Nano-iron-loaded polyvinylidene fluoride membrane and preparation method thereof

By evenly distributing nano zero-valent iron on the polyvinylidene fluoride film, using the electric field force of the high-voltage electrostatic generator to make it fit on the membrane surface, the problems of easy deactivation of nano iron and sludge are solved, and heavy metal chromium is achieved The efficient adsorption and reduction of the chemical pollution risk is reduced, and it has good recycling and economic benefits.

CN119034693APending Publication Date: 2024-11-29HUAIYIN INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411107990.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing nano-irons are prone to deactivate when dealing with heavy metal pollution, produce difficult-to-treat sludge, and have low utilization efficiency and lack effective recycling methods. Traditional membrane separation technology has the risk of secondary pollution.

Method used

By uniformly distributing nano-zero-valent iron on the polyvinylidene fluoride film, the electric field force generated by the high-voltage electrostatic generator is used to make the nano-iron fit on the film surface, and combined with electric field driving technology, the uniform distribution and efficient adsorption and reduction of nano-iron are achieved.

Benefits of technology

Improve the utilization efficiency of nano-iron, extend its active life, reduce the risk of chemical pollution, achieve efficient adsorption and reduction of heavy metal chromium, reduce the impact of other ions on pollution treatment, and has good recycling and economic benefits. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034693A_ABST
    Figure CN119034693A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of heavy metal pollution repair materials, and discloses a preparation method of a nano-iron-loaded polyvinylidene fluoride membrane, which comprises the following specific steps: mixing N-N dimethylacetamide and polyvinylidene fluoride particles, carrying out ultrasonic treatment, stirring and heating treatment, standing, and condensing to obtain a membrane casting solution; vertically pulling the membrane casting solution to prepare a membrane, so as to obtain a wet polyvinylidene fluoride membrane; and dispersing nano zero-valent iron powder on the wet polyvinylidene fluoride membrane by utilizing high-voltage static electricity, standing and drying to obtain the nano iron-loaded polyvinylidene fluoride membrane. The nano-iron-loaded polyvinylidene fluoride membrane material prepared by the invention has the capabilities of adsorbing organic pollutants and reducing high-valence metal ions, and can be used for treating hexavalent chromium in industrial wastewater and water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heavy metal pollution repair materials, and in particular to a nano-iron-loaded polyvinylidene fluoride film and a preparation method thereof. Background Art

[0002] Chromium is widely recognized to be highly toxic to organisms and humans, and is biologically active in terrestrial and aquatic organisms. Due to its high toxicity and strong bioaccumulation, cadmium is classified as a Class I carcinogen. Compared with other heavy metals, cadmium is more soluble and mobile, causing it to be absorbed by plants, then transported and accumulated in different parts of edible plants, and finally enriched in the human body. The high toxicity of cadmium affects multiple organs in the human body and can cause cardiovascular, cerebrovascular and "Itai-itai" diseases.

[0003] In recent years, although improved methods such as sulfidation and porous material support have made great progress in improving the reaction activity and stability of nano-iron, it will be continuously consumed, quickly deactivated and produce a large amount of difficult-to-handle sludge during the treatment process. There has been a lack of effective solutions to this problem, which has become a bottleneck that seriously restricts its application and promotion. Microbial, photocatalytic, electrochemical and other methods have been applied to the reduction treatment of inactivated nano-iron, which has improved the recycling of nano-iron to a certain extent. However, the problem of low utilization efficiency of nano-iron still exists. Due to the toxicity of heavy metals, the strong dependence on light energy and the conductivity of electrochemistry on the carrier, membrane separation technology has been widely used in wastewater separation due to its low energy consumption and high separation efficiency. Traditional organic modified membranes have secondary pollution. Compared with other types of polymer membranes, polyvinylidene fluoride membranes have attracted widespread attention due to their thermal stability, chemical resistance and excellent mechanical strength. In addition, polyvinylidene fluoride membranes also have the advantage of being directly salvaged from the water body after use, simple post-use treatment, no secondary pollution, and easy recovery of separated products, so they are very suitable for the treatment of heavy metal pollution in wastewater. Summary of the invention

[0004] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a nano-iron-loaded polyvinylidene fluoride membrane and a preparation method thereof. By applying a constant electric field, the strong adsorption and strong reducing properties of nano zero-valent iron are utilized to prepare a reducing membrane with polyvinylidene fluoride as a carrier. The nano-iron-loaded polyvinylidene fluoride membrane material prepared by the present invention has the ability to adsorb organic pollutants and reduce high-valent metal ions, and can be used for the treatment of hexavalent chromium in industrial wastewater and water bodies.

[0005] Technical solution: The present invention provides a method for preparing a polyvinylidene fluoride film loaded with nano-iron, comprising the following steps: S1: mixing N-N-dimethylacetamide and polyvinylidene fluoride particles, subjecting them to ultrasonic treatment, stirring and heating, and then allowing them to stand and condense to obtain a casting solution; vertically pulling the casting solution to form a film to obtain a wet polyvinylidene fluoride film; S2: using high voltage static electricity to disperse nanometer zero-valent iron powder on the wet polyvinylidene fluoride membrane, allowing it to stand, and drying it to obtain a polyvinylidene fluoride membrane loaded with nanometer iron.

[0006] Furthermore, in S2, the high voltage static electricity is generated by a high voltage static electricity generator; the high voltage static electricity generator includes a DC voltage source and a boost module; the positive pole of the DC voltage source is connected to the powder tank through the boost module, and the negative pole of the DC voltage source is connected to the static adsorption area through the boost module.

[0007] Furthermore, the powder trough includes a side wall and a screen arranged below the side wall; wherein the side wall is an insulating material; and the screen is specifically a 150-200 mesh metal conductive screen.

[0008] Furthermore, the boost module includes a self-excited oscillation circuit and a voltage doubling circuit.

[0009] Furthermore, the wet polyvinylidene fluoride film is electrically connected to the high-voltage electrostatic generator through the electrostatic adsorption area.

[0010] Furthermore, the specific steps of dispersing the nano zero-valent iron powder on the wet polyvinylidene fluoride membrane by high voltage static electricity are as follows: Turn on the DC voltage source, adjust the voltage, place the powder trough close to the wet polyvinylidene fluoride membrane placed in the electrostatic adsorption area, then load the nano zero-valent iron powder into the powder trough, slowly shake the powder trough while making circular motions to disperse the nano zero-valent iron powder on the wet polyvinylidene fluoride membrane, then demold, let it stand, and vacuum dry to obtain the polyvinylidene fluoride membrane loaded with nano iron.

[0011] Furthermore, when the powder tank is shaken, the distance between the powder tank and the electrostatic adsorption area is 3-5 mm.

[0012] Further, in S1, the mass ratio of the NN dimethylacetamide to the polyvinylidene fluoride particles is 1:6-1:7; The mass ratio of the casting liquid to the nanometer zero-valent iron powder is 15:2-10:1.2.

[0013] Furthermore, in S2, the voltage of the high voltage static electricity is greater than 2000V.

[0014] Preferably, in S1, the specific conditions of the heating treatment are: heating temperature is 55-65°C, and heating time is 4-6h; In S2, the specific conditions of the drying are: drying temperature is 45-60°C, and drying time is 20-30 minutes.

[0015] Theoretical explanation: The present invention utilizes polyvinylidene fluoride membrane to load nano zero-valent iron, and utilizes a purely physical method of electric field regulation to evenly distribute the nano zero-valent iron on the polyvinylidene fluoride membrane. The principle is as follows: the nano zero-valent iron is charged after passing through a high-voltage electrostatic generator, and is embedded in the surface of the polyvinylidene fluoride membrane under the action of the electric field force and gravity. At the same time, due to the action of the electrostatic force, the nano iron itself will repel each other and can be evenly distributed on the polyvinylidene fluoride membrane, thereby improving the purity of the membrane. Compared with single nano iron, it also has the advantage of being easy to recycle. In addition, due to the electric field force in the vertical direction of electrostatic adsorption, the nano zero-valent iron will not be buried too deeply in the polyvinylidene fluoride membrane, thereby affecting its active sites, resulting in reduced adsorption and reduction effects.

[0016] Beneficial effects: Compared with the prior art, the specific beneficial effects of the present invention are as follows: (1) Inspired by electrostatic sand planting, the present invention uses electric field to drive the spraying of nano zero-valent iron onto the polyvinylidene fluoride membrane, laying an ideal material foundation for improving the utilization efficiency of nano zero-valent iron and in-situ regeneration of deactivated nano iron, and also provides a new solution for the treatment of chromium-containing wastewater; (2) The polyvinylidene fluoride membrane obtained by the present invention using a purely physical method can not only improve the economic benefits of treating chromium-containing wastewater, but also reduce chemical pollution. At the same time, because there is no chemical reaction involved, the purity of the membrane is further improved, greatly reducing the possibility of other ions affecting the pollution treatment; (3) The present invention solves the shortcomings of nano zero-valent iron, such as easy aggregation, oxidation, and instability. It can also be recycled to further increase the economic effect and be environmentally friendly. At the same time, it has low cost and high efficiency, and has good adsorption and reduction effects on chromium. It can be used for the repair of heavy metal chromium pollution in the environment and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a structural schematic diagram of the high voltage electrostatic generator in the present invention; Figure 2 This is a physical diagram of the high voltage electrostatic generator of the present invention; Figure 3 The circuit diagram of the boost module in the high-voltage electrostatic generator of the present invention; Figure 4 This is a surface scanning electron microscope image of a polyvinylidene fluoride membrane loaded with nano-iron prepared in Embodiment 2 of the present invention, magnified 5000 times; Figure 5 This is an XRD comparison diagram of the nano-iron loaded polyvinylidene fluoride film and the pure polyvinylidene fluoride film prepared in Embodiment 2 of the present invention; Figure 6This is a comparison chart of the removal rates of chromium-containing wastewater of a certain concentration by the nano-iron-loaded polyvinylidene fluoride membranes prepared in Embodiments 2, 3 and 4 of the present invention, and by pure polyvinylidene fluoride membranes and pure nano-iron; Illustration: 1. DC voltage source; 2. Booster module; 3. Powder tank; 4. Electrostatic adsorption area; 31. Side wall; 32. Screen. DETAILED DESCRIPTION

[0018] The present invention is described in detail below in conjunction with the embodiments.

[0019] Implementation 1: This embodiment provides a high voltage electrostatic generator, such as Figure 1-2 As shown, its specific structure is as follows: The high-voltage electrostatic generator is composed of a DC voltage source 1, a boost module 2, a powder tank 3 and an electrostatic adsorption area 4. Among them, the positive electrode of the DC voltage source 1 is connected to the powder tank 3 through the boost module 2, and the negative electrode of the DC voltage source 1 is connected to the electrostatic adsorption area 4 through the boost module 2. The powder tank 3 is an annular container, including a side wall 31 made of an insulating material and a screen 32 arranged under the side wall 31, and the screen 32 is specifically a 200-mesh metal conductive screen. The boost module 2 is composed of a self-excited oscillation circuit and a 4-fold voltage circuit, and its specific circuit diagram is shown in Figure 3 shown.

[0020] Optionally, the electrostatic adsorption area 4 can use an aluminum electrode plate; it can also use a glass plate. When a glass plate is used, the boost module 2 is connected to the glass plate through a metal conductive needle, and the metal conductive needle is in contact with the polyvinylidene fluoride membrane, so that when the high-voltage electrostatic generator is working, the polyvinylidene fluoride membrane and the boost module 2 are electrically connected.

[0021] Optionally, the size of the electrostatic adsorption area is 0.5mm*150mm*150mm.

[0022] Implementation 2: This embodiment provides a method for preparing a polyvinylidene fluoride film loaded with nano-iron by using the high-voltage electrostatic generator in Embodiment 1, and the specific operations are as follows: (1) Weigh 7 g of polyvinylidene fluoride particles and dissolve them in 85 g of NN-dimethylacetamide. Ultrasonicate for 10 min, heat at 60 °C with magnetic stirring for 6 h, seal the mixture, and let it stand for 4 h to degas. Then, obtain a casting solution. Take 1.5 g of the casting solution and place it on the electrostatic adsorption area. Use a 200 μm film forming device to vertically pull the film to obtain a wet polyvinylidene fluoride film. Place the film in the air for 20 s to stabilize it.

[0023] (2) The powder tank is placed close to the wet polyvinylidene fluoride membrane on the electrostatic adsorption area, and the distance between the powder tank and the wet polyvinylidene fluoride membrane is maintained at 5 mm. The DC voltage source is turned on and adjusted to the LV gear. In this embodiment, the number of coil turns in the self-excited oscillation circuit is 1:200. The input voltage of the DC voltage source is adjusted to 3V, and the output voltage is 3*200*4=2400V. Then, 0.5g of nano zero-valent iron powder is loaded into the powder tank of the high-voltage electrostatic generator, and the powder tank is slowly shaken while making a circular motion for 30 seconds to disperse the nano zero-valent iron powder on the wet polyvinylidene fluoride membrane. Finally, the wet polyvinylidene fluoride membrane dispersed with nano zero-valent iron powder is placed in deionized water for demolding, and after standing for 24 hours, it is fished out and vacuum dried at 40°C for 15 minutes to obtain a polyvinylidene fluoride membrane loaded with nano iron.

[0024] Implementation 3: This embodiment is substantially the same as Embodiment 2, except that in this embodiment, the input voltage of the DC voltage source is 5V, and the output voltage is 5*200*4=4000V.

[0025] Apart from this, this embodiment is completely the same as Embodiment 1 and will not be described in detail here.

[0026] Implementation 4: This embodiment is substantially the same as Embodiment 2, except that in this embodiment, the input voltage of the DC voltage source is 7.5V, and the output voltage is 7.5*200*4=6000V.

[0027] Apart from this, this embodiment is completely the same as Embodiment 1 and will not be described in detail here.

[0028] The nano-iron-loaded polyvinylidene fluoride membrane prepared in Embodiment 2 was analyzed: Figure 4 This is a 5000-fold magnified surface scanning electron microscope image of a polyvinylidene fluoride membrane loaded with nano-iron: It can be seen that the nano-zero-valent iron is dispersed and evenly distributed on the surface and does not appear in the pores of the polyvinylidene fluoride membrane.

[0029] Figure 5 This is the XRD comparison diagram of polyvinylidene fluoride membrane loaded with nano-iron and pure polyvinylidene fluoride membrane: It can be seen that after loading with nano-zero-valent iron, there is no obvious effect on the structure of the polyvinylidene fluoride membrane, and a unique peak of zero-valent iron appears at 45°-48°, indicating that the nano-zero-valent iron is successfully attached to the membrane surface.

[0030] The nano-iron-loaded polyvinylidene fluoride membranes prepared in Embodiment 2, Embodiment 3, and Embodiment 4 are compared and analyzed with the nano-iron and polyvinylidene fluoride membranes: Figure 6The comparison chart of the removal rate of chromium-containing wastewater of a certain concentration by the nano-iron loaded polyvinylidene fluoride membrane prepared in embodiments 2, 3 and 4 of the present invention, pure polyvinylidene fluoride membrane and pure nano-iron is as follows: It can be seen that the removal rate of Cr(VI) gradually increases with time and finally tends to be stable, and the removal rate of Example 4 with the largest input voltage reaches the highest removal rate of 94.22%, compared with the removal rate of nano-iron of only about 43%, and the removal rate of polyvinylidene fluoride membrane approaches 0%, indicating that the electrostatic adsorption method can make the nano zero-valent iron evenly dispersed on the surface of the polyvinylidene fluoride membrane, greatly improving its purification efficiency for chromium-containing wastewater.

[0031] In summary, the electrostatic adsorption method has effectively solved the shortcomings of easy agglomeration and instability of nano-zero-valent iron, and achieved its uniform and dispersed distribution on the polyvinylidene fluoride membrane. It can be used for the remediation of heavy metal chromium pollution in the environment and has good application prospects.

[0032] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyvinylidene fluoride film loaded with nano-iron, characterized in that: The following steps are involved: S1: mixing N-N-dimethylacetamide and polyvinylidene fluoride particles, subjecting them to ultrasonic treatment, stirring and heating, and then allowing them to stand and condense to obtain a casting solution; vertically pulling the casting solution to form a film to obtain a wet polyvinylidene fluoride film; S2: using high voltage static electricity to disperse nanometer zero-valent iron powder on the wet polyvinylidene fluoride membrane, allowing it to stand, and drying it to obtain a polyvinylidene fluoride membrane loaded with nanometer iron.

2. The method for preparing the nano-iron-loaded polyvinylidene fluoride film according to claim 1, characterized in that: In S2, the high-voltage static electricity is generated by a high-voltage static electricity generator; the high-voltage static electricity generator comprises a DC voltage source (1) and a boost module (2); the positive electrode of the DC voltage source (1) is connected to the powder tank (3) through the boost module (2), and the negative electrode of the DC voltage source (1) is connected to the static electricity adsorption area (4) through the boost module (2).

3. The method for preparing the nano-iron-loaded polyvinylidene fluoride film according to claim 2, characterized in that: The powder trough (3) comprises a side wall (31) and a screen (32) arranged below the side wall (31); wherein the side wall (31) is made of insulating material; and the screen (32) is specifically a 150-200 mesh metal conductive screen.

4. The method for preparing the nano-iron-loaded polyvinylidene fluoride film according to claim 2, characterized in that: The boost module (2) comprises a self-excited oscillation circuit and a voltage doubling circuit.

5. The method for preparing the nano-iron-loaded polyvinylidene fluoride film according to claim 2, characterized in that: The wet polyvinylidene fluoride membrane is electrically connected to the high-voltage electrostatic generator via the electrostatic adsorption area (4).

6. The method for preparing a nano-iron-loaded polyvinylidene fluoride membrane according to any one of claims 1 to 5, characterized in that: The specific steps of dispersing nano zero-valent iron powder on a wet polyvinylidene fluoride membrane by high voltage electrostatics are as follows: Turn on the DC voltage source (1), adjust the voltage, place the powder tank (3) close to the wet polyvinylidene fluoride membrane placed in the electrostatic adsorption area (4), then load the nano zero-valent iron powder into the powder tank (3), slowly shake the powder tank (3) while making a circular motion to disperse the nano zero-valent iron powder on the wet polyvinylidene fluoride membrane, then demould, let it stand, and vacuum dry to obtain the polyvinylidene fluoride membrane loaded with nano iron.

7. The method for preparing the nano-iron loaded polyvinylidene fluoride membrane according to claim 6, characterized in that: When the powder tank (3) is shaken, the distance between the powder tank (3) and the electrostatic adsorption area (4) is 3-5 mm.

8. The method for preparing the nano-iron loaded polyvinylidene fluoride membrane according to claim 1, characterized in that: In S1, the mass ratio of the NN dimethylacetamide to the polyvinylidene fluoride particles is 1:6-1:7; The mass ratio of the casting liquid to the nanometer zero-valent iron powder is 15:2-10:1.

2.

9. The method for preparing the nano-iron loaded polyvinylidene fluoride film according to claim 1, characterized in that: In S2, the voltage of the high voltage static electricity is greater than 2000V.

10. The method for preparing the nano-iron loaded polyvinylidene fluoride film according to claim 1, characterized in that: In S1, the specific conditions of the heating treatment are: heating temperature is 55-65°C, and heating time is 4-6h; In S2, the specific conditions of the drying are: drying temperature is 45-60°C, and drying time is 20-30 minutes.

Citation Information

Cited By

  • Zero-valent iron protection catalytic membrane as well as preparation method and application thereof

    CN120618528A

  • Method for in-situ regeneration and inactivation of nZVI through electron beam irradiation and nanoscale zero-valent iron film

    CN121158884A