Preparation method of hydrophobic SiO2-agarose-polyurea composite aerogel microspheres

By combining coal gangue with polyurea and agarose, hydrophobic SiO2-agarose-polyurea composite aerogel microspheres are prepared, which solves the problems of high brittleness and high cost of traditional SiO2 aerogel materials, and achieves low cost. High-performance aerogel microsphere preparation, suitable for a variety of application scenarios.

CN119034629APending Publication Date: 2024-11-29INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411399676.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The ethyl orthosilicate used in the preparation of traditional silica aerogel materials is expensive and moderately toxic, and the prepared SiO2 aerogel materials have high brittleness problems, which is difficult to meet the needs of widespread applications.

Method used

Using coal gangue solid waste as raw material, hydrophobic SiO2-agarose-polyurea composite aerogel microspheres are prepared by compounding with polyurea polymer material and natural polymer agarose, and the core shell is obtained by supercritical carbon dioxide drying technology. Structure of aerogel microspheres.

Benefits of technology

It has achieved low cost and high-value utilization of materials, imparted good mechanical properties and hydrophobicity to aerogel microspheres, solved the inherent high brittleness problems of SiO2 aerogel materials, and is suitable for thermal insulation, oil stain adsorption and gas adsorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034629A_ABST
    Figure CN119034629A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, and relates to the field of aerogel materials, coal gangue solid waste is used as a production raw material of an aerogel material, and the aerogel microspheres are prepared by compounding a polyurea polymer material, natural polymer agarose and inorganic SiO2; the aerogel microsphere prepared by the invention is of a core-shell structure, the outer layer is a macromolecular polyurea layer, and the interior is a three-dimensional porous network formed by SiO2 and agarose fibers; the polyurea on the outer layer is used as a high polymer material to form a uniform and stable ureido structure, so that the microspheres are endowed with better mechanical properties; the interior of the microsphere is of a porous structure formed by SiO2 and agarose fibers, so that the microsphere is endowed with a relatively high specific surface area; the aerogel microspheres have good hydrophobicity and are stable in form; the problem of inherent high brittleness of the SiO2 aerogel material is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aerogel materials, and in particular to a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres. Background Art

[0002] Aerogel is a super porous three-dimensional nanomaterial, which is obtained by special drying treatment of wet gel so that the liquid phase between the gel skeleton is replaced by the gas phase, while the gel skeleton is preserved intact. The unique microstructure gives the aerogel material excellent properties such as high porosity, high specific surface area, and ultra-low density. Due to these unique properties, aerogel has broad application prospects in various fields such as thermal insulation, chemical catalysis, aerospace, and energy storage.

[0003] Traditional silica aerogel is mainly prepared by sol-gel method, using tetraethyl orthosilicate (TEOS) as raw material and combining ethanol supercritical drying process. TEOS is expensive and moderately toxic, and the prepared SiO2 aerogel material also has the problem of high brittleness. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, using coal gangue solid waste as the production raw material of aerogel materials, and preparing aerogel microspheres by compositely using polyurea polymer materials, natural polymer agarose and inorganic SiO2.

[0005] The present invention adopts the following technical scheme: The present invention provides a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, comprising the following steps:

[0006] Step S1, using coal gangue to prepare SiO2 wet gel.

[0007] Step S2, preparing SiO2 wet gel into SiO2-agarose wet gel solution.

[0008] Step S3, preparing SiO2-agarose composite wet gel microspheres from the SiO2-agarose wet gel solution.

[0009] Step S4, compounding the SiO2-agarose composite wet gel microspheres with a polymer polyurea shell.

[0010] Step S5, subjecting the microspheres prepared in step S4 to supercritical carbon dioxide drying to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres.

[0011] In an exemplary embodiment of the present invention, in step S1, the method for preparing SiO2 wet gel using coal gangue is as follows: the coal gangue is mixed with an alkaline activator and calcined to obtain clinker; the clinker is then dissolved with a sulfuric acid solution; thereafter, a silicate solution is vacuum filtered to obtain a silicate solution; the silicate solution is heated and aged to obtain a gel; and the gel is washed with deionized water to obtain a SiO2 wet gel.

[0012] In an exemplary embodiment of the present invention, the alkaline activator is sodium carbonate; the calcination temperature is 500-1300° C.; and sulfuric acid is used to adjust the pH of the slurry to 2-4.

[0013] In an exemplary embodiment of the present invention, in step S2, the method of preparing SiO2 wet gel into SiO2-agarose wet gel solution is as follows: SiO2 wet gel is mixed with deionized water to form a slurry; then agarose is added and stirred; and then microwave heating is performed until boiling to obtain SiO2-agarose wet gel solution.

[0014] In an exemplary embodiment of the present invention, the amount of agarose used is 1-4% of the mass of the slurry.

[0015] In an exemplary embodiment of the present invention, in step S3, the method of preparing SiO2-agarose wet gel solution into SiO2-agarose composite wet gel microspheres is as follows: the SiO2-agarose wet gel solution is dropped into silicone oil to form microspheres, and then the microspheres are removed and washed with water, and then placed in anhydrous ethanol for sufficient replacement to obtain SiO2-agarose composite wet gel microspheres.

[0016] In an exemplary embodiment of the present invention, the silicone oil is selected from any one of diethyl silicone oil, dimethyl silicone oil, and phenyl silicone oil.

[0017] In an exemplary embodiment of the present invention, in step S4, the method of composite SiO2-agarose composite wet gel microspheres with a polymer polyurea shell is as follows: react the SiO2-agarose composite wet gel microspheres with a component A solution capable of synthesizing polyurea under heating conditions, wherein the component A solution is an isocyanate component diluted by a diluent; then place them in a diluent for replacement; then react with a component B solution capable of synthesizing polyurea at room temperature, wherein the component B solution is an amino compound diluted by a diluent; then place them in a diluent for replacement; then place them in anhydrous ethanol for replacement; the diluent is any one of acetonitrile, n-hexane, toluene, and acetone.

[0018] In an exemplary embodiment of the present invention, the method for preparing the component A solution is as follows: diphenylmethane diisocyanate (MDI-50) and a diluent are mixed in a mass ratio of 1:1 to 8 to prepare the component A solution.

[0019] In an exemplary embodiment of the present invention, the preparation method of the component B solution is as follows: terminal amino polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) are prepared into component B in a molar ratio of 2:1:1, and component B is mixed with a diluent in a mass ratio of 1:1 to 8 to prepare the component B solution.

[0020] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, adopts coal gangue solid waste as the production raw material of aerogel materials, and prepares aerogel microspheres by compositely using polyurea polymer materials, natural polymer agarose and inorganic SiO2; using coal gangue as the raw material has low cost and realizes the high-value utilization of coal gangue waste; the aerogel microspheres prepared by the present invention are of a core-shell structure, the outer layer is a polymer polyurea layer, and the interior is a three-dimensional porous network composed of SiO2 and agarose fibers; the outer layer of polyurea as a polymer material forms a uniform and stable urea-based structure, which gives the microspheres good mechanical properties; the interior of the microspheres is a porous structure composed of SiO2 and agarose fibers, which gives the microspheres a higher specific surface area; the aerogel microspheres have good hydrophobicity and stable morphology; and the inherent high brittleness problem of SiO2 aerogel materials is solved.

[0021] The aerogel microspheres prepared by the present invention can be used as aerogel special thermal insulation coatings, and applied to energy-saving and thermal insulation fields such as buildings, chemical pipelines, and cold chain vehicles; compared with solid thermal insulation layers such as felt materials, they have better fit and thermal insulation effects for special-shaped parts. The aerogel microspheres prepared by the present invention can also be used in environmental treatment fields such as oil pollution adsorption and gas adsorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Shown is the XRF analysis result diagram of the coal gangue used in the present invention.

[0023] Figure 2 Shown is the XRD diagram of the coal gangue used in the present invention before activation.

[0024] Figure 3 Shown is the XRD diagram of the activated coal gangue used in the present invention.

[0025] Figure 4 Shown is a line graph showing the change in activation reaction rate of the coal gangue used in the present invention with temperature.

[0026] Figure 5 Shown is a scanning electron microscope image of the cross section of the SiO2-agarose-polyurea composite aerogel microsphere prepared in Example 1 of the present invention.

[0027] Figure 6Shown are water contact angle graphs of SiO2-agarose-polyurea composite aerogel microspheres prepared in Examples 1 to 3 of the present invention.

[0028] Figure 7 Shown is a stress-strain curve of the SiO2-agarose-polyurea composite aerogel microspheres prepared in Example 1 of the present invention under compression test.

[0029] Figure 8 Shown is the infrared spectrum of SiO2-agarose-polyurea composite aerogel microspheres prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with specific examples. The following description is only used to illustrate the technical solution of the present invention but not to limit it. The experimental methods used in the examples are conventional methods unless otherwise specified. The materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified. For example, the present invention uses agarose provided by Zhongke Ruitai Biotechnology Co., Ltd.

[0031] The invention provides a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, adopting coal gangue solid waste as a production raw material of aerogel materials, and preparing aerogel microspheres by compositely using polyurea polymer materials, natural polymer agarose and inorganic SiO2.

[0032] The following is an explanation of coal gangue: coal gangue is a mineral associated with coal during the coal formation process, with a lower carbon content, stronger than coal, and a black-gray color. The main components of coal gangue are kaolinite, quartz, etc. The composition and content of coal gangue in different regions are different; the coal gangue selected in the embodiment of the present invention comes from Tuyou Banner, Baotou City, Inner Mongolia Autonomous Region. Figure 1 The figure shows the XRF analysis result of the coal gangue used in the present invention. Through XRF testing, the content of SiO2 in the coal gangue used in the present invention is about 43.77%.

[0033] The method of the present invention comprises the following steps:

[0034] Step S1, using coal gangue to prepare SiO2 wet gel. The specific method is as follows: coal gangue is mixed with an alkaline activator and calcined to obtain clinker; then the clinker is dissolved with a sulfuric acid solution; then, a silicate solution is vacuum filtered to obtain a silicate solution; the silicate solution is heated and aged to obtain a gel; and the gel is washed with deionized water to obtain a SiO2 wet gel.

[0035] In an exemplary embodiment of the present invention, coal gangue powder and sodium carbonate (alkaline activator) are taken at a mass ratio of 1:0.4-0.8, and the two are evenly mixed to form a mixed powder; then, the mixed powder is placed in a muffle furnace for calcination to obtain clinker, the calcination temperature is 500-1300°C, and the calcination time is 1-5h; thereafter, the clinker is mixed with deionized water to form a slurry, and the mass ratio of clinker to deionized water is 1:2-6; then, the pH of the slurry is adjusted to 2-4 with 3-9 mol / L sulfuric acid for dissolution; the dissolved slurry is stirred and vacuum filtered to obtain a silicate solution; the obtained silicate solution is placed in an oven for heating and aging to obtain a gel, the heating temperature is 60-80°C, and the aging time is 12-24h. 100-150mL of deionized water is poured into the gel, and stirred and washed on a magnetic stirrer for 1-2h to remove Na in the gel. + , K + , Fe 3+ The pH of the gel is adjusted to 5-7 by washing; then, the gel is placed in a centrifuge and centrifuged at 10000-12000 rpm / min for 10-15 minutes to separate the solution from the colloid; the gel is washed 3-5 times to remove impurities, and a SiO2 wet gel is obtained.

[0036] In the present invention, sulfuric acid is used to adjust the pH value of the slurry to 2-4, the purpose of which is to enable SiO2 to maintain a certain period of time in a solution state to avoid its rapid gelation. Sulfuric acid is a non-volatile acid and tasteless, and sulfate ions can be subsequently converted into calcium sulfate precipitation through other processes, which is convenient for recovery.

[0037] Step S2, preparing SiO2 wet gel into SiO2-agarose wet gel solution. The specific method is as follows: mixing SiO2 wet gel with deionized water to prepare slurry; then adding agarose and stirring to mix; then heating with microwave to boiling to prepare SiO2-agarose wet gel solution.

[0038] In an exemplary embodiment of the present invention, SiO2 wet gel and deionized water are mixed in a mass ratio of 1:1 to 5, and then mechanically beaten at a temperature of 20 to 35°C to form a slurry, so that the gel and deionized water form a stable and uniform phase. After that, agarose is added to the slurry, and the amount of agarose is 1 to 4% of the mass of the slurry; then it is placed under a magnetic stirrer for mechanical mixing for 5 to 10 minutes, and the speed of the magnetic stirrer is 200 to 500 rpm / min and the stirring temperature is 20 to 35°C. Then, a microwave reactor is used to heat to boiling to obtain a SiO2-agarose wet gel solution; the microwave reactor has a heating power of 500 to 700 W, a heating time of 3 to 5 minutes, and it is boiled 5 to 10 times; in this way, agarose can be fully dissolved. The prepared SiO2-agarose wet gel solution is placed in an oven at 80 to 100°C for standby to prevent it from gelling.

[0039] Step S3, preparing SiO2-agarose wet gel solution into SiO2-agarose composite wet gel microspheres. The specific method is as follows: dropping SiO2-agarose wet gel solution into silicone oil to form microspheres, then taking out the microspheres, washing them with water, and then placing them in anhydrous ethanol for full replacement to obtain SiO2-agarose composite wet gel microspheres.

[0040] In an exemplary embodiment of the present invention, a SiO2-agarose wet gel solution is placed in a 5-20 ml syringe, and then squeezed and dripped into silicone oil to form microspheres; the needle model can be selected from 18 to 30, and the injection rate is controlled at 1.8 to 15 mL / min; the microspheres are then removed and rinsed with a large amount of deionized water, and then placed in anhydrous ethanol for sufficient replacement to obtain SiO2-agarose composite wet gel microspheres.

[0041] In the present invention, the silicone oil can be selected from any one of diethyl silicone oil, dimethyl silicone oil and phenyl silicone oil.

[0042] Step S4, composite SiO2-agarose composite wet gel microspheres with polymer polyurea shells. The specific method is as follows: react SiO2-agarose composite wet gel microspheres with a component A solution capable of synthesizing polyurea under heating conditions, wherein the component A solution is an isocyanate component diluted by a diluent; then place in a diluent for replacement; then react with a component B solution capable of synthesizing polyurea at room temperature, wherein the component B solution is an amino compound diluted by a diluent; then place in a diluent for replacement; and then place in anhydrous ethanol for replacement. The diluent is any one of acetonitrile, n-hexane, toluene, and acetone.

[0043] In an exemplary embodiment of the present invention, the method for preparing the component A solution is as follows: diphenylmethane diisocyanate (MDI-50) and a diluent are mixed in a mass ratio of 1:1 to 8 to prepare the component A solution.

[0044] In an exemplary embodiment of the present invention, the preparation method of the component B solution is as follows: terminal amino polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) are prepared into component B in a molar ratio of 2:1:1, and component B is mixed with a diluent in a mass ratio of 1:1 to 8 to prepare the component B solution.

[0045] In an exemplary embodiment of the present invention, SiO2-agarose composite wet gel microspheres and component A solution are mixed and shaken in a round-bottom flask at a mass ratio of 1:5-10; then placed in an oil bath for heating reaction; the heating temperature is 60-120°C, and the heating time is 2-6 hours. Then the microspheres are placed in a diluent for replacement for 1-2 hours; then the microspheres and component B solution are reacted in a beaker at room temperature (10-30°C) for 2-6 hours, and the amount of SiO2-agarose composite wet gel microspheres and component B solution is a mass ratio of 1:5-10; then the microspheres are placed in a diluent for replacement for 1-2 hours; and then placed in anhydrous ethanol for full replacement.

[0046] Step S5, subjecting the microspheres prepared in step S4 to supercritical carbon dioxide drying to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres.

[0047] In an exemplary embodiment of the present invention, the drying pressure of supercritical carbon dioxide drying is 11-20 MPa, and the drying temperature is 40-60°C.

[0048] The macroscopic morphology of the aerogel microspheres prepared by the present invention is microsphere-shaped, with a diameter of 0.2 to 4 mm and a density of 0.015 to 0.065 g·cm -3 , with a specific surface area of ​​200 to 800 m 2 / g, the compression deformation of a single particle is 80-85%, and the single compression fracture strength is 120-145N.

[0049] Example 1, a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, comprising the following steps:

[0050] Step S1, take coal gangue powder and sodium carbonate at a mass ratio of 1:0.6, and mix the two evenly to form a mixed powder; then, place the mixed powder in a muffle furnace and calcine to obtain clinker, the calcination temperature is 875°C, and the calcination time is 2.5h; then, mix the clinker with deionized water to form a slurry, and the mass ratio of clinker to deionized water is 1:3; then, adjust the pH of the slurry to 2 with 6mol / L sulfuric acid for dissolution; stir and vacuum filter the dissolved slurry to obtain a silicate solution; place the obtained silicate solution in an oven for heating and aging to obtain a gel, the heating temperature is 80°C, and the aging time is 12h. Pour 150mL of deionized water into the gel, stir and wash it on a magnetic stirrer for 1h to remove Na in the gel. + , K + , Fe 3+ The pH of the gel was adjusted to 6 by washing; then, the gel was placed in a centrifuge and centrifuged at 12000 rpm / min for 10 min to separate the solution from the colloid; the gel was washed 5 times to remove impurities and obtain SiO2 wet gel.

[0051] Step S2, SiO2 wet gel and deionized water are mixed in a mass ratio of 1:3, and then mechanically slurried at a temperature of 25°C so that the gel and deionized water form a stable and uniform phase. After that, 2wt% agarose is added thereto, and the mixture is placed under a magnetic stirrer for mechanical mixing for 10 minutes, the speed of the magnetic stirrer is 250rpm / min, and the stirring temperature is 25°C. Next, a microwave reactor is used to heat to boiling to obtain a SiO2-agarose wet gel solution; the microwave reactor has a heating power of 700W, a heating time of 5min, and boils 5 times; in this way, the agarose can be fully dissolved. The prepared SiO2-agarose wet gel solution is placed in an oven at 80°C for standby use to prevent it from gelling.

[0052] Step S3, placing the SiO2-agarose wet gel solution in a 15 ml syringe, then squeezing it and dropping it into silicone oil to form microspheres; the needle model can be selected as No. 24, and the injection rate is controlled at 12 mL / min; then the microspheres are removed and rinsed with a large amount of deionized water, and then placed in anhydrous ethanol for full replacement to obtain SiO2-agarose composite wet gel microspheres.

[0053] Step S4, compounding SiO2-agarose composite wet gel microspheres with a polymer polyurea shell. The specific method is as follows:

[0054] Prepare component A solution: mix diphenylmethane diisocyanate (MDI-50) and diluent in a mass ratio of 1:2 to prepare component A solution.

[0055] Prepare component B solution: prepare component B by mixing amino-terminated polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) in a molar ratio of 2:1:1, and prepare component B solution by mixing component B with diluent in a mass ratio of 1:2.

[0056] SiO2-agarose composite wet gel microspheres and component A solution were mixed and shaken in a round-bottom flask at a mass ratio of 1:6; then placed in an oil bath for heating reaction; the heating temperature was 80°C and the heating time was 4 hours. Then the microspheres were replaced in a diluent for 1 hour; then the microspheres and component B solution were reacted in a beaker at room temperature for 4 hours, and the amount of SiO2-agarose composite wet gel microspheres and component B solution was 1:6 in mass ratio; then the microspheres were replaced in a diluent for 1 hour; and then placed in anhydrous ethanol for full replacement.

[0057] Step S5, supercritical carbon dioxide drying the microspheres prepared in step S4 to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres; the supercritical carbon dioxide drying pressure is 15 MPa and the drying temperature is 50°C.

[0058] The diameter of the hydrophobic SiO2-agarose-polyurea composite aerogel microspheres prepared in this example is 4 mm and the density is 0.077 g·cm -3 , with a specific surface area of ​​800m 2 / g; the compression breaking strength of a single particle is 132N.

[0059] Example 2, a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, comprising the following steps:

[0060] Step S1, take coal gangue powder and sodium carbonate at a mass ratio of 1:04, and mix the two evenly to form a mixed powder; then, place the mixed powder in a muffle furnace and calcine to obtain clinker, the calcination temperature is 500°C, and the calcination time is 1h; then, mix the clinker with deionized water to form a slurry, and the mass ratio of clinker to deionized water is 1:2; then, adjust the pH of the slurry to 2 with 3mol / L sulfuric acid for dissolution; stir and vacuum filter the dissolved slurry to obtain a silicate solution; place the obtained silicate solution in an oven for heating and aging to obtain a gel, the heating temperature is 60°C, and the aging time is 12h. Pour 100mL of deionized water into the gel, stir and wash it on a magnetic stirrer for 1h to remove Na in the gel. + , K + , Fe 3+ The pH of the gel was adjusted to 5 by washing; then, the gel was placed in a centrifuge and centrifuged at 10,000 rpm / min for 10 minutes to separate the solution from the colloid; the gel was washed three times to remove impurities, and a SiO2 wet gel was obtained.

[0061] Step S2, SiO2 wet gel and deionized water are mixed in a mass ratio of 1:1, and then mechanically slurried at a temperature of 20°C so that the gel and deionized water form a stable and uniform phase. After that, 1wt% agarose is added thereto, and the mixture is placed under a magnetic stirrer for mechanical mixing for 5 minutes, the speed of the magnetic stirrer is 200rpm / min, and the stirring temperature is 20°C. Next, a microwave reactor is used to heat the mixture to boiling to obtain a SiO2-agarose wet gel solution; the microwave reactor has a heating power of 500W, a heating time of 3min, and the mixture is boiled 5 times; in this way, the agarose can be fully dissolved. The prepared SiO2-agarose wet gel solution is placed in an oven at 80°C for standby use to prevent it from gelling.

[0062] Step S3, placing the SiO2-agarose wet gel solution in a 5 ml syringe, then squeezing it and dropping it into silicone oil to form microspheres; the needle model can be selected as No. 18, and the injection rate is controlled at 1.8 mL / min; then the microspheres are removed and rinsed with a large amount of deionized water, and then placed in anhydrous ethanol for full replacement to obtain SiO2-agarose composite wet gel microspheres.

[0063] Step S4, compounding SiO2-agarose composite wet gel microspheres with a polymer polyurea shell. The specific method is as follows:

[0064] Prepare component A solution: mix diphenylmethane diisocyanate (MDI-50) and diluent in a mass ratio of 1:1 to prepare component A solution.

[0065] Prepare component B solution: prepare component B by mixing amino-terminated polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) in a molar ratio of 2:1:1, and prepare component B solution by mixing component B with a diluent in a mass ratio of 1:1.

[0066] SiO2-agarose composite wet gel microspheres and component A solution were mixed and shaken in a round-bottom flask at a mass ratio of 1:5; then placed in an oil bath for heating reaction; the heating temperature was 60°C and the heating time was 2 hours. Then the microspheres were replaced in a diluent for 1 hour; then the microspheres and component B solution were reacted in a beaker at room temperature for 2 hours, and the amount of SiO2-agarose composite wet gel microspheres and component B solution was 1:5 in mass ratio; then the microspheres were replaced in a diluent for 1 hour; and then placed in anhydrous ethanol for full replacement.

[0067] Step S5, supercritical carbon dioxide drying the microspheres prepared in step S4 to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres; the supercritical carbon dioxide drying pressure is 11 MPa and the drying temperature is 40°C.

[0068] Example 3, a method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, comprising the following steps:

[0069] Step S1, take coal gangue powder and sodium carbonate at a mass ratio of 1:0.8, and mix the two evenly to form a mixed powder; then, place the mixed powder in a muffle furnace and calcine to obtain clinker, the calcination temperature is 1300℃, and the calcination time is 5h; then, mix the clinker with deionized water to form a slurry, and the mass ratio of clinker to deionized water is 1:6; then, adjust the pH of the slurry to 4 with 9mol / L sulfuric acid for dissolution; stir and vacuum filter the dissolved slurry to obtain a silicate solution; place the obtained silicate solution in an oven for heating and aging to obtain a gel, the heating temperature is 80℃, and the aging time is 24h. Pour 150mL of deionized water into the gel, stir and wash it on a magnetic stirrer for 2h to remove Na in the gel. + , K + , Fe 3+ The pH of the gel was adjusted to 7 by washing; then, the gel was placed in a centrifuge and centrifuged at 12000 rpm / min for 15 min to separate the solution from the colloid; the gel was washed 5 times to remove impurities and obtain SiO2 wet gel.

[0070] Step S2, SiO2 wet gel and deionized water are mixed in a mass ratio of 1:5, and then mechanically slurried at a temperature of 35°C so that the gel and deionized water form a stable and uniform phase. After that, 4wt% agarose is added thereto, and the mixture is placed under a magnetic stirrer for mechanical mixing for 10 minutes. The speed of the magnetic stirrer is 500rpm / min and the stirring temperature is 35°C. Next, a microwave reactor is used to heat the mixture to boiling to obtain a SiO2-agarose wet gel solution; the microwave reactor has a heating power of 700W and a heating time of 5min, and the mixture is boiled 10 times; in this way, the agarose can be fully dissolved. The prepared SiO2-agarose wet gel solution is placed in an oven at 100°C for standby use to prevent it from gelling.

[0071] Step S3, placing the SiO2-agarose wet gel solution in a 20 ml syringe, then squeezing it and dropping it into silicone oil to form microspheres; the needle model can be selected as No. 30, and the injection rate is controlled at 15 mL / min; then the microspheres are removed and rinsed with a large amount of deionized water, and then placed in anhydrous ethanol for full replacement to obtain SiO2-agarose composite wet gel microspheres.

[0072] Step S4, compounding SiO2-agarose composite wet gel microspheres with a polymer polyurea shell. The specific method is as follows:

[0073] Prepare component A solution: mix diphenylmethane diisocyanate (MDI-50) and diluent in a mass ratio of 1:8 to prepare component A solution.

[0074] Prepare component B solution: prepare component B by mixing amino-terminated polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) in a molar ratio of 2:1:1, and prepare component B solution by mixing component B with diluent in a mass ratio of 1:8.

[0075] SiO2-agarose composite wet gel microspheres and component A solution were mixed and shaken in a round-bottom flask at a mass ratio of 1:10; then placed in an oil bath for heating reaction; the heating temperature was 120°C and the heating time was 6 hours. Then the microspheres were replaced in a diluent for 2 hours; then the microspheres and component B solution were reacted in a beaker at room temperature for 6 hours, and the amount of SiO2-agarose composite wet gel microspheres and component B solution was 1:10; then the microspheres were replaced in a diluent for 2 hours; and then placed in anhydrous ethanol for full replacement.

[0076] Step S5, drying the microspheres prepared in step S4 with supercritical carbon dioxide to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres. The supercritical carbon dioxide drying has a drying pressure of 20 MPa and a drying temperature of 60°C.

[0077] Furthermore, the present invention uses Example 1 as a reference, and only changes the types of reagents used in the component A solution and the component B solution to test the effects of different reagents on the present invention.

[0078] The experimental conclusions are as follows: Examples 4, 5, and 6 change component A. The experiment shows that compared with Example 1, the aerogels prepared in Examples 4, 5, and 6 shrink more severely, and the contact angle becomes smaller, and the hydrophobic ability is poor. Examples 7, 8, and 9 change component B. Compared with Example 1, the aerogels prepared in Examples 7, 8, and 9 do not shrink, but the contact angle is also small, some samples experience structural collapse, and the distribution of the modifier is uneven. Therefore, the aerogels prepared by the A component solution and the B component solution used as modifiers in Example 1 of the present invention are highly hydrophobic and will not shrink to cause structural collapse. At the same time, the surface modifier of the microspheres is flat and uniform.

[0079] Further, the activation analysis of coal gangue in the present invention is as follows:

[0080] Figure 1 Shown is the XRF analysis result diagram of the coal gangue used in the present invention; Figure 2 Shown is the XRD pattern of the coal gangue used in the present invention before activation; Figure 3 Shown is the XRD diagram of the activated coal gangue used in the present invention.

[0081] The XRF test analysis of the coal gangue used in the present invention shows that the proportion of silicon dioxide in the coal gangue can reach 43.77; by observing the XRD diagram of the coal gangue, it can be found that the silicon dioxide in the coal gangue is composed of quartz and Al4Si4O 10 The physical and chemical properties of the two are extremely stable. Therefore, the present invention activates the coal gangue. The present invention uses anhydrous sodium carbonate as an activation aid for the coal gangue. When the two are calcined at high temperature, the quartz phase in the coal gangue reacts with Al4Si4O 10 (kaolinite) will react chemically with anhydrous sodium carbonate to form sodium aluminum silicate (nepheline phase) which is easily soluble in acidic liquid ( Figure 3 As shown). This makes it easier to extract the silicon dioxide later.

[0082] Figure 4 The figure shows the line graph of the activation reaction rate of the coal gangue used in the present invention as a function of temperature. Figure 4It can be seen that in the range of 650℃~825℃, the reaction rate is low, at this time, sodium carbonate has not reached the melting point and is in solid state; coal gangue and sodium carbonate are solid-solid reaction. When the temperature reaches 850℃, the reaction rate increases significantly, reaching 94.72%. At this time, sodium carbonate is basically in a molten state, and it reacts with coal gangue in a solid-liquid state, so the reaction rate increases. In the range of 875℃-900℃, sodium carbonate is completely melted, and the reaction rate with coal gangue reaches the highest 95.67%, and basically remains stable. When the temperature continues to rise, the hardness of the calcined product will increase accordingly, and it is difficult to grind. This is because substances such as alumina and silica in coal gangue generate spinel and inert mullite at too high a temperature. Therefore, the reaction rate is the highest and most economical when the reaction temperature is 875℃.

[0083] Further, the microstructure analysis of the aerogel of the present invention is as follows:

[0084] like Figure 5 The SiO prepared in Example 1 of the present invention is shown. 2- Scanning electron micrograph of the cross section of agarose-polyurea composite aerogel microspheres. Figure 5 It can be seen that the aerogel microspheres prepared by the present invention are core-shell structures, with the outer layer being a polymer polyurea layer and the inner layer being a three-dimensional porous network composed of SiO2 and agarose fibers. The outer layer of polyurea, as a polymer material, forms a uniform and stable urea-based structure, giving the microspheres good mechanical properties. The interior of the microspheres is a porous structure composed of SiO2 and agarose fibers, giving the microspheres a higher specific surface area, and the cross-sections are relatively regular and complete, which reflects that the morphology of the aerogel microspheres is relatively uniform and complete, and no obvious shrinkage occurs during the supercritical drying process.

[0085] Further, the wettability analysis of the aerogel of the present invention is as follows:

[0086] Figure 6 The water contact angle diagram of SiO2-agarose-polyurea composite aerogel microspheres prepared in Examples 1 to 3 of the present invention is shown. Figure 6 It can be seen that the water contact angles of the aerogel microspheres prepared in Examples 1 to 3 are all greater than 115°; this indicates that the composite aerogel microspheres of the present invention have good hydrophobicity. This is attributed to the reaction of the -NCO group at one end of the diisocyanate with the hydroxyl groups on the surface of agarose and SiO2 aerogel, thereby grafting and fixing the diisocyanate, and the -NCO group at the other end of the diisocyanate reacts with the amino compound to form polyurea. Since hydrophobic groups such as methyl and benzene rings are widely present in polyurea, the composite aerogel microspheres are endowed with good hydrophobicity. The aerogels prepared in Examples 4 to 9 verify the properties of good hydrophobicity and stable morphology of the A and B components selected in Example 1.

[0087] Further, the mechanical properties of the aerogel of the present invention are analyzed as follows:

[0088] Figure 7 The stress-strain curve of the SiO2-agarose-polyurea composite aerogel microspheres prepared in Example 1 of the present invention under compression test is shown. Figure 7 It can be seen that the stress of the aerogel microspheres prepared in Example 1 can reach about 13MPa. By comparing the samples prepared in Examples 1 to 3, it can be found that under the premise that the compression deformation of the three samples is 80% (not broken), the force they are subjected to can be seen. As the agarose concentration increases, the force on the composite aerogel microspheres gradually increases, from about 120N to 140N. The sample prepared in Example 3 can withstand the greatest pressure, and the force can reach about 139N when the compression deformation is 80% (not broken), and the overall trend of all samples is that the pressure they are subjected to increases accordingly with the increase of agarose concentration.

[0089] On the other hand, because polyurea is an organic polymer with a strong urea-based structure, when compressed by external force, the strong structure of polyurea will resist the external force, thereby increasing the pressure resistance. Furthermore, since the silica aerogel clusters inside the aerogel microspheres contain abundant hydroxyl groups on the surfaces of silica and agarose, the two can be connected by forming hydrogen bonds, and since the silica aerogel clusters are relatively rigid, when subjected to external force, the force will be transmitted along the agarose network to the silica aerogel clusters, resisting the external force. Therefore, if the sample is to reach the same strain, a greater force is required. And as the amount of agarose added gradually increases, the gel formation of the microspheres is faster, resulting in difficulty in microsphere formation. At the same time, the increase in agarose concentration will clog the syringe during the microsphere formation stage.

[0090] Further, the infrared spectrum test of the aerogel of the present invention is as follows:

[0091] like Figure 8 The infrared spectrum of SiO2-agarose-polyurea composite aerogel microspheres prepared in Example 1 of the present invention is shown. Figure 8 It can be seen that the aerogel prepared in Example 1 has a -1 The asymmetric stretching vibration peak attributed to COC appeared, and at 2970 cm -1 The stretching vibration peak attributed to CH appeared at 2865cm -1 The peak of stretching vibration attributed to NH appeared at 1305cm-1, which preliminarily proved the existence of polyurea. The peak of stretching vibration attributed to tertiary amine group appeared at 1305cm-1, which proved that the secondary amine in MDBA was converted into tertiary amine to generate urea group. -1 The stretching vibration peak of CN appears at 1540cm -1The bending vibration attributed to the NH on the urea group appeared at 1720 cm -1 The stretching vibration peaks of C=O appeared, which are characteristic peaks of polyurea. It can be seen from the peak intensity in the figure that the polyurea content of the SiO2-agarose-polyurea composite aerogel microspheres in Example 1 is relatively high.

[0092] The above embodiments are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation methods. For those of ordinary skill in the art, other different forms of changes can be made based on the above description. And the obvious changes derived from this belong to the scope of protection of the present invention. Finally, it should be noted that the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

Claims

1. A method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres, characterized in that: The steps include: Step S1, using coal gangue to prepare SiO2 wet gel; Step S2, preparing SiO2 wet gel into SiO2-agarose wet gel solution; Step S3, preparing SiO2-agarose composite wet gel microspheres from the SiO2-agarose wet gel solution; Step S4, compounding SiO2-agarose composite wet gel microspheres with a polymer polyurea shell; Step S5, subjecting the microspheres prepared in step S4 to supercritical carbon dioxide drying to obtain hydrophobic SiO2-agarose-polyurea composite aerogel microspheres.

2. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 1, characterized in that the steps In S1, the method for preparing SiO2 wet gel using coal gangue is as follows: the coal gangue is mixed with an alkaline activator and calcined to obtain clinker; the clinker is then dissolved with a sulfuric acid solution; thereafter, a silicate solution is vacuum filtered to obtain a silicate solution; the silicate solution is heated and aged to obtain a gel; and the gel is washed with deionized water to obtain a SiO2 wet gel.

3. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 2, characterized in that: The alkaline activator is sodium carbonate; the calcination temperature is 500-1300°C; and the pH value of the slurry is adjusted to 2-4 by sulfuric acid.

4. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 1, characterized in that the steps In S2, the method for preparing SiO2 wet gel into SiO2-agarose wet gel solution is as follows: SiO2 wet gel is mixed with deionized water and slurried to prepare slurry; then agarose is added and stirred; and then microwave heating is performed until boiling to obtain SiO2-agarose wet gel solution.

5. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 4, characterized in that: The amount of agarose used is 1-4% of the slurry mass.

6. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 1, characterized in that: In step S3, the method for preparing SiO2-agarose wet gel solution into SiO2-agarose composite wet gel microspheres is as follows: drop the SiO2-agarose wet gel solution into silicone oil to form microspheres, then remove the microspheres, wash them with water, and then place them in anhydrous ethanol for sufficient replacement to obtain SiO2-agarose composite wet gel microspheres.

7. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 6, characterized in that: The silicone oil can be any one of diethyl silicone oil, dimethyl silicone oil and phenyl silicone oil.

8. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 1, characterized in that: In step S4, the method for composite SiO2-agarose composite wet gel microspheres with a polymer polyurea shell is as follows: reacting SiO2-agarose composite wet gel microspheres with a component A solution capable of synthesizing polyurea under heating conditions, wherein the component A solution is an isocyanate component diluted by a diluent; then placing in a diluent for replacement; then reacting with a component B solution capable of synthesizing polyurea at room temperature, wherein the component B solution is an amino compound diluted by a diluent; then placing in a diluent for replacement; and then placing in anhydrous ethanol for replacement; the diluent is any one of acetonitrile, n-hexane, toluene, and acetone.

9. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 8, characterized in that: The method for preparing the A component solution is as follows: diphenylmethane diisocyanate (MDI-50) and a diluent are mixed in a mass ratio of 1:1 to 8 to prepare the A component solution.

10. The method for preparing hydrophobic SiO2-agarose-polyurea composite aerogel microspheres according to claim 8, characterized in that: The preparation method of component B solution is as follows: terminal amino polyether (D-2000), diethyltoluenediamine (DETDA-80) and 4.4'-bis-sec-butylaminodiphenyl (MDBA) are prepared into component B in a molar ratio of 2:1:1, and component B is mixed with a diluent in a mass ratio of 1:1 to 8 to prepare component B solution.