Ni-Sn-coated C-SDB catalyst, application thereof and method for catalyzing aqueous-phase catalytic synthesis of high alcohols from ethanol by using Ni-Sn-coated C-SDB catalyst

By combining Ni-Sn@C-SDB catalyst with ball milling technology, the problems of catalyst water poisoning and numerous side reactions were solved, achieving highly efficient catalytic synthesis of higher alcohols from ethanol, with high selectivity and low cost.

CN119034756AActive Publication Date: 2024-11-29GUANGDONG UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411143738.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Existing catalysts suffer from problems such as water poisoning and deactivation, numerous side reactions, weak catalytic activity, and high cost during alcohol coupling, making it difficult to efficiently catalyze the synthesis of higher alcohols from ethanol.

Method used

By employing Ni-Sn@C-SDB catalyst, the Ni-Sn bimetallic catalyst is combined with hydrophobic styrene-divinylbenzene copolymer SDB through ball milling, thereby improving the hydrophobic properties of the catalyst and promoting the coupling of lower alcohols to higher alcohols.

Benefits of technology

It improves ethanol conversion and selectivity for higher alcohols, reduces catalyst deactivation, lowers costs, and exhibits excellent catalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034756A_ABST
    Figure CN119034756A_ABST
Patent Text Reader

Abstract

The invention discloses a Ni-Sn-coated C-SDB catalyst and application thereof and a method for catalyzing ethanol water-phase catalytic synthesis of high alcohols, the catalyst is obtained by ball-milling a Ni-Sn bimetallic catalyst and a hydrophobic polymer SDB to prepare NiSn-coated C-SDB, and the hydrophobic degree of the catalyst is greatly increased by ball-milling the hydrophobic polymer; and the phenomenon of inactivation caused by'water poisoning 'due to dehydration in aldol condensation reaction and blockage of pore channels in the catalyst caused by water molecules in reaction raw materials in the reaction process is reduced. When the catalyst is applied to a reaction for catalyzing aqueous-phase ethanol to synthesize higher alcohols in one step, the catalyst shows excellent catalytic efficiency, higher reaction activity, higher ethanol conversion rate and higher selectivity to C6 + higher alcohols; the catalyst is simple to prepare and low in cost, the reaction performance of the catalyst is improved through simple ball milling, and production and application of the catalyst are facilitated; belongs to the technical field of catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst, in particular to a Ni-Sn@C-SDB catalyst. The present invention also relates to the application of the Ni-Sn@C-SDB catalyst and a method for catalyzing ethanol aqueous phase catalytic synthesis of higher carbon alcohols. Technical Background

[0002] At present, environmental problems are becoming increasingly serious mainly because of the excessive consumption of fossil resources. The supply of traditional energy is facing tremendous pressure, which has triggered people's increasing attention to renewable energy and accelerated energy transformation. Biomass is recognized as the only renewable carbon resource. The use of biomass is of great significance for sustainable alternative energy and reducing carbon emissions. Due to the long history of industrial fermentation production, ethanol extracted from biomass sugar has been identified as the most successful commercial biofuel among existing alternative biofuels, accounting for the largest share of global biofuel production and consumption. Blending ethanol into motor gasoline can replace pure fossil fuels, provide additional oxygen, improve combustion performance, thereby improving engine performance and reducing pollutant emissions. Although fuel ethanol has many advantages, its inherent disadvantages such as low cetane number (11), low energy density (26MJ / kg), high autoignition temperature (420℃), and high hygroscopicity have hindered its widespread application in diesel engines. Compared with ethanol, high carbon alcohols (such as isoheptanol) have higher cetane number (≥17), higher energy density (≥32MJ / kg), lower autoignition temperature (≤345℃), lower hygroscopicity and better compatibility with traditional fuel systems, making them ideal diesel additives.

[0003] In the Guerbet coupling process of low-order alcohols, the main reaction of chain propagation is carried out through a series of cascade steps, including the initial dehydrogenation of alcohols to form aldehydes, the subsequent aldol self-condensation / cross-condensation and dehydration, and the final hydrogenation of unsaturated condensation products to form saturated higher-order alcohols. Guerbet coupling provides an atom- and step-economical strategy, using abundant fuel ethanol, mainly studying the coupling between isopentanol and ethanol in fuel ethanol to form high-carbon isomeric alcohols. Aldol condensation usually requires alkaline condensation agents and hydrogenation / dehydrogenation metal catalysts. In the second step of the Guerbet coupling process, aldol self-condensation / cross-condensation and dehydration are carried out, which will produce water molecules, which will enter the internal pores of the catalyst, block the reaction site, and cause "water poisoning" and rapid deactivation. Therefore, higher requirements are placed on the hydrophobic properties of the catalyst.

[0004] In the past few decades, people have extensively explored heterogeneous catalysts for alcohol coupling. Initially, bifunctional catalysts with acid and base sites (such as MgO, MgAlO, HAP, etc.) were used to complete the alcohol coupling process. However, due to the weak catalytic activity of the catalyst, a high reaction temperature of more than 300°C is required, which usually leads to excessive side reactions, such as dehydration or decomposition of alcohols, reducing the yield of high alcohols (less than 20%). In order to address these shortcomings, the introduction of transition metal promoters with dehydrogenation functions (such as Ru, Rh, Pd, Pt, Au, Ni, Cu, etc.) combined with homogeneous bases can also very effectively accelerate the coupling reaction rate. In particular, compared with precious metal catalysts, nickel-based catalysts have been widely studied in ethanol coupling because of their low cost and easy availability.

[0005] Compared with rare noble metals such as Pd and Ru, transition metal Ni is abundant and has good catalytic performance in many typical reactions. Therefore, Ni-based non-noble metal catalysts can well replace noble metal catalysts, reduce catalyst costs and improve economic benefits. At the same time, although Ni-based metal catalysts have excellent catalytic activity for alcohol dehydrogenation and hydrogenation reactions, the selectivity of by-products is too high due to the strong CC bond breaking ability of Ni-based single metal catalysts. Summary of the invention

[0006] In order to overcome the deficiencies of the above-mentioned prior art, the first object of the present invention is to propose a Ni-Sn@C-SDB catalyst. The Ni-Sn bimetallic catalyst is simply ball-milled with a hydrophobic styrene-divinylbenzene copolymer to improve the hydrophobic properties of a simple Ni-Sn carbon-coated catalyst, thereby promoting the further coupling of low-carbon alcohols to higher alcohols. The ball-milled catalyst has improved ethanol conversion rate and selectivity for C6+ alcohol products for the synthesis of higher-carbon alcohols by ethanol coupling.

[0007] The second object of the present invention is to provide a method for synthesizing higher carbon alcohols from ethanol in aqueous phase catalyzed by a Ni-Sn@C-SDB catalyst, wherein the catalyst catalyzes the further coupling of low carbon alcohols to higher alcohols, and the ball-milled catalyst improves the ethanol conversion rate and the selectivity of C6+ alcohol products for the synthesis of higher carbon alcohols from ethanol coupling.

[0008] To this end, the first technical solution provided by the present invention is as follows:

[0009] A Ni-Sn@C-SDB catalyst is prepared by ball milling using a Ni-Sn bimetallic catalyst and a hydrophobic polymer SDB;

[0010] The mass ratio of the Ni-Sn bimetallic catalyst to the hydrophobic polymer SDB is 1:(0.5-3).

[0011] The ball milling time is 3-5h, and the ball milling rate is 100-500rpm; more preferably, the ball milling time is 4h, and the ball milling rate is 300rpm;

[0012] Furthermore, the mass ratio of the NiSn@C catalyst and the hydrophobic polymer SDB used in ball milling is preferably 1:1.

[0013] Furthermore, the Ni-Sn@C-SDB catalyst is prepared by the following method:

[0014] S1, dissolving nickel salt, tin salt and carbon source precursor in a solvent, stirring at room temperature to form a complex to obtain a homogeneous solution, and then heating and stirring to form a nickel-tin bimetallic catalyst gel precursor;

[0015] The molar ratio of Ni / Sn in the nickel salt and the tin salt is (1-30):1, and the molar ratio of Ni in the nickel salt to the carbon source precursor is 1:(0.2-5);

[0016] S2, placing the nickel-tin bimetallic catalyst gel precursor prepared in S1 in an inert gas atmosphere at 1-10°C

[0017] A controlled high-temperature self-reduction carbonization reaction is carried out at 400-700°C for 2-4 hours at a heating rate of 1 / min to obtain a Ni-Sn bimetallic carbon-coated bimetallic catalyst.

[0018] Furthermore, the nickel salt includes nickel nitrate, nickel chloride, nickel acetate, nickel hydroxide, preferably nickel nitrate.

[0019] Furthermore, the tin salt includes tin nitrate, tin citrate, tin chloride, preferably tin chloride.

[0020] Furthermore, the preferred molar ratio of Ni / Sn in the nickel salt and the tin salt is 20:1.

[0021] Furthermore, the carbon source precursor is an organic compound containing C, H, and O that can be complexed with nickel and tin metal ions, preferably citric acid, and the molar ratio of Ni in the nickel salt to the carbon source precursor is 1:2.

[0022] Furthermore, the temperature of the controlled high temperature self-reduction carbonization reaction is 500-600°C, and the reaction time is 2-4 hours; more preferably, the reaction time is 550°C for 2 hours.

[0023] Furthermore, the heating rate of the controlled high temperature self-reduction carbonization reaction is 1-10°C / min. When the heating rate is controlled within this range, the average particle size of the obtained catalyst is smaller and more uniform, and more preferably 2-5°C / min.

[0024] Furthermore, in the above-mentioned Ni-Sn@C-SDB catalyst, the hydrophobic polymer SDB is prepared by the following method:

[0025] S1. Styrene (St) monomer needs to be refined before use to improve the conversion rate. The steps are as follows: ① Weigh 50 mL of St into a 250 mL separatory funnel, add 30 mL of 15% NaOH solution, shake and wash, let stand to separate layers after shaking, take the upper layer of liquid, and repeat the operation three times; ② Wash the collected liquid with deionized water several times until it is neutral, use an appropriate amount of anhydrous Na2SO4 (it is better to use anhydrous Na2SO4 without lumps) to dry and remove water until the liquid is transparent; ③ Distill the liquid under reduced pressure, collect the effluent, and refrigerate for later use.

[0026] S2. Commercially available benzoyl peroxide (BPO) is prone to decomposition when left for a long time and needs to be recrystallized before use: ① Slowly stir and dissolve 6g BPO in 25mL chloroform; ② Filter the solution, drop the filtrate into an appropriate amount of methanol solution, and refrigerate and let stand; ③ Filter and collect the crystals, wash with a small amount of methanol, and drain; ④ Vacuum dry at 25℃ and store in a brown bottle at room temperature.

[0027] S3. Prepare a dispersion: add 1 to 5 parts by mass of organic matter, 0.1 to 0.6 parts by mass of sodium dodecylbenzene sulfonate (SDBS) and 0.1 to 0.6 parts by mass of cellulose ether (CE) to a three-necked flask, measure 100 to 300 parts by mass of ultrapure water in a three-necked flask, stir and disperse at 75° C. until clear, cool for use, and mark it as liquid A.

[0028] S4, prepare the oil phase: weigh 5-15 parts by mass of styrene (St) purified by S1, 5-15 parts by mass of divinylbenzene (DVB) purified by S1, 10-20 parts by mass of toluene, 10-20 parts by mass of 1,2-dichloroethane, and 5-16 parts by mass of n-heptane, mix them evenly, add 0.1-0.5 parts by mass of benzoyl peroxide (BPO) recrystallized by S2, stir slowly until it is completely dissolved, and mark it as liquid B.

[0029] S5. Heat the dispersion prepared in S3 to 45°C in an oil bath for later use. In a nitrogen atmosphere, slowly add the oil phase prepared in S4, pay attention to controlling the stirring speed, so that uniform oil droplets are formed on the surface, slowly raise the temperature to 88°C and react for 4 hours, and pass nitrogen protection throughout the process; after the small balls are formed, raise the temperature to 92°C and continue the reaction for 3 hours before ending.

[0030] S6. Washing and drying: The obtained product was washed with deionized water, ethanol and acetone three times respectively, dried under vacuum at 60°C for 2 h, and then taken out and bagged, which was recorded as SDB.

[0031] It should be noted that: anhydrous MgSO4 was used for drying during the purification of divinylbenzene (DVB) monomer, and the rest of the process was the same as S1.

[0032] Furthermore, the organic matter in step S3 is any one of polyvinyl alcohol-1799, polyvinyl alcohol-2099, polyvinyl alcohol-2499, and polyvinyl alcohol-2699.

[0033] Furthermore, in step S3, the mass ratio of the organic matter to the cellulose ether is preferably 7:1.

[0034] Furthermore, the mass ratio of sodium dodecylbenzene sulfonate and cellulose ether in step S3 is preferably 6:5.

[0035] Furthermore, the mass ratio of styrene and divinylbenzene used in step S4 is preferably 1:1.

[0036] The first technical solution provided by the second technical solution of the present invention is the application of the above-mentioned NiSn@C-SDB catalyst in the catalytic synthesis of higher carbon alcohols from ethanol in aqueous phase.

[0037] The third technical solution of the present invention provides a method for catalyzing ethanol aqueous phase catalytic synthesis of higher carbon alcohols according to the first technical solution,

[0038] Specifically, the NiSn@C-SDB catalyst described in the third aspect is combined with alkali, ethanol and water to form a reaction system, and under a H2 atmosphere, the initial pressure is set to 0.1-1MPa, and the reaction is carried out at 160-230°C for 6-24h to synthesize high carbon alcohols.

[0039] The mass ratio of the catalyst: base: ethanol: water is 0.15:0.88:5:5 to 0.6:0.88:5:5; more preferably, the mass ratio of NiSn@C-SDB catalyst: base: small molecule alcohol: water is 0.3:0.88:5:5.

[0040] Furthermore, the base in the reaction system is sodium hydroxide or potassium hydroxide.

[0041] Compared with the prior art, the present invention has the following advantages:

[0042] 1. The technical solution provided by the present invention introduces the promoting effect of metal Sn on the formation of higher alcohols. The inhibitory effect of metal Sn on Ni CO bond breaking may inhibit the continued breaking process of CO bonds of aldehyde intermediates formed by dehydrogenation, and the released aldehyde intermediates further promote the subsequent aldol condensation process, achieving the growth of the carbon chain; the inhibitory effect of metal Sn on Ni CO bond breaking may be related to the Sn atoms located at the Ni defect site and the formation of surface Ni3Sn alloy.

[0043] 2. The technical solution provided by the present invention is to synthesize NiSn@C-SDB catalyst by ball milling the prepared NiSn@C and hydrophobic polymer SDB; the hydrophobicity of the catalyst is greatly increased by ball milling the hydrophobic polymer, thereby reducing the dehydration of the aldol condensation reaction and the clogging of the internal pores of the catalyst due to water molecules in the reaction raw materials during the reaction, thereby reducing the phenomenon of deactivation caused by "water poisoning".

[0044] 3. The technical solution provided by the present invention applies the prepared NiSn@C-SDB catalyst to the reaction of catalyzing the one-step synthesis of higher alcohols from aqueous phase ethanol, showing excellent catalytic efficiency, higher reaction activity, higher ethanol conversion rate and increased selectivity for C6+ higher carbon alcohols.

[0045] 4. The technical solution provided by the present invention is simple to prepare the catalyst with low cost, and the reaction performance of the catalyst is improved through simple ball milling, which is more conducive to its production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 TEM image of the NiSn@C catalyst prepared in Example 1.

[0047] Figure 2 TEM image of NiSn@C-SDB after ball milling of NiSn@C catalyst and hydrophobic polymer SDB.

[0048] Figure 3 XRD patterns of NiSn@C and NiSn@C-SDB after ball milling of NiSn@C catalyst and hydrophobic polymer SDB.

[0049] Figure 4 is the contact angle of NiSn@C-SDB after ball milling of NiSn@C catalyst and hydrophobic polymer SDB.

[0050] Figure 5 This is the GC gas chromatogram of the oil phase product of NiSn@C-SDB with a ball milling ratio of 1:1.

[0051] Specific embodiment

[0052] The following is a further description of specific embodiments of the present invention. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention.

[0053] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental raw materials used in the following examples can be purchased through conventional commercial channels unless otherwise specified.

[0054] Example 1

[0055] This embodiment provides a Ni-Sn bimetallic catalyst, which is prepared by the following steps in sequence:

[0056] 1) Weigh 10 g of ultrapure water, 5.6 g of citric acid, 0.22 g of tin chloride and 3.68 g of nickel nitrate respectively, add them in sequence and stir to dissolve to form a uniform complex solution, stir at room temperature for 4 h, then place the obtained homogeneous solution on a 100 ° C heating plate and continue stirring at a speed of 500 rpm until the solvent evaporates to form a gel, and then transfer it to a 100 ° C oven and dry it for 36 h to obtain a Ni-Sn bimetallic catalyst precursor.

[0057] 2) The prepared Ni-Sn bimetallic catalyst precursor was placed in a tubular furnace, heated to a calcination temperature of 550°C at a heating rate of 5°C / min under a nitrogen atmosphere, and calcined at this temperature for 2 h to obtain a NiSn@C catalyst.

[0058] The NiSn@C catalyst was characterized by transmission electron microscopy (TEM). Figure 1 The catalyst has the characteristics of high loading and good dispersibility. Through X-ray diffraction (XRD) observation, it can be seen that the Ni3Sn alloy phase appears in the catalyst, but due to the low proportion of Sn in the metal, its diffraction peak is easily submerged in the strong diffraction peak of metal Ni. Through contact angle measurement, it can be observed that the hydrophobic angle of NiSn@C is small and the hydrophobic performance is not strong.

[0059] Example 2

[0060] This embodiment provides a method for preparing a hydrophobic polymer styrene-divinylbenzene copolymer, which is prepared by the following methods in sequence:

[0061] Step 1) Pretreatment of styrene monomer and divinylbenzene (DVB) monomer

[0062] 1) Pretreatment of styrene monomer

[0063] ① Weigh 50 mL of styrene monomer (St) into a 250 mL separatory funnel, add 30 mL of 15% NaOH solution and shake to wash, shake well and let stand to separate the layers, take the upper layer, and repeat the operation three times;

[0064] ② Wash the collected liquid with deionized water several times until it is neutral, and dry it with an appropriate amount of anhydrous Na2SO4 (preferably anhydrous Na2SO4 without agglomeration) until the liquid is transparent;

[0065] ③The liquid is distilled under reduced pressure at a pressure of 0.1MPa and a temperature of 90-95℃, the effluent is collected and refrigerated for later use.

[0066] 2) Pretreatment of divinylbenzene (DVB) monomer

[0067] ① Weigh 50mL of divinylbenzene (DVB) into a 250mL separatory funnel, add 30mL of 15% NaOH solution and shake to wash, shake well and let stand to separate the layers, take the upper layer, and repeat the operation three times;

[0068] ② Wash the collected liquid with deionized water three times until it is neutral, and dry it with an appropriate amount of anhydrous MgSO4 (preferably anhydrous MgSO4 without agglomeration) until the liquid is transparent;

[0069] ③The liquid is distilled under reduced pressure at a pressure of 0.1 MPa and a temperature of 125°C, the effluent is collected and refrigerated for later use.

[0070] Step 2) Benzoyl oxide (BPO) pre-treatment:

[0071] ① Slowly dissolve 6g BPO in 25mL chloroform by stirring;

[0072] ② Filter the solution, drop the filtrate into 20 ml of methanol solution, and refrigerate and let stand;

[0073] ③ Collect the crystals by filtration, wash them three times with 25 ml of methanol, and drain them;

[0074] ④ Dry in a vacuum oven at 25℃ and 0.1MPa and store in a brown bottle at room temperature.

[0075] Step 3) Preparation of dispersion

[0076] Add 3.5 g of polyvinyl alcohol, 0.6 g of sodium dodecylbenzene sulfonate (SDBS) and 0.5 g of cellulose ether (CE) into a three-necked flask, measure 300 g of ultrapure water into the three-necked flask, stir and disperse at 75° C. until clear, cool and set aside, and mark it as liquid A.

[0077] Step 4) Preparation of oil phase

[0078] Weigh 10 g of purified styrene (St), 10 g of purified divinylbenzene (DVB), 15.8 g of toluene, 12.4 g of 1,2-dichloroethane, and 11.6 g of n-heptane and mix them evenly, add 0.2 g of recrystallized benzoyl peroxide (BPO), and stir slowly until it is completely dissolved, and mark it as liquid B.

[0079] Step 5) Heat the prepared dispersion A liquid in an oil bath to 45°C for later use. In a nitrogen atmosphere, slowly add the prepared B liquid oil phase, control the stirring speed to 1000rpm, so that uniform oil droplets are generated on the surface, slowly heat to 88°C and react for 4h, and pass nitrogen protection throughout the process; after the small balls are formed, raise the temperature to 92°C, continue the reaction for 3h and then end.

[0080] Step 6) Washing and drying: The obtained product was washed with deionized water, ethanol and acetone three times respectively, dried under vacuum at 60° C. for 2 h, and then taken out and bagged, which was recorded as SDB.

[0081] Example 3

[0082] The present embodiment provides a method for preparing a hydrophobic catalyst NiSn@C-SDB, which comprises ball-milling the NiSn@C catalyst prepared in Example 1 and the hydrophobic polymer SDB prepared in Example 2 at a speed of 300 rpm for 4 hours according to a superhydrophobic mass ratio of 1:0.5 to obtain hydrophobic catalysts NiSn@C-SDB with different mixing ratios.

[0083] Example 4

[0084] The present embodiment provides a method for preparing a hydrophobic catalyst NiSn@C-SDB, which comprises ball-milling the NiSn@C catalyst prepared in Example 1 and the hydrophobic polymer SDB prepared in Example 2 at a speed of 300 rpm for 4 hours in a superhydrophobic mass ratio of 1:1 to obtain hydrophobic catalysts NiSn@C-SDB with different mixing ratios.

[0085] Example 5

[0086] The present embodiment provides a method for preparing a hydrophobic catalyst NiSn@C-SDB, which comprises ball milling the NiSn@C catalyst prepared in Example 1 and the hydrophobic polymer SDB prepared in Example 2 at a superhydrophobic mass ratio of 1:1.5 at a rotation speed of 300 rpm for 4 hours to obtain a hydrophobic catalyst NiSn@C-SDB.

[0087] Example 6

[0088] The present embodiment provides a method for preparing a hydrophobic catalyst NiSn@C-SDB, which comprises ball-milling the NiSn@C catalyst prepared in Example 1 and the hydrophobic polymer SDB prepared in Example 2 at a speed of 300 rpm for 4 hours according to a super-hydrophobic mass ratio of 1:2 to obtain hydrophobic catalysts NiSn@C-SDB with different mixing ratios.

[0089] Example 7

[0090] The present embodiment provides a method for preparing a hydrophobic catalyst NiSn@C-SDB, which comprises ball-milling the NiSn@C catalyst prepared in Example 1 and the hydrophobic polymer SDB prepared in Example 2 at a speed of 300 rpm for 4 hours according to a super-hydrophobic mass ratio of 1:3 to obtain hydrophobic catalysts NiSn@C-SDB with different mixing ratios.

[0091] Example 8

[0092] The hydrophobic catalyst NiSn@C-SDB with different mixing ratios prepared in Example 1 was applied to the reaction system of ethanol aqueous phase synthesis of higher alcohols. The reaction conditions were: 0.15g of the catalyst prepared in Example 1, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous product and the liquid product were collected. The liquid product was centrifuged to obtain an oil phase, an aqueous phase and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohols. The catalytic activity results of the products are shown in Table 1 below.

[0093] Example 9

[0094] The hydrophobic catalyst NiSn@C-SDB with different mixing ratios prepared in Example 3 was applied to the reaction system of ethanol water phase synthesis of higher alcohols, and the reaction conditions were: 0.225g of Example 3 catalyst, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous product and liquid product were collected, and the liquid product was centrifuged to obtain an oil phase, an aqueous phase and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohols. The catalytic activity results of the products are shown in Table 1 below.

[0095] Example 10

[0096] The hydrophobic catalyst NiSn@C-SDB prepared in Example 4 with different mixing ratios was applied to the reaction system of synthesizing higher alcohols from ethanol water phase. The reaction conditions were: 0.3g of the catalyst in Example 4, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous product and the liquid product were collected. The liquid product was centrifuged to obtain an oil phase, an aqueous phase, and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohol. The gas chromatogram of the oil phase product gc is shown in FIG. Figure 5 The catalytic activity results of the products are shown in Table 1 below.

[0097] Embodiment 11

[0098] The hydrophobic catalyst NiSn@C-SDB with different mixing ratios prepared in Example 5 was applied to the reaction system of ethanol water phase synthesis of higher alcohols, and the reaction conditions were: 0.375g of Example 5 catalyst, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous product and liquid product were collected, and the liquid product was centrifuged to obtain an oil phase, an aqueous phase and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohols. The catalytic activity results of the products are shown in Table 1 below.

[0099] Example 12

[0100] The hydrophobic catalyst NiSn@C-SDB with different mixing ratios prepared in Example 6 was applied to the reaction system of ethanol water phase synthesis of higher alcohols, and the reaction conditions were: 0.45g of the catalyst in Example 6, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous products and liquid products were collected. The liquid products were centrifuged to obtain an oil phase, an aqueous phase and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohols. The catalytic activity results of the products are shown in Table 1 below.

[0101] Embodiment 13

[0102] The hydrophobic catalyst NiSn@C-SDB with different mixing ratios prepared in Example 7 was applied to the reaction system of ethanol water phase synthesis of higher alcohols, and the reaction conditions were: 0.6g of Example 7 catalyst, 0.88g of sodium hydroxide, 5g of ethanol, 5g of water, an initial pressure of 0.1MPa, and a reaction time of 12h at 230°C. After the reaction, the reactor was cooled to room temperature, and then the gaseous products and liquid products were collected. The liquid products were centrifuged to obtain an oil phase, an aqueous phase and a catalyst solid phase. The oil phase and the aqueous phase were then detected and analyzed by gas chromatography. The main product of the oil phase was C6+ higher alcohols. The catalytic activity results of the products are shown in Table 1 below.

[0103] in:

[0104]

[0105] From the data in Table 1, it can be seen that when the ball-milling mass ratio of NiSn@C catalyst and hydrophobic polymer SDB is 1:0.5-1:3, its ethanol conversion rate, alcohol product yield and high-carbon alcohol product selectivity are higher than those of the catalyst without ball-milling. Especially when the mass ratio of NiSn@C catalyst and hydrophobic polymer SDB is 1:1, the catalytic reaction can have an ethanol conversion rate of 79.4% and a high-carbon alcohol product selectivity of 70.5%. When the ball-milling ratio is increased or decreased, the ethanol conversion rate and the selectivity of C6+ products are slightly decreased. In addition, the ethanol conversion rate, alcohol product carbon yield and C6+ product selectivity of the catalyst without ball-milling hydrophobic polymer are all low.

[0106] Table 1 Catalytic performance test results of hydrophobic NiSn@C-SDB catalyst

[0107] Proportion Ethanol conversion rate Carbon yield of alcohol products C6+ product selectivity 1:0 64.6 34.2 59.8 1:0.5 76.1 39.3 66.8 1:1 79.4 48.0 70.5 1:1.5 78.6 45.9 70.4 1:2 76.3 45.5 69.3 1:3 77.2 43.6 69.3

[0108] In summary, the hydrophobic NiSn@C-SDB catalyst synthesized by the method of the present invention is applied in the reaction of catalyzing the one-step synthesis of higher alcohols from ethanol, and exhibits excellent catalytic efficiency, high reaction activity and high selectivity for high-value C6+ higher carbon alcohol products, and the selectivity of C6+ alcohol products can be as high as 70%. In addition, the present invention is simple to prepare and inexpensive, and the reaction performance of the catalyst can be changed by simple ball milling, which is more conducive to its production and application.

[0109] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A Ni-Sn@C-SDB catalyst, characterized in that: It was prepared by ball milling using Ni-Sn bimetallic catalyst and hydrophobic polymer SDB; The mass ratio of the Ni-Sn bimetallic catalyst to the hydrophobic polymer SDB is 1:(0.5-3).

2. The Ni-Sn@C-SDB catalyst according to claim 1, characterized in that The ball milling time is 3-5h, and the ball milling speed is 100-500rpm.

3. The Ni-Sn@C-SDB catalyst according to claim 1, characterized in that The Ni-Sn bimetallic catalyst is prepared by the following method: S1, dissolving nickel salt, tin salt and carbon source precursor in a solvent, stirring at room temperature to form a complex to obtain a homogeneous solution, and then heating and stirring to form a nickel-tin bimetallic catalyst gel precursor; The molar ratio of Ni / Sn in the nickel salt and the tin salt is (1-30):1, and the molar ratio of Ni in the nickel salt to the carbon source precursor is 1:(0.2-5); S2. The nickel-tin bimetallic catalyst gel precursor prepared in S1 is placed in an inert gas atmosphere, and subjected to a controlled high-temperature self-reduction carbonization reaction at 400-700°C at a heating rate of 1-10°C / min for 2-4 hours to obtain a Ni-Sn bimetallic carbon-coated bimetallic catalyst. The nickel salt is one of nickel nitrate, nickel chloride, nickel acetate and nickel hydroxide; the tin salt is one of tin nitrate, tin citrate and tin chloride.

4. The Ni-Sn@C-SDB catalyst according to claim 1, characterized in that The hydrophobic polymer SDB is prepared by the following method: S1. Refined styrene or divinylbenzene monomer; S2, recrystallized benzoyl oxide; S3. Preparation of dispersion Add 1-5 parts by weight of organic matter, 0.1-0.6 parts by weight of sodium dodecylbenzene sulfonate and 0.1-0.6 parts by weight of cellulose ether to a three-necked flask, weigh 100-300 parts by weight of ultrapure water in the three-necked flask, stir and disperse at 75° C. until clear, cool and set aside, and mark as liquid A; S4, prepare oil phase: weigh 5-15 parts by mass of styrene purified by S1, 5-15 parts by mass of divinylbenzene purified by S1, 10-20 parts by mass of toluene, 10-20 parts by mass of 1,2-dichloroethane, 5-16 parts by mass of n-heptane and mix them evenly, add 0.1-0.5 parts by mass of benzoyl peroxide recrystallized by S2, stir slowly until it is completely dissolved, and mark it as liquid B; S5. Heat the dispersion prepared in S3 to 45°C in an oil bath for later use. In a nitrogen atmosphere, slowly add the oil phase prepared in S4, pay attention to controlling the stirring speed to produce uniform oil droplets on the surface, slowly raise the temperature to 88°C and react for 4 hours, with nitrogen protection throughout the process; after the small balls are formed, raise the temperature to 92°C and continue the reaction for 3 hours before ending; S6. Washing and drying: The obtained product was washed with deionized water, ethanol and acetone three times respectively, dried under vacuum at 60°C for 2 h, and then taken out and bagged, which was recorded as SDB.

5. The Ni-Sn@C-SDB catalyst according to claim 4, characterized in that The organic matter in step S3 is any one of polyvinyl alcohol-1799, polyvinyl alcohol-2099, polyvinyl alcohol-2499, and polyvinyl alcohol-2699.

6. The Ni-Sn@C-SDB catalyst according to claim 4, characterized in that The method for refining styrene monomer described in step S1 is: weigh 50 mL of styrene into a separatory funnel, add 30 mL of 15% NaOH solution, shake and wash, let stand to separate layers after shaking, take the upper layer of liquid, and repeat the operation three times; wash the collected liquid with deionized water several times until it is neutral, dry it with anhydrous Na2SO4 to remove water until the liquid is transparent; distill the dried liquid under reduced pressure, collect the effluent, and refrigerate it for later use.

7. The Ni-Sn@C-SDB catalyst according to claim 4, characterized in that The method for refining divinylbenzene monomer described in step S1 is as follows: weigh 50 mL of divinylbenzene into a separatory funnel, add 30 mL of 15% NaOH solution, shake and wash, let stand to separate layers after shaking, take the upper layer of liquid, and repeat the operation three times; wash the collected liquid with deionized water several times until it is neutral, dry it with anhydrous MgSO4 to remove water until the liquid is transparent; distill the dried liquid under reduced pressure, collect the effluent, and refrigerate it for later use.

8. The Ni-Sn@C-SDB catalyst according to claim 4, characterized in that The method for recrystallizing benzoyl oxide described in step S2 is: slowly stirring and dissolving 6 g of BPO in 25 mL of chloroform; filtering the solution, dropping the filtrate into an appropriate amount of methanol solution, and refrigerating and standing; filtering and collecting the crystals, washing with methanol, draining, and then vacuum drying at 25° C., and storing in a brown bottle at room temperature.

9. The Ni-Sn@C-SDB catalyst according to claim 1 is used for catalyzing the aqueous phase synthesis of higher alcohols from ethanol.

10. A method for synthesizing higher alcohols by catalytic ethanol aqueous phase, characterized in that: The steps are as follows: The Ni-Sn@C-SDB catalyst described in claim 1 is combined with alkali, ethanol and water to form a reaction system, and the reaction is carried out at 160-230° C. for 6-24 hours under a H2 atmosphere with an initial pressure of 0.1-1 MPa to synthesize high carbon alcohols; The mass ratio of the catalyst: alkali: ethanol: water is 0.15:0.88:5:5 to 0.6:0.88:5:5.

Citation Information

Patent Citations

  • Preparation method of styrene-divinylbenzene copolymer hydrophobic catalyst support

    CN104262521A

  • NiSn / C core-shell composite nano-catalyst, preparation method and application thereof

    CN112973707A

  • Polypropylene-based tin-doped carbon-coated nickel catalyst as well as preparation method and application thereof

    CN115445630A

  • Embedded hydrothermal-resistant NiSn-CS nano-catalyst as well as preparation method and application thereof

    CN115722230A

  • Hydrophobic catalyst for preparing mixed alcohol through CO hydrogenation as well as preparation method and application of hydrophobic catalyst