Anti-infection repair material as well as preparation method and application thereof
The anti-infection repair material that combines silk fibroin with enzyme-free cell matrix peptides solves the problem of conformational transformation and infection risk, and achieves the stability and rapid regeneration effect of the material, which is suitable for tissue repair in complex locations.
Patent Information
- Application Number
- CN202411139783.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
Existing tissue repair materials can easily lead to a conformational transformation of silk fibroin under long-term environmental exposure, affecting material performance, and have a risk of infection, making it difficult to meet the rapid regeneration needs of organ cells.
Silk fibroin is used to complex with the polypeptide obtained by enzymatic liberation of the cell matrix, and combined with specific process treatment to prepare anti-infection repair materials to ensure the stability and anti-infection effect of the material in an aqueous environment.
It extends the life of the material, improves the regeneration speed of tissue cells, overcomes the problem of conformational transformation of silk fibroin, provides a rapid repair solution for defects in various complex locations, and has good market application prospects.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomaterials, and particularly relates to an anti-infection repair material and a preparation method and application thereof. Background Art
[0002] In clinical medicine, the application of surgery for tissue repair is a very important topic. In surgical operations for tissue repair, it is crucial to select appropriate repair materials. In the field of cardiovascular repair, blood vessels play the role of transporting oxygen and nutrients, and slow regeneration means that organs cannot receive nutrients through blood vessels in time, thus failing to fully meet the needs of organ cells; in the human body environment, biological repair materials have good biocompatibility to help tissue cells grow in, but it also means that such a good environment may also become a breeding ground for bacteria, leading to bacterial infection and granulation tissue hyperplasia. Therefore, slow regeneration and infection are two challenges currently faced by tissue repair materials.
[0003] CN116814526A discloses an artificial basement membrane and its preparation method and application, wherein the artificial basement membrane comprises: a first component, a second component and a third component; wherein the first component is collagen; the second component is selected from any one or more of type III collagen, type IV collagen, gelatin, silk fibroin, and polysaccharide; and the third component is selected from any one or more of polylactic acid, polyglycolic acid, polylactic acid-glycolic acid, polycaprolactone, and polyvinyl alcohol. It does not involve the performance improvement of silk fibroin. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an anti-infection repair material and a preparation method and application thereof, which overcomes the problem that the conformational change of silk fibroin affects the material performance after long-term environmental exposure.
[0005] The invention provides an anti-infection repair material, which is obtained by compounding silk fibroin with a polypeptide obtained by enzymatically decellularizing a cell matrix.
[0006] Preferably, the molecular weight of the silk fibroin is 100-150 kDa.
[0007] Preferably, the decellularized matrix is selected from one or more of small intestinal submucosa, porcine bladder basement membrane, peritoneum, pericardium, dermis and the like.
[0008] More preferably, the decellularized matrix is selected from the group consisting of small intestinal submucosa, porcine bladder basement membrane, peritoneum, pericardium, dermis, and the like.
[0009] More preferably, the decellularized matrix is small intestinal submucosa or porcine bladder basement membrane.
[0010] Most preferably, the acellular matrix is porcine bladder basement membrane.
[0011] Preferably, the polypeptide obtained by enzymatically decellularizing the cell matrix is obtained by enzymatically decellularizing the cell matrix with trypsin for 1-2 hours and then rinsing with PBS buffer.
[0012] The present invention also provides a method for preparing an anti-infection repair material, comprising the following steps:
[0013] (1) mixing silk fibroin and polypeptide obtained by enzymatic decellularization at a mass ratio of 1:1-3, and adding the mixture into deionized water to obtain a raw material solution;
[0014] (2) The raw material solution obtained in step (1) is mixed with an ethanol / n-butanol mixed solvent in a volume ratio of (2-5):1, and then placed in a mold, and the mold is placed in a -10--5°C refrigerator for 2-4 hours to obtain a repair film; after the repair film is taken out of the mold, it is immersed in anhydrous ethanol, rinsed, and freeze-dried to obtain an anti-infection repair material.
[0015] Preferably, the concentration of the mixture of silk fibroin and polypeptide in the raw material solution in step (1) is 10-25 mg / mL.
[0016] More preferably, the concentration of the mixture of silk fibroin and polypeptide in the raw material solution in step (1) is 14-17 mg / mL.
[0017] The concentration of the mixture of silk fibroin and polypeptide in the raw material solution is measured by a BCA protein concentration kit, which can measure the concentration of proteins (including polypeptides).
[0018] Preferably, the polypeptide is prepared by enzymatic hydrolysis of the decellularized matrix in an aqueous trypsin solution at a pH of 7-9.
[0019] The pH of the above-mentioned trypsin aqueous solution can be adjusted with PBS buffer or sodium hydroxide aqueous solution, etc., and is not specifically limited as long as the pH condition of 7-9 is reached.
[0020] More preferably, the polypeptide is prepared by enzymatic hydrolysis of the decellularized matrix in an aqueous solution of trypsin at a pH of 7-8 or a pH of 8-9.
[0021] More preferably, in the trypsin aqueous solution at a pH of 7-9, the concentration of trypsin is 0.1-0.5 wt %.
[0022] More preferably, in the trypsin aqueous solution at a pH of 7-9, the concentration of trypsin is 0.3 wt %.
[0023] Preferably, the volume ratio of ethanol to n-butanol in the ethanol / n-butanol mixed solvent in step (2) is 0.8:0.8-1.5.
[0024] Preferably, the mold in step (2) is a cylindrical mold with a radius of 2-15 cm and a thickness of 50-150 μm.
[0025] Preferably, the soaking temperature in step (2) is 2-5°C.
[0026] Preferably, the flushing time in step (2) is 10 min-25 min.
[0027] The invention also provides an application of an anti-infection repair material in tissue repair.
[0028] Beneficial Effects
[0029] The present invention compounds silk fibroin with a mixture of polypeptides of different chain lengths after enzymatic hydrolysis, especially the enzymatic hydrolysate of the small intestinal submucosa or the pig bladder basement membrane, and uses a specific process for post-processing, thereby extending the life of the material and overcoming the problem that the conformational change of silk fibroin affects the material performance after long-term environmental exposure. This improvement is particularly significant for silk fibroin with a larger molecular weight of 100-150kDa. The material obtained by the present invention still has a stable release of anti-infection effect in an aqueous environment. After the material is implanted, the regeneration speed of tissue cell ingrowth is improved, and it is suitable for the rapid repair of defects in various complex locations, and has good market application prospects. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0031] The raw materials in the embodiment are as follows:
[0032] Silk fibroin: Examples 1-3 and Comparative Examples 1-4 are lyophilized silk fibroin powders with a molecular weight of 100-150 kDa, purchased from Shanghai Qifa Experimental Reagent Co., Ltd., model #5352; Comparative Example 5 is a silk fibroin solution with a molecular weight of approximately 20 kDa, purchased from Suzhou Suhao Biomaterials Technology Co., Ltd.
[0033] Example 1
[0034] (1) The polypeptide is prepared by enzymatic hydrolysis of a decellularized matrix (porcine bladder basement membrane) in a trypsin aqueous solution at a pH of 7.3±0.3, wherein the concentration of trypsin in the trypsin aqueous solution is 0.3 wt %; silk fibroin and the polypeptide obtained by enzymatic hydrolysis of the decellularized matrix are mixed in a mass ratio of 1:1, and added to deionized water to obtain a raw material solution, wherein the concentration of the mixture of silk fibroin and the polypeptide in the raw material solution is 15 mg / mL;
[0035] (2) The raw material solution obtained in step (1) is mixed with an ethanol / n-butanol mixed solvent (ethanol:n-butanol volume ratio of 1:1) at a volume ratio of 1:5, and then placed in a mold, and the mold is placed in a -10°C refrigerator for 2 hours to obtain a repair film; after taking the repair film out of the mold, immerse it in anhydrous ethanol in a 4°C refrigerator, rinse the repair film with deionized water for 10 minutes, and freeze-dry to obtain an anti-infection repair material.
[0036] Example 2
[0037] (1) The polypeptide is prepared by enzymatic hydrolysis of a decellularized matrix (porcine bladder basement membrane) in a trypsin aqueous solution at a pH of 7.3±0.3, wherein the concentration of trypsin in the trypsin aqueous solution is 0.4 wt %; silk fibroin is mixed with the polypeptide obtained by enzymatic hydrolysis of a decellularized matrix (small intestinal submucosal layer) in a mass ratio of 1:2, and added to deionized water to obtain a raw material solution, wherein the concentration of the mixture of silk fibroin and polypeptide in the raw material solution is 17 mg / mL;
[0038] (2) The raw material solution obtained in step (1) is mixed with an ethanol / n-butanol mixed solvent (ethanol:n-butanol volume ratio of 1:1) at a volume ratio of 1:5, and then placed in a mold, and the mold is placed in a -10°C refrigerator for 3 hours to obtain a repair film; after taking the repair film out of the mold, immerse it in anhydrous ethanol in a 4°C refrigerator, rinse the repair film with deionized water for 10 minutes, and freeze-dry to obtain an anti-infection repair material.
[0039] Example 3
[0040] (1) The polypeptide is prepared by enzymatic hydrolysis of a decellularized matrix (porcine bladder basement membrane) in a trypsin aqueous solution at a pH of 8.2±0.3, wherein the concentration of trypsin in the trypsin aqueous solution is 0.2 wt %; silk fibroin and the polypeptide obtained by enzymatic hydrolysis of the decellularized matrix (porcine bladder basement membrane) are mixed in a mass ratio of 1:3, and added to deionized water to obtain a raw material solution, wherein the concentration of the mixture of silk fibroin and the polypeptide in the raw material solution is 20 mg / mL;
[0041] (2) The raw material solution obtained in step (1) is mixed with an ethanol / n-butanol mixed solvent (ethanol:n-butanol volume ratio of 1:1) at a volume ratio of 1:5, and then placed in a mold, and the mold is placed in a -10°C refrigerator for 2 hours to obtain a repair film; after taking the repair film out of the mold, immerse it in anhydrous ethanol in a 4°C refrigerator, rinse the repair film with deionized water for 10 minutes, and freeze-dry to obtain an anti-infection repair material.
[0042] Comparative Example 1
[0043] The difference from Example 1 is that in step (1), the silk fibroin and the polypeptide obtained by enzymatically decellularizing the cell matrix are mixed in a mass ratio of 2:1.
[0044] Comparative Example 2
[0045] The difference from Example 3 is that in step (1), the concentration of trypsin in the trypsin aqueous solution is 0.5 wt %; and the concentration of the mixture of silk fibroin and polypeptide in the raw material solution in step (1) is 34 mg / mL.
[0046] Comparative Example 3
[0047] The difference from Example 1 is that in the ethanol / n-butanol mixed solvent in step (2), the volume ratio of ethanol to n-butanol is 0.8:2.2.
[0048] Comparative Example 4
[0049] The difference from Example 1 is that in step (2), the raw material solution is mixed with the ethanol / n-butanol mixed solvent in a volume ratio of 1:1.
[0050] Comparative Example 5
[0051] The difference from Example 3 is that in step (1), the source of silk fibroin is different.
[0052] Performance Test:
[0053] ① Mechanical properties in water environment (elongation at break, Young's modulus): After the anti-infection repair materials obtained in Examples 1-3 and Comparative Examples 1-5 were immersed in physiological saline for 20 minutes, the elongation at break and Young's modulus were tested using an Elf3330 dynamic / static multifunctional biomechanical testing machine. The results are shown in Table 1. (The Young's modulus of human skin is about 0.64 MPa, and the Young's modulus of soft tissue is 1.8 MPa)
[0054] ② Antibacterial rate of Escherichia coli and Staphylococcus aureus: The anti-infection repair materials obtained in Examples 1-3 and Comparative Examples 1-4 were made into discs with a diameter of 1 cm and placed on bacterial suspensions (bacterial suspension concentration 10 6CFU / ml) on a solid plate culture medium and incubated in a constant temperature incubator at 37°C for 24 h. The antibacterial property of the material was tested by the antibacterial ring method. The larger the antibacterial ring diameter, the better the antibacterial property. The results showed that the antibacterial ring diameter of Example 1 was slightly larger than the antibacterial ring diameter of Example 3, the antibacterial ring diameter of Example 1 was close to the antibacterial ring diameter of Example 2, and the antibacterial ring diameters of Examples 1-3 were much larger than the antibacterial ring diameters of Comparative Examples 1-4, that is, Example 1≈Example 3>Example 2>Comparative Example 1>Comparative Example 2>Comparative Example 3>Comparative Example 4.
[0055] ③ Skin wound healing rate experiment: A total of 40 8-week-old healthy mice weighing 24±2g were taken and divided into 4 groups, 10 mice in each group. The back hair of all mice was shaved, and a 15mm×15mm wound was burned on the back of the mouse using a laser. The anti-infection repair materials obtained in Example 1 (1 group of mice) and Comparative Examples 1-3 (2 groups of mice, 3 groups of mice, and 4 groups of mice) were applied to the wounds, and the wound areas on the 5th day, 7th day, and 10th day were recorded respectively to calculate the wound healing rate (the average wound healing rate of 10 mice in each group was taken). The results are shown in Table 2.
[0056] Table 1
[0057] Example Elongation at break (%) Young's modulus (MPa) Example 1 54 1.2 Example 2 51 1.3 Example 3 58 1.5 Comparative Example 1 46 0.9 Comparative Example 2 35 0.6 Comparative Example 3 21 0.4 Comparative Example 4 14 / Comparative Example 5 37 0.9
[0058] Table 2
[0059] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Wound healing rate on the 5th day (%) 45 25 33 23 Wound healing rate on the 7th day (%) 88 50 82 35 Wound healing rate on the 10th day (%) 98 76 91 59
Claims
1. An anti-infection repair material, characterized in that: The material is obtained by compounding silk fibroin with a polypeptide obtained by enzymatically decellularizing a cell matrix.
2. The anti-infection repair material according to claim 1, characterized in that: The molecular weight of the silk fibroin is 100-150 kDa.
3. The anti-infection repair material according to claim 1, characterized in that: The polypeptide obtained by enzymatically decellularizing the matrix is obtained by enzymatically decellularizing the matrix with trypsin for 1-2 hours and then rinsing with PBS buffer.
4. A method for preparing the anti-infection repair material according to claim 1, comprising the following steps: (1) mixing silk fibroin and polypeptide obtained by enzymatic decellularization at a mass ratio of 1:1-3, and adding the mixture into deionized water to obtain a raw material solution; (2) The raw material solution obtained in step (1) is mixed with an ethanol / n-butanol mixed solvent in a volume ratio of (2-5):1, and then placed in a mold, and the mold is placed in an environment of -10--5°C for 2-4 hours to obtain a repair film; after the repair film is taken out of the mold, it is immersed in anhydrous ethanol, rinsed, and freeze-dried to obtain an anti-infection repair material.
5. The preparation method according to claim 4, characterized in that: The concentration of the mixture of silk fibroin and polypeptide in the raw material solution in step (1) is 10-25 mg / mL.
6. The preparation method according to claim 4, characterized in that: The volume ratio of ethanol to n-butanol in the ethanol / n-butanol mixed solvent in step (2) is 0.8:0.8-1.
5.
7. The preparation method according to claim 4, characterized in that: The mold in step (2) is a cylindrical mold with a radius of 2-15 cm and a thickness of 50-150 μm.
8. The preparation method according to claim 4, characterized in that: The soaking temperature in step (2) is 2-5°C.
9. The preparation method according to claim 4, characterized in that: The flushing time in step (2) is 10 min to 25 min.
10. Use of the anti-infection repair material according to claim 1 in tissue repair.