Preparation method of copper ion adsorption material for sewage treatment
By forming a linear polyacrylamide layer on a sponge iron matrix and then performing cross-linking and functionalization treatments, a highly efficient copper ion adsorption material was prepared, which solved the problems of low copper ion adsorption rate and unsatisfactory removal efficiency in the existing technology, and realized highly efficient copper ion removal for industrial applications.
Patent Information
- Application Number
- CN202411256710.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
Existing adsorption materials have low copper ion adsorption rates and unsatisfactory removal efficiency when treating copper-containing wastewater, which cannot meet the requirements for industrial applications.
By forming a linear polyacrylamide (PAM) layer on the surface of a sponge iron matrix and converting it into a malonyl crosslinked polyacrylamide (PAM-C3H2O2-PAM) network crosslinked layer through a crosslinking reaction, and then performing [Mn(CO)5]-functionalization, an adsorbent material with excellent copper ion removal efficiency and wide pH applicability stability was prepared.
The material achieves efficient adsorption of copper ions over a wide pH range, significantly improving the copper ion removal rate and adsorption rate, thus meeting the needs of industrial applications.
Smart Images

Figure CN119034697A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sewage treatment adsorption materials, in particular to a method for preparing a copper ion adsorption material for sewage treatment. Background Art
[0002] A large amount of copper ion wastewater is generated in the production process of chemical industry, electroplating, mining, electronics and printing and dyeing enterprises. Copper ion wastewater is difficult to degrade and is easy to migrate and enrich. Since copper ion wastewater pollutes the environment, animals are prone to ingest excessive copper ions through the food chain, which causes them to accumulate in the animal body, thus causing toxicity to the animal body, such as inhibiting the activity of copper-containing enzymes, changing protein structure, damaging the blood system, and causing cancer. In addition, copper ions enriched in copper ion wastewater will harm plant growth and development and metabolic processes.
[0003] At present, the methods for removing copper ions from wastewater containing copper ions include membrane separation, ion exchange, coagulation and adsorption. The membrane separation method has the disadvantages of high cost and serious membrane pollution, while the ion exchange method has the disadvantages of long treatment cycle, large amount of product waste liquid, organic pollution, etc. The coagulation method has the disadvantages of secondary pollution caused by the addition of chemicals, the generation of suspended solids and long treatment cycle. The adsorption method has the advantages of short treatment cycle, no need to add chemicals, simple operation and controllable cost, and is an effective means of treating wastewater containing copper ions.
[0004] However, the current adsorption rate of copper ions in treating copper ion-containing wastewater by adsorption materials is low, and the copper ion removal efficiency is not ideal, which cannot meet the requirements of industrial applications. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a copper ion adsorption material for sewage treatment. The adsorption material prepared by the method has excellent copper ion removal efficiency, outstanding copper ion adsorption rate and wide pH applicable stability.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] The present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0008] Step [1] forming a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate;
[0009] Step [2] converting the linear polyacrylamide (PAM) layer into a malonyl cross-linked polyacrylamide (PAM-C3H2O2-PAM) network cross-linked layer through a cross-linking reaction;
[0010] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5]- Functionalization is performed to finally obtain the adsorption material.
[0011] Preferably, the step [1] specifically includes the following operations:
[0012] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base liquid; add ethyl mercaptan to anhydrous ethanol and mix to form an additive liquid; add a certain amount of the additive liquid to the base liquid and mix to form a PAM synthetic liquid;
[0013] a2. Immerse the sponge iron sample in the PAM synthesis solution, heat it in a water bath to 35-50°C, and react at a constant temperature for 7-10 hours to obtain a sponge iron having a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0014] Preferably, in step a1, the concentration of acrylamide in the base liquid is 230 g / L-260 g / L, the concentration of peroxyformic acid is 30 mL / L-70 mL / L, the concentration of glucose is 80 g / L-120 g / L, and the concentration of ammonium sulfite is 50 g / L-80 g / L; the concentration of ethyl mercaptan in the additive liquid is 90 mL / L-120 mL / L; and the volume ratio between the additive liquid and the base liquid in the PAM synthetic liquid is 1-3:5-7.
[0015] Preferably, in step a2, the weight of the sponge iron immersed in each liter of the PAM synthetic liquid is 80-110 g.
[0016] Preferably, the step [2] specifically includes the following operations:
[0017] b1. Add malonic acid, citric acid and ferrous sulfate to deionized water and mix to form a cross-linking solution;
[0018] b2. Immerse the intermediate A in the cross-linking solution and react at room temperature for 2-4 hours to obtain a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0019] Preferably, in step b1, the concentration of malonic acid in the cross-linking solution is 160 g / L-200 g / L, the concentration of citric acid is 100 g / L-130 g / L, and the concentration of ferrous sulfate is 20 g / L-40 g / L.
[0020] Preferably, in step b2, the weight of the intermediate A immersed in each liter of the cross-linking solution is 170-230 g.
[0021] Preferably, the step [3] specifically includes the following operations:
[0022] c1. adding ammonium nitrate and urea to deionized water to form a precursor solution; immersing the intermediate B in the precursor solution and reacting at room temperature for 20-24 hours to obtain an intermediate C;
[0023] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized solution; immerse the intermediate C in the functionalized solution, heat to 30-55°C in a water bath, and react at a constant temperature for 12-16 hours to complete [Mn(CO)5] - Functional operation.
[0024] Preferably, in step c1, the ammonium nitrate concentration of the precursor solution is 60 g / L-100 g / L, and the urea concentration is 40 g / L-70 g / L; the weight of the intermediate B immersed in each liter of the precursor solution is 90-140 g.
[0025] Preferably, in step c2, the amount of manganese bromide pentacarbonyl added to each liter of the functionalization liquid is 180 g-210 g; and the weight of the intermediate C immersed in each liter of the functionalization liquid is 50-80 g.
[0026] The positive effects of the present invention are as follows: the copper ion adsorption material (sponge iron-based manganese complex ion-functionalized malonyl cross-linked polyacrylamide) prepared by the method of the present invention has the following structural characteristics: acrylamide monomer is polymerized on the surface of the sponge iron matrix to form linear polyacrylamide, and then cross-linked polyacrylamide is formed by polycondensation with malonic acid; manganese complex ions [Mn(CO)5] are introduced by utilizing the chemical activity of the amide group of the cross-linked polyacrylamide. - Based on the above structural characteristics, the prepared adsorbent material is stable in a wide pH range and has excellent hydrophilicity, so that it has a good wetting effect on wastewater containing copper ions; at the same time, its amide group and [Mn(CO)5] - The ligand ion has a strong affinity for copper ions and can effectively promote the adsorption of copper ions.
[0027] In summary, the copper ion adsorption material prepared according to the present invention has excellent copper ion removal efficiency, outstanding copper ion adsorption rate and wide pH applicability stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the preparation process of the copper ion adsorption material of the present invention;
[0029] Figure 2 It is NO3 - Schematic diagram of the structure of ion-modified PAM-C3H2O2-PAM precursor;
[0030] Figure 3It is a schematic diagram of the structure of manganese ion functionalized cross-linked polyacrylamide;
[0031] Figure 4 It is a graph showing the change of copper ion adsorption removal rate over time in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention when treating simulated sewage;
[0032] Figure 5 Comparison of copper ion adsorption removal rates under different pH conditions among Example 1, Comparative Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0033] Reference Figure 1 The present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0034] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0035] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 230 g / L-260 g / L, a peroxyformic acid concentration of 30 mL / L-70 mL / L, a glucose concentration of 80 g / L-120 g / L and an ammonium sulfite concentration of 50 g / L-80 g / L; add ethyl mercaptan to anhydrous ethanol to form an additive solution having an ethyl mercaptan concentration of 90 mL / L-120 mL / L; add the additive solution to the base solution in a volume ratio of 1 to 3:5 to 7 to form a PAM synthetic solution;
[0036] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 80-110 g), heat it in a water bath to 35-50°C, and react at a constant temperature for 7-10 hours to obtain a sponge iron having a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0037] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0038] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 160g / L-200g / L, a citric acid concentration of 100g / L-130g / L and a ferrous sulfate concentration of 20g / L-40g / L;
[0039] b2. Immerse the intermediate A in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 170-230 g), and react at room temperature for 2-4 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0040] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5] - Functionalization, including the following operations:
[0041] c1. Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 60 g / L-100 g / L and a urea concentration of 40 g / L-70 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 90-140 g), and react at room temperature for 20-24 hours to obtain NO3 on the surface of the sponge iron substrate. - Ion-modified malonyl polyacrylamide precursor (schematic structure as shown in Figure 2 As shown), intermediate C is obtained;
[0042] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized liquid (the amount of pentacarbonyl manganese bromide added to each liter of the functionalized liquid is 180 g-210 g); immerse the intermediate C in the functionalized liquid (the weight of the intermediate C immersed in each liter of the functionalized liquid is 50-80 g), heat to 30-55° C. in a water bath, and react at a constant temperature for 12-16 hours to complete the [Mn(CO)5] of the malonyl polyacrylamide. - Functionalization operation (the structure of manganese ion functionalized cross-linked polyacrylamide is shown in the figure below) Figure 3 As shown), the copper ion adsorption material (sponge iron with manganese ligand ion functionalized malonyl cross-linked polyacrylamide loaded on the surface) is finally obtained.
[0043] The preferred embodiments of the present invention are described below by way of example.
[0044] Example 1
[0045] Preferred embodiment 1 of the present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0046] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0047] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 252 g / L, a peroxyformic acid concentration of 65 mL / L, a glucose concentration of 115 g / L and an ammonium sulfite concentration of 70 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 115 mL / L of an additive solution; add the additive solution to the base solution in a volume ratio of 2:7 to form a PAM synthetic solution;
[0048] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 105 g), heat it to 50°C in a water bath, and react at a constant temperature for 9 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0049] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0050] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 190 g / L, a citric acid concentration of 120 g / L and a ferrous sulfate concentration of 40 g / L;
[0051] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 225 g), and reacted at room temperature for 4 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0052] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5] - Functionalization, including the following operations:
[0053] c1. Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 90 g / L and a urea concentration of 70 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 120 g), and react at room temperature for 24 hours to obtain NO3 on the surface of the sponge iron substrate. - Ion-modified malonyl polyacrylamide precursor to obtain intermediate C;
[0054] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized liquid (the amount of pentacarbonyl manganese bromide added to each liter of the functionalized liquid is 200 g); immerse the intermediate C in the functionalized liquid (the weight of the intermediate C immersed in each liter of the functionalized liquid is 70 g), heat to 45° C. in a water bath, and react at a constant temperature for 14 hours to complete the [Mn(CO)5] of malonyl polyacrylamide. - Functionalization operation was performed to finally obtain the copper ion adsorption material (sponge iron with manganese ligand ion functionalized malonyl cross-linked polyacrylamide loaded on the surface), which is recorded as Example 1.
[0055] Comparative Example 1
[0056] This comparative example 1 provides a method for preparing an adsorbent material, comprising the following steps:
[0057] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0058] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 240 g / L, a peroxyformic acid concentration of 35 mL / L, a glucose concentration of 90 g / L and an ammonium sulfite concentration of 60 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 100 mL / L of the additive solution; add the additive solution to the base solution in a volume ratio of 2:5 to form a PAM synthetic solution;
[0059] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 100 g), heat it to 40°C in a water bath, and react at a constant temperature for 8 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0060] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0061] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 170 g / L, a citric acid concentration of 120 g / L and a ferrous sulfate concentration of 30 g / L;
[0062] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 180 g), and reacted at room temperature for 2 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0063] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to NO3 - Ion modification includes the following operations:
[0064] Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 70 g / L and a urea concentration of 50 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 100 g), and react at room temperature for 20 hours to obtain NO3 on the surface of the sponge iron matrix. - The ion-modified malonyl polyacrylamide precursor and the finally obtained sponge iron adsorption material are recorded as Comparative Example 1.
[0065] Comparative Example 2
[0066] This comparative example 2 provides a method for preparing an adsorbent material, comprising the following steps:
[0067] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0068] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 255 g / L, a peroxyformic acid concentration of 40 mL / L, a glucose concentration of 100 g / L and an ammonium sulfite concentration of 60 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 110 mL / L of the additive solution; add the additive solution to the base solution in a volume ratio of 3:5 to form a PAM synthetic solution;
[0069] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 95 g), heat it to 40°C in a water bath, and react at a constant temperature for 9 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0070] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0071] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 185 g / L, a citric acid concentration of 120 g / L and a ferrous sulfate concentration of 30 g / L;
[0072] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 210 g), and reacted at room temperature for 4 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is the adsorption material, recorded as Comparative Example 2.
[0073] In order to analyze the adsorption performance of Example 1, Comparative Example 1 and Comparative Example 2 in treating wastewater containing copper ions, copper sulfate was added to deionized water to prepare a solution with a copper sulfate concentration of 20 mg / L as simulated sewage. The pH value of the simulated sewage prepared above was adjusted with hydrochloric acid and sodium hydroxide to obtain simulated sewage with pH values of 7, 8, 9 and 10, respectively. 30 g of sewage treatment material (i.e., Example 1, Comparative Example 1 and Comparative Example 2) was placed in each liter of simulated sewage for copper ion adsorption treatment. The treatment time was 50 min, and the adsorption removal rate of copper ions was calculated by the residual copper ion concentration in the simulated sewage. Under the condition of a pH value of 8, the change of the copper ion adsorption removal rate over time during the treatment of copper ion-containing sewage for 50 minutes using Example 1, Comparative Example 1 and Comparative Example 2 is shown as follows. Figure 4 As shown in the figure, Example 1 achieved a copper ion adsorption removal rate of 92% in the 18th minute. 2+ The adsorption removal rate and removal rate are significantly higher than those of Comparative Example 1 and Comparative Example 2, indicating that Example 1 has an excellent copper ion adsorption removal rate and a high copper ion adsorption rate. Under the conditions of pH values of 7, 8, 9 and 10, after Example 1, Comparative Example 1 and Comparative Example 2 treated the simulated sewage for 50 minutes, the corresponding copper ion removal rates are as follows: Figure 5 As shown in Example 1, the pH values of Cu at 7, 8, 9 and 10 were 2+ The removal rates of Cu in Comparative Examples 1 and 2 were all greater than 90%. 2+ The removal rate of Cu in Comparative Examples 1 and 2 is not only significantly lower than that in Example 1, but also 2+ The adsorption performance of Cu 2+ The adsorption removal rate was significantly reduced.
[0074] In summary, the copper ion adsorption material prepared according to the present invention has excellent copper ion removal efficiency, outstanding copper ion adsorption rate and wide pH applicability stability.
[0075] To illustrate in further detail, three additional examples are provided below.
[0076] Example 2
[0077] Preferred embodiment 2 of the present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0078] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0079] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 230 g / L, a peroxyformic acid concentration of 30 mL / L, a glucose concentration of 120 g / L and an ammonium sulfite concentration of 50 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 90 mL / L of an additive solution; add the additive solution to the base solution in a volume ratio of 1:5 to form a PAM synthetic solution;
[0080] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 80 g), heat it to 50°C in a water bath, and react at a constant temperature for 7 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0081] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0082] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 160 g / L, a citric acid concentration of 130 g / L and a ferrous sulfate concentration of 20 g / L;
[0083] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 170 g), and reacted at room temperature for 2 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0084] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5] - Functionalization, including the following operations:
[0085] c1. Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 60 g / L and a urea concentration of 40 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 90 g), and react at room temperature for 20 hours to obtain NO3 on the surface of the sponge iron substrate. - Ion-modified malonyl polyacrylamide precursor to obtain intermediate C;
[0086] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized liquid (the amount of pentacarbonyl manganese bromide added to each liter of the functionalized liquid is 210 g); immerse the intermediate C in the functionalized liquid (the weight of the intermediate C immersed in each liter of the functionalized liquid is 80 g), heat to 30° C. in a water bath, and react at a constant temperature for 16 hours to complete the [Mn(CO)5] of malonyl polyacrylamide. - Functionalization operation is performed to finally obtain the copper ion adsorption material (sponge iron with manganese ligand ion functionalized malonyl cross-linked polyacrylamide loaded on the surface).
[0087] Example 3
[0088] Preferred embodiment 3 of the present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0089] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0090] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 260 g / L, a peroxyformic acid concentration of 70 mL / L, a glucose concentration of 80 g / L and an ammonium sulfite concentration of 80 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 120 mL / L of an additive solution; add the additive solution to the base solution in a volume ratio of 3:7 to form a PAM synthetic solution;
[0091] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 110 g), heat it to 35°C in a water bath, and react at a constant temperature for 10 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0092] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0093] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 200 g / L, a citric acid concentration of 100 g / L and a ferrous sulfate concentration of 40 g / L;
[0094] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 230 g), and reacted at room temperature for 4 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0095] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5] - Functionalization, including the following operations:
[0096] c1. Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 100 g / L and a urea concentration of 70 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 140 g), and react at room temperature for 24 hours to obtain NO3 on the surface of the sponge iron substrate. - Ion-modified malonyl polyacrylamide precursor to obtain intermediate C;
[0097] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized liquid (the amount of pentacarbonyl manganese bromide added to each liter of the functionalized liquid is 180 g); immerse the intermediate C in the functionalized liquid (the weight of the intermediate C immersed in each liter of the functionalized liquid is 50 g), heat to 55° C. in a water bath, and react at a constant temperature for 12 hours to complete the [Mn(CO)5] - Functionalization operation is performed to finally obtain the copper ion adsorption material (sponge iron with manganese ligand ion functionalized malonyl cross-linked polyacrylamide loaded on the surface).
[0098] Example 4
[0099] Preferred embodiment 4 of the present invention provides a method for preparing a copper ion adsorption material for sewage treatment, comprising the following steps:
[0100] Step [1] forms a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate, specifically comprising the following operations:
[0101] a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base solution having an acrylamide concentration of 245 g / L, a peroxyformic acid concentration of 50 mL / L, a glucose concentration of 100 g / L and an ammonium sulfite concentration of 65 g / L; add ethyl mercaptan to anhydrous ethanol to form an ethyl mercaptan concentration of 105 mL / L of the additive solution; add the additive solution to the base solution in a volume ratio of 2:6 to form a PAM synthetic solution;
[0102] a2. Immerse the sponge iron sample in the PAM synthetic solution (the weight of the sponge iron immersed in each liter of the PAM synthetic solution is 95 g), heat it to 42°C in a water bath, and react at a constant temperature for 9 hours to obtain a sponge iron with a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
[0103] Step [2] converting the linear polyacrylamide PAM layer into a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer through a cross-linking reaction, specifically comprising the following operations:
[0104] b1. Malonic acid, citric acid and ferrous sulfate were added to deionized water and mixed to form a cross-linking solution having a malonic acid concentration of 180 g / L, a citric acid concentration of 115 g / L and a ferrous sulfate concentration of 30 g / L;
[0105] b2. The intermediate A is immersed in the cross-linking solution (the weight of the intermediate A immersed in each liter of the cross-linking solution is 200 g), and reacted at room temperature for 3 hours to convert the linear polyacrylamide PAM into malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM through a cross-linking reaction, thereby obtaining a sponge iron having a malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM network cross-linked layer formed on the surface, which is recorded as intermediate B.
[0106] Step [3]: subjecting the malonyl cross-linked polyacrylamide PAM-C3H2O2-PAM to [Mn(CO)5] - Functionalization, including the following operations:
[0107] c1. Add ammonium nitrate and urea to deionized water to form a precursor solution with an ammonium nitrate concentration of 80 g / L and a urea concentration of 55 g / L; immerse the intermediate B in the precursor solution (the weight of the intermediate B immersed in each liter of the precursor solution is 115 g), and react at room temperature for 22 hours to obtain NO3 on the surface of the sponge iron substrate. - Ion-modified malonyl polyacrylamide precursor to obtain intermediate C;
[0108] c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized liquid (the amount of pentacarbonyl manganese bromide added to each liter of the functionalized liquid is 195 g); immerse the intermediate C in the functionalized liquid (the weight of the intermediate C immersed in each liter of the functionalized liquid is 65 g), heat to 45° C. in a water bath, and react at a constant temperature for 14 hours to complete the [Mn(CO)5] - Functionalization operation is performed to finally obtain the copper ion adsorption material (sponge iron with manganese ligand ion functionalized malonyl cross-linked polyacrylamide loaded on the surface).
[0109] The above are only preferred embodiments of the present invention. It should be understood that the description of the above embodiments is only used to help understand the method and core ideas of the present invention, and is not used to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, etc. made within the ideas and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a copper ion adsorption material for sewage treatment, It is characterized in that The following steps are included: Step [1] forming a linear polyacrylamide (PAM) layer on the surface of the sponge iron substrate; Step [2] converting the linear polyacrylamide PAM layer into malonyl cross-linked polyacrylamide PAM-C through a cross-linking reaction 3 H 2 O 2 -PAM network cross-linked layer; Step [3]: cross-linking the malonyl polyacrylamide PAM-C 3 H 2 O 2 -PAM for [Mn(CO) 5 ] - Functionalization is performed to finally obtain the adsorption material.
2. A method for preparing a copper ion adsorption material for sewage treatment according to claim 1, It is characterized in that The step [1] specifically includes the following operations: a1. Add acrylamide, peroxyformic acid, glucose and ammonium sulfite to deionized water and mix to form a base liquid; add ethyl mercaptan to anhydrous ethanol and mix to form an additive liquid; add a certain amount of the additive liquid to the base liquid and mix to form a PAM synthetic liquid; a2. Immerse the sponge iron sample in the PAM synthesis solution, heat it in a water bath to 35-50°C, and react at a constant temperature for 7-10 hours to obtain a sponge iron having a linear polyacrylamide PAM layer formed on the surface, which is recorded as intermediate A.
3. A method for preparing a copper ion adsorbent material for sewage treatment according to claim 2, Features: In step a1, the concentration of acrylamide in the base liquid is 230g / L-260g / L, the concentration of peroxyformic acid is 30mL / L-70mL / L, the concentration of glucose is 80g / L-120g / L, and the concentration of ammonium sulfite is 50g / L-80g / L; the concentration of ethyl mercaptan in the additive liquid is 90mL / L-120mL / L; and the volume ratio between the additive liquid and the base liquid in the PAM synthetic liquid is 1-3:5-7.
4. A method for preparing a copper ion adsorption material for sewage treatment according to claim 2, Features: In step a2, the weight of the sponge iron immersed in each liter of the PAM synthetic liquid is 80-110 g.
5. A method for preparing a copper ion adsorption material for sewage treatment according to claim 1, It is characterized in that The step [2] specifically includes the following operations: b1. Add malonic acid, citric acid and ferrous sulfate to deionized water and mix to form a cross-linking solution; b2. Immersing the intermediate A in the crosslinking solution and reacting at room temperature for 2-4 hours to obtain a surface having malonyl crosslinked polyacrylamide PAM-C 3 H 2 O 2 -PAM network cross-linked layer of sponge iron, denoted as intermediate B.
6. A method for preparing a copper ion adsorption material for sewage treatment according to claim 5, Features: In step b1, the concentration of malonic acid in the cross-linking solution is 160 g / L-200 g / L, the concentration of citric acid is 100 g / L-130 g / L, and the concentration of ferrous sulfate is 20 g / L-40 g / L.
7. A method for preparing a copper ion adsorption material for sewage treatment according to claim 5, Features: In step b2, the weight of the intermediate A immersed in each liter of the cross-linking solution is 170-230 g.
8. A method for preparing a copper ion adsorbent material for sewage treatment according to claim 1, It is characterized in that The step [3] specifically includes the following operations: c1. adding ammonium nitrate and urea to deionized water to form a precursor solution; immersing the intermediate B in the precursor solution and reacting at room temperature for 20-24 hours to obtain an intermediate C; c2. Add pentacarbonyl manganese bromide to N-methylpyrrolidone and mix to form a functionalized solution; immerse the intermediate C in the functionalized solution, heat to 30-55°C in a water bath, and react at a constant temperature for 12-16 hours to complete [Mn(CO) 5 ] - Functional operation.
9. A method for preparing a copper ion adsorption material for sewage treatment according to claim 8, Features: In step c1, the ammonium nitrate concentration of the precursor solution is 60g / L-100g / L, and the urea concentration is 40g / L-70g / L; the weight of the intermediate B immersed in each liter of the precursor solution is 90-140g.
10. The method for preparing a copper ion adsorption material for sewage treatment according to claim 8, Features: In step c2, the amount of manganese bromide pentacarbonyl added to each liter of the functionalization liquid is 180 g-210 g; the weight of the intermediate C immersed in each liter of the functionalization liquid is 50-80 g.