is isolated, the same effect can be obtained even if not the window layer 16 (GaP window layer) is exposed but the second cladding layer 15 is exposed. Figure 4 18a is shown in the figure as a region where the lower layer of the light-emitting layer is exposed. Figure 4 2 shows a case where the window layer 16 is exposed as the lower layer exposed region 18 a.
[0088] In the method for manufacturing a light emitting element comprising the steps of growing an epitaxial layer 18 including a light emitting layer on a starting substrate 11 and forming an isolation groove for forming an element on the light emitting layer, the present invention sets the top view shape of each of the plurality of light emitting elements to be manufactured as follows when implementing the element isolation step (the step of forming an isolation groove for forming an element on the light emitting layer). Figures 5 to 8 The prescribed hexagonal shape shown. This hexagonal shape is a line-symmetric hexagon with an axis of symmetry, and has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°. In this case, it is preferred that the two vertex angles are set to be greater than 90° and less than 120°. In addition, in the present invention, the plurality of light-emitting elements to be manufactured are set to be isolated by an isolation groove of a prescribed width, and the isolation groove is formed in a manner that the plurality of light-emitting elements are arranged without gaps across the isolation groove (refer to Figure 7 ). If this configuration is arranged in a regular hexagon, it is similar to a configuration called a honeycomb structure.
[0089] Reference Figure 5 The plan view shape of one light emitting element will be described. Figure 5 It is through Figure 1 to Figure 4 The top view of the epitaxial layer 18 having the light emitting layer is formed by performing each step and isolating the elements by using the isolation groove 47. In the hexagonal shape, Figure 5 The area indicated by the symbol 54 is the position of the upper electrode 54 described later. Figure 5 The area indicated by the symbol 56 in FIG. 1 is the position of the lower electrode 56 described later. In addition, the triangular area around the lower electrode 56 (the area indicated by the symbol 18a divided by the dotted line in the hexagon indicated by the solid line) is Figure 4 The lower layer shown has exposed area 18a. Further, Figure 5 The dotted line outside the hexagon indicated by the solid line is the element isolation intermediate line 48. The element isolation intermediate line 48 indicates the intermediate line of the isolation trench 47 between the individual light emitting layers isolated by the element isolation. Figure 7 There are multiple Figure 5 The state of the light-emitting layer (the illustration of the exposed area 18a of the lower layer is omitted).
[0090] Further, refer to Figure 6 The shape of the light-emitting element in the present invention will be described. Figure 6 The hexagonal shape shown corresponds to Figure 5 The shape of the light-emitting layer. Figure 6The hexagonal shape shown is a line-symmetric hexagonal shape having an axis of symmetry SA. Further, the hexagonal shape has two sides (side A and side B) parallel to the axis of symmetry SA, and the length of the two parallel sides (side A and side B) is longer than the other four sides (side C, side D, side E, and side F). Furthermore, the two vertex angles (α and β) through which the axis of symmetry SA passes are greater than 90° and less than 180°.
[0091] In the present invention, further Figure 7 As shown, the light emitting elements having the hexagonal shape defined as described above are isolated by isolation trenches having a predetermined width, and the isolation trenches are formed so that a plurality of light emitting elements are arranged without any gap therebetween.
[0092] Figure 8 It is shown in Figure 5 The relationship between the positions of the light emitting elements and the contact pads 60 is shown.
[0093] By the manufacturing method of the above-mentioned light-emitting element, the above-mentioned specific hexagonal light-emitting element can be manufactured. Thus, compared with the rectangular light-emitting element, the yield of the light-emitting element per wafer can be further improved. In addition, by making the length of the parallel sides longer than the other sides, the short circuit caused by positional offset can be suppressed during installation. In addition, as long as the vertex angle is more than 90°, the mechanical strength of the top of the triangular shape can be prevented from weakening, and cracking in the triangular portion can be suppressed.
[0094] Furthermore, it is preferred that the above two vertex angles (α and β) are set to be greater than 90° and less than 120°. By setting the vertex angle to the above range, the yield of the light-emitting element per wafer can be further improved. In addition, the area ratio of the light-emitting layer, that is, the ratio of the area of the light-emitting layer to the overall area of the element, can be further improved. When the vertex angle is less than 90°, the triangular portion will protrude too much and cause a decrease in mechanical strength, so it cannot withstand the stress when electrically connected to the mounting electrode, and the protruding portion is prone to notches and cracks. If the vertex angle is above 90°, such grain breakage is not likely to occur.
[0095] The present invention is particularly effective in manufacturing a small light-emitting element, ie, a micro-LED, in which the distance between the two sides (A and B) parallel to the symmetric axis SA is set to 1 μm or more and 100 μm or less.
[0096] Preferred: In implementation Figure 1 to Figure 4 After the component isolation process is carried out, the end surface is formed as Fig. 9 The protective film 52 ( Fig. 9 As the protective film 52, for example, SiO2 can be used, but it is not limited to SiO2. Any material can be selected as long as it can protect the end face and has insulating properties. SiN xAnd titanium oxide, magnesium oxide, etc.
[0097] Then, if Fig.10 As shown, a first conductive layer (in Fig.10 The electrode (upper electrode 54) in contact with the first cladding layer 13) and the second conductive layer (in Fig.10 The electrode (lower electrode 56) in contact with the window layer 16 is subjected to heat treatment ( Fig.10 ), thereby forming an ohmic contact. For example, the first conductivity type can be set to n-type and the second conductivity type can be set to p-type for design, and a metal containing Au and Si, for example, is used as an electrode in contact with the n-type layer, and a metal containing Au and Be, for example, is used as an electrode in contact with the p-type layer. As an n-type electrode, it is not limited to metals of Au and Si, and the same result can be obtained when a metal containing Au and Ge is used. In addition, as a p-type electrode, it is not limited to metals of Au and Be, and the same result can be obtained when a metal containing Au and Zn is used.
[0098] This embodiment (first embodiment) in which the device formed with electrodes is bonded via BCB can be provided as a product for the above-mentioned EZ-PETAMP process. After the light-emitting element is bonded to the template substrate processed with a convex pattern on a synthetic quartz substrate via silicone, laser is irradiated from the bonded substrate side to sublimate the BCB and move the device from the bonded substrate to the template substrate. Then, the moved device is transferred again to the mounting substrate with a driving circuit to form an RGB display device.
[0099] When transferring to the mounting substrate, Fig.11 As schematically shown, the displacement is performed in a discrete manner in both the lateral and longitudinal directions. This is because, when forming an RGB display device, the formation pitch of the micro LEDs is usually different from the pitch on the mounting side.
[0100] (Second embodiment)
[0101] Next, the second embodiment of the present invention is described. In this embodiment, the following epitaxial wafer is prepared: on a starting substrate such as a light-transmitting sapphire, for example, a first conductive type GaN buffer layer is grown, and then a first conductive type GaN first cladding layer is grown in a thickness of 1.0 μm, an undoped InGaN active layer is grown in a thickness of 0.5 μm, and a second conductive type AlGaN second cladding layer is grown in a thickness of 6 μm, and an epitaxial wafer having a light-emitting element structure as an epitaxial functional layer is grown in sequence. Here, the first cladding layer to the second cladding layer are referred to as a DH structure portion.
[0102] Next, patterning is performed by photolithography, and element isolation and exposure are performed by ICP. This process is the same as that of the first embodiment.
[0103] After the element isolation process, the process and structure of forming a protective film as an end surface treatment are the same as those of the first embodiment.
[0104] After forming a protective film in the same manner as in the first embodiment, an electrode is formed and an ohmic contact is formed. The electrode is different from the first embodiment and uses Ti / Al / Ni / Au or the like.
[0105] Regarding the displacement method and installation method after the electrode is formed, although the operation of irradiating the laser from a translucent substrate such as a sapphire substrate is the same as the first embodiment, the following operation is different from the first embodiment: instead of sublimating BCB, the GaN buffer layer is partially sublimated and then peeled off.
[0106] Example
[0107] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0108] (Example)
[0109] First, if Figure 1 As shown, an epitaxial layer including a light-emitting layer is grown on a starting substrate. Specifically, it is as follows. First, after stacking an n-type GaAs buffer layer on an n-type GaAs starting substrate 11, an n-type GaInP first etch stop layer with a thickness of 0.1 μm and an n-type GaAs second etch stop layer with a thickness of 0.1 μm are formed, thereby forming an etch stop layer 12. An n-type AlGaInP first cladding layer 13 with a thickness of 1.0 μm, an undoped AlGaInP active layer 14, a p-type AlGaInP second cladding layer 15 with a thickness of 1.0 μm, a p-type GaInP intermediate layer with a thickness of 0.1 μm (not shown), and a p-type GaP window layer 16 with a thickness of 6 μm are sequentially grown on the etch stop layer 12, thereby preparing an epitaxial wafer 20 (light-emitting element structure) having a light-emitting layer as an epitaxial functional layer. Figure 1 ).
[0110] Then, if Figure 2 As shown, benzocyclobutene (BCB) as a bonding material 25 is spin-coated on the epitaxial wafer 20, and overlapped with a sapphire wafer as a light-transmitting substrate 30 in a manner facing each other, and the bonding material 25 is spin-coated on the epitaxial wafer 20 at 2 N / cm 2 The bonding was performed under the bonding condition of 250° C., thereby manufacturing a first epitaxial bonding substrate ( Figure 2 ). When BCB was applied by spin coating, the film thickness was set to 0.6 μm.
[0111] Then, if Figure 3 As shown, the GaAs starting substrate 11 is removed by wet etching to expose the first etch stop layer, and the etchant is switched to remove the second etch stop layer, thereby removing the etch stop layer 12. Thus, the first cladding layer 13 is exposed to produce a second epitaxial bonding substrate ( Figure 3 ).
[0112] Then, if Figure 4 As shown, a pattern is formed by photolithography, and an element isolation process is performed by ICP. The gas used for ICP is set to chlorine gas and argon gas, and the ICP process is performed twice: an element isolation process to expose the BCB layer 25 and an exposure process to expose the GaP window layer 16 ( Figure 4 ). Thus, an isolation trench 47 for forming an element is formed on the light emitting layer.
[0113] When implementing the component isolation process, such as Figure 5 to Figure 7 As shown, the top view shape of the element is set to be a line-symmetric hexagon with a symmetry axis SA, wherein the hexagon has two sides (side A and side B) parallel to the symmetry axis SA, the length of the two parallel sides (side A and side B) is longer than the other four sides (side C to side F), and the two vertex angles (α and β) passed by the symmetry axis SA are 120° ( Figure 5 to Figure 7 ).
[0114] Regarding the specific element size, the distance between the top (vertex angle α) and the top (vertex angle β) on the symmetry axis SA is 13.50 μm, the distance between the parallel sides A and B is 7.79 μm, and the area of one element in the element isolation groove 47 is 87.64 μm. 2 .
[0115] The electrodes are placed at Figure 5 The isosceles triangle portion (upper electrode 54 and lower electrode 56) within the hexagonal shape shown. Figure 5 In the area with an angle of 120 degrees ( Figure 6 The ohmic contact electrode described later is arranged adjacent to the region including the vertex angle α and the vertex angle β shown in the figure. The distance between the electrode and the outer edge of the grain depends on the tolerance during photolithography. In this embodiment, the tolerance is 0.25 μm. The ohmic contact electrode area is set to 6.93 μm 2 , the distance between the electrodes is 9.00 μm.
[0116] In this embodiment, the isolation width between elements is set to 0.87 μm. Figure 5 The dotted line corresponds to the middle line between the components (component isolation middle line 48). The area inside this dotted line is the area required for component manufacturing, which is 103.92 μm. 2, wherein the width is 8.66 μm and the distance from top to top on the symmetry axis SA is 14.50 μm.
[0117] like Figure 7 As shown, each hexagonal element is arranged, and each element has an isosceles triangle top, and the vertically arranged elements are arranged in a staggered manner. Figure 8 In FIG. 1 , the contact pad 60 is shown with the contact pad 60 disposed at Figure 5 The arrangement of the mounting substrate on the component shown in the figure. The alignment tolerance when forming the contact pad 60 is 0.25 μm, the width from the electrode end (vertical direction in the figure) is 4.00 μm, and the spacing distance between the two electrodes with different polarities is 1.00 μm.
[0118] After the element isolation process, a SiO2 protective film 52 is formed as an end surface treatment ( Fig. 9 Next, an electrode in contact with the n-type layer and an electrode in contact with the p-type layer (upper electrode 54 and lower electrode 56) are formed and heat treated to form an ohmic contact ( Fig.10 ).
[0119] (Comparative Example)
[0120] The light emitting element ( Fig.12 ).
[0121] Regarding the shape of the light-emitting element, the distance in the long axis direction is 11.25 μm, and the width in the short axis direction is 7.79 μm. The element area in the element isolation trench is 87.64 μm. 2 , the same as in the embodiment.
[0122] The distance between the electrodes (upper electrode 154 and lower electrode 156) and the outer edge of element 118 depends on the tolerance during photolithography, and the tolerance is 0.25 μm as in the embodiment. Fig.12 The lower layer exposed area 118a is also shown in FIG. As in the embodiment, the ohmic electrode area is set to 6.93 μm 2 , the distance between the electrodes is 8.75 μm.
[0123] The isolation width between the elements was set to 0.87 μm in the same manner as in the embodiment. Fig.12 The area required for making the element represented by the dotted line (element isolation middle line 148) is 104.96μm 2 , wherein the width is 8.66 μm and the major axis length is 12.12 μm. Therefore, under the same design as the embodiment, the area required for manufacturing the element in the comparative example becomes larger.
[0124] Fig.13 The contact pad 160 is shown in FIG. Fig.12 Configuration of the mounting substrate on it. The alignment tolerance when forming the contact pad 160 is 0.25μm, and the width (vertical direction in the figure) from the end of the electrode is 4.00μm, and the spacing distance between the two electrodes with different polarities is 0.75μm. The distance between the electrodes in the embodiment is 1.00μm, so under the same design as the embodiment, the spacing distance between the contact pads in the comparative example becomes smaller. If the spacing distance becomes shorter, it becomes easier to cause a short circuit due to position offset during installation, so the required alignment tolerance becomes more stringent. Therefore, it is necessary to set the spacing distance between the electrodes to be larger to match the alignment tolerance, so the grains in the comparative example must be longer in the long axis direction than the embodiment in a manner that matches the alignment tolerance. Naturally, the required grain area will also be relatively larger than that of the embodiment.
[0125] In the comparative example, although the light emitting element area is set to be the same as that in the embodiment, when matching the required tolerances for installation, it is impossible to design at the same size as the comparative example, and the grain must be longer in the long axis direction. Naturally, the area required for forming the grain needs to be designed to be larger than that in the embodiment. When the spacing distance of the contact pad is set to 1.00μm as in the embodiment, it is necessary to extend the long axis direction from 11.25μm by 0.25μm to 11.50μm. In order to achieve the same alignment as in the embodiment, the grain area required needs to be increased from 87.64μm to 11.50μm. 2 Increased by 2.2% to 89.59μm 2 As a result, the area required for making the element (equivalent to the inner area of the element isolation middle line 148 indicated by the dotted line) is reduced from 104.96 μm 2 Increased by 2.9% to 108.00μm 2 Compared with the embodiment, this area is increased by 3.9%. Therefore, compared with the embodiment, the grain yield per wafer is reduced.
[0126] (Comparison between Example and Comparative Example)
[0127] In the example Figure 5 The width of the light-emitting element is 7.79 μm, and the plane viewing area of the light-emitting element is 87.64 μm. 2 . The distance (width) to the middle line (element isolation middle line 48) between the adjacent elements represented by the dotted line is 0.43μm (the distance to the adjacent grain is 0.86μm). At this time, the area required for each light-emitting element is the area surrounded by the middle line (the area surrounded by the element isolation middle line 48 represented by the dotted line). The area of the area surrounded by the element isolation middle line 48 is 103.92μm 2When configured while maintaining the spacing distance rule Fig.12 In the case of the rectangular element of the comparative example shown in FIG. 1 , when the area of the light emitting element is set to be the same, the area surrounded by the element isolation intermediate line 148 is 104.96 μm 2 , the design of the embodiment has an area 1.00% smaller than that of the rectangular case (comparative example).
[0128] As described above, there is a 1.00% difference in the light emitting element area, and there is also a difference in the comparison of the area of the effective light emitting layer.
[0129] In both the embodiment and the comparative example, the lower layer is exposed (at Figure 5 In the figure, it is shown as the lower layer exposed area 18a. Fig.12 In the figure, the exposed lower layer region 118a is shown, but an ohmic contact electrode (lower electrode 56 and lower electrode 156 in the embodiment and the comparative example, respectively) is formed in contact with the exposed lower layer. Figure 5 and Fig.12 The electrode area in contact with the lower layer is unified to 6.93 μm 2 .
[0130] Embodiment Figure 5 The electrodes in the comparative example are triangular. Fig.12 The electrodes are rectangular in shape. The distances from the element isolation ends in the longitudinal and lateral directions (alignment tolerance in the photolithography process) are uniformly set to the same regular 0.25 μm in the above example.
[0131] At this time, the light-emitting layer remains in the area other than the area reduced by the exposure of the lower layer, and the area of the remaining light-emitting layer contributes to the effective light emission. This area is 75.49 μm in the embodiment. 2 , 74.55 μm in the comparative example 2 , resulting in a difference of about 1.25%. The various characteristics of LEDs depend on the current density injected into the light-emitting layer. The current density is determined by the area of the light-emitting layer and the amount of electricity injected into the active layer. Therefore, it is the area of the light-emitting layer, not the area of the entire grain, that determines the characteristics of the LED.
[0132] That is, by using the technology of the present invention, the area of the entire light-emitting element can be reduced smaller than before, and the occupied area required when manufacturing the light-emitting element can be reduced smaller than before.
[0133] In addition, regarding the effect of generating a difference in the light-emitting layer while maintaining the same crystal grain area, the effect is highest when the electrode in contact with the lower layer has a triangular shape rather than a quadrangular or trapezoidal shape.
[0134] In addition, the case where the grain area is unified is exemplified here. When the grain area is unified, the area of the light-emitting layer portion is larger in the embodiment. When the technology of the present invention is used, it is obvious that the grain area can be reduced to be smaller than the grain of the prior art. Therefore, when the light-emitting layer area (not the grain area) is unified to be the same as the prior art and the present technology is applied, the technical effect will be greater than the effect shown here. In addition, the same effect can be obtained when the light-emitting layer area is made consistent and the light-emitting element area is further reduced, rather than being consistent in the light-emitting element area.
[0135] This specification includes the following protocols.
[0136] [1]: A method for manufacturing a light-emitting element, which is a method for manufacturing a plurality of light-emitting elements and comprises the following steps:
[0137] a step of growing an epitaxial layer including a light emitting layer on a starting substrate, and
[0138] forming an isolation groove on the light emitting layer for forming an element,
[0139] The method for manufacturing the light emitting element is characterized in that:
[0140] The top view shape of each of the plurality of light-emitting elements to be manufactured is set to be a line-symmetric hexagon having an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°;
[0141] The plurality of light emitting elements to be manufactured are isolated by the isolation trench having a predetermined width, and the isolation trench is formed so that the plurality of light emitting elements are arranged without a gap therebetween.
[0142] [2]: The method for manufacturing a light-emitting element according to [1] above, further comprising, after the step of growing the epitaxial layer, a step of bonding a light-transmitting substrate to the epitaxial layer via a bonding material and removing the starting substrate.
[0143] [3]: The method for manufacturing a light-emitting element according to [1] or [2], wherein the two vertex angles are set to be greater than or equal to 90° and less than or equal to 120°.
[0144] [4]: The method for manufacturing a light-emitting element according to [1], [2] or [3] above, wherein the distance between two sides parallel to the axis of symmetry is set to be greater than 1 μm and less than 100 μm.
[0145] [5]: The method for manufacturing a light-emitting element according to [1], [2], [3] or [4] above, wherein the isolation trench is formed by an inductively coupled plasma dry etching method.
[0146] [6]: The method for manufacturing a light-emitting element according to [2], [3], [4] or [5], wherein the light-transmitting substrate is any one of sapphire, quartz and glass.
[0147] [7]: A method for manufacturing a light-emitting element according to [2], [3], [4], [5] or [6], wherein the bonding material is at least one of benzocyclobutene, fluororesin and epoxy resin.
[0148] [8]: A light-emitting element, characterized in that its top view shape is a line-symmetrical hexagon with an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertices through which the axis of symmetry passes are greater than 90° and less than 180°.
[0149] [9]: The light-emitting element according to [8] above, wherein the light-emitting element is bonded to a light-transmitting substrate via a bonding material.
[0150]
[10] : The light-emitting element according to [8] or [9], wherein the two vertex angles are greater than or equal to 90° and less than or equal to 120°.
[0151]
[11] : The light-emitting element according to [8], [9] or
[10] , wherein the distance between two sides parallel to the axis of symmetry is greater than or equal to 1 μm and less than or equal to 100 μm.
[0152]
[12] : The light-emitting element according to [9],
[10] or
[11] above, wherein the light-transmitting substrate is any one of sapphire, quartz and glass.
[0153]
[13] : The light-emitting element according to [9],
[10] ,
[11] or
[12] , wherein the bonding material is at least one of benzocyclobutene, fluororesin and epoxy resin.
[0154] In addition, the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and any technical solution having substantially the same structure and exerting the same technical effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.
Claims
1. A method for manufacturing a light-emitting element, which is a method for manufacturing a plurality of light-emitting elements, and comprises the following steps: a step of growing an epitaxial layer including a light emitting layer on a starting substrate, and forming an isolation groove on the light emitting layer for forming an element, The method for manufacturing the light emitting element is characterized in that: After the step of growing the epitaxial layer, the method further comprises: bonding a light-transmitting substrate to the epitaxial layer via a bonding material, and removing the starting substrate. The top view shape of each of the plurality of light emitting elements to be manufactured is set to be a line-symmetric hexagon having a symmetry axis, wherein: The hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°. The plurality of light emitting elements to be manufactured are isolated by the isolation trench having a predetermined width, and the isolation trench is formed so that the plurality of light emitting elements are arranged without a gap therebetween.
2. The method for manufacturing a light emitting element according to claim 1, wherein: The two vertex angles are set to be greater than or equal to 90° and less than or equal to 120°.
3. The method for manufacturing a light emitting element according to claim 1 or 2, characterized in that: The distance between two sides parallel to the symmetry axis is set to be 1 μm or more and 100 μm or less.
4. The method for manufacturing a light emitting element according to claim 1 or 2, characterized in that: The isolation trench is formed by an inductively coupled plasma dry etching method.
5. The method for manufacturing a light emitting element according to claim 1, wherein: The light-transmitting substrate is made of any one of sapphire, quartz and glass.
6. The method for manufacturing a light emitting element according to claim 1, wherein: The bonding material is at least one of benzocyclobutene, fluororesin, and epoxy resin.
7. A light emitting element, characterized in that: Its top view shape is a line-symmetric hexagon with an axis of symmetry, wherein the hexagon has two sides parallel to the axis of symmetry, the lengths of the two parallel sides are longer than the other four sides, and the two vertex angles through which the axis of symmetry passes are greater than 90° and less than 180°; The light emitting element is bonded to a light-transmitting substrate via a bonding material.
8. The light emitting element according to claim 7, characterized in that The two vertex angles are greater than or equal to 90° and less than or equal to 120°.
9. The light emitting element according to claim 7 or 8, characterized in that: The distance between two sides parallel to the symmetry axis is 1 μm or more and 100 μm or less.
10. The light emitting element according to claim 7, wherein: The light-transmitting substrate is any one of sapphire, quartz and glass.
11. The light emitting element according to claim 7, characterized in that The bonding material is at least any one of benzocyclobutene, fluororesin and epoxy resin.