Method for purifying iron, carbon and zinc from blast furnace cloth bag ash

Through cyclone classification and spiral chute sorting combined with flotation and magnetic separation technology, high-speed iron concentrate, carbon powder and zinc sludge were separated, solving the problems of waste of blast furnace bag ash resources and environmental pollution, and achieving efficient purification of iron, carbon and Zinc reduces production costs and pollutant emissions.

CN119034927APending Publication Date: 2024-11-29ANSTEEL GRP MINING DESIGN & RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411080915.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The treatment method of blast furnace bag ash has problems of resource waste and environmental pollution. It is difficult for the existing technology to effectively recover iron, carbon and zinc, and the production costs are high and the equipment investment is large, which has pollution problems.

Method used

By mixing blast furnace bag ash with water to make slurry, cyclone classification and spiral chute sorting, combined with flotation and magnetic separation technology, high-speed iron concentrate, carbon powder and zinc sludge are separated, and the grade of iron, carbon and zinc are improved. Recovery rate, reduce production costs.

Benefits of technology

It has achieved efficient purification of iron, carbon and zinc, increased the added value of blast furnace bag ash, reduced production costs, reduced pollutant emissions, and improved resource utilization efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034927A_ABST
    Figure CN119034927A_ABST
Patent Text Reader

Abstract

The invention relates to a method for purifying iron, carbon and zinc from blast furnace cloth bag ash, which is characterized by comprising the following steps: mixing the blast furnace cloth bag ash with water to make slurry, feeding the slurry into a first-stage cyclone and a first-stage spiral chute to obtain an iron-containing inner ring product and a carbon-containing outer ring product, and feeding the outer ring product into a carbon powder sedimentation tank; an agent is added into the iron-containing inner ring product, the iron-containing inner ring product is fed into flotation operation for first-stage flotation operation and second-stage flotation operation, water is added into rough concentrate obtained after flotation operation for size mixing, then the rough concentrate is fed into a second-stage cyclone for gravity separation, iron-containing second-stage settled sand and zinc-containing second-stage overflow products are obtained, and the overflow products enter a zinc mud settling pond; the second-stage sand setting product is fed into first-stage and second-stage magnetic separation operation, final iron ore concentrate and tailings are obtained, the first-stage magnetic separation tailings and the second-stage magnetic separation tailings are combined and enter a second-section spiral chute for gravity separation, and inner-ring product tailings and outer-ring product carbon powder products are obtained; and finally, products in the sedimentation tanks are concentrated to obtain zinc mud, final iron ore concentrate, carbon powder and tailings, and clear water obtained after filtration is used for slurry making and recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical waste treatment, and in particular relates to a method for purifying iron, carbon and zinc from blast furnace bag ash. Background Art

[0002] Blast furnace bag ash, also known as blast furnace gas ash or blast furnace secondary ash, refers to the dust collected by bag dust collector after the flue gas generated from the top of the furnace passes through the gravity dust collector during the blast furnace smelting process. Blast furnace bag ash has fine particle size and is easily dispersed in the air. At the same time, the small particle size and low boiling point metal in it are easy to react with oxygen in the air, causing serious pollution to the atmosphere and soil.

[0003] At present, the disposal methods for blast furnace bag ash mainly include: direct stacking or landfill treatment, direct return to the factory for sintering, pyrometallurgical treatment, wet treatment, etc. Direct stacking or landfill treatment is the simplest operation, but the valuable element resources therein cannot be recycled, resulting in resource waste and serious pollution to the ecological environment. Returning blast furnace bag ash directly to the blast furnace solves the problem of high roasting temperature and can also recover iron, but the zinc element with a small content circulates and accumulates in the blast furnace, which is easy to form nodules in the blast furnace, which has a serious impact on the operation, performance, output and heat distribution of the blast furnace, and in severe cases, it will shorten the service life of the blast furnace. Pyrometallurgical treatment is widely used in practical applications, with high recovery rates of metals such as zinc and lead, and good comprehensive benefits, but the products are basically crude products and need further treatment, and there are problems such as large equipment investment and high energy consumption. Wet treatment generally uses acid or alkaline solutions to separate zinc, lead and other heavy metal elements to obtain high-quality products, but its productivity is not high, the later production costs increase, and it will also cause secondary pollution to the environment. Therefore, how to effectively develop and utilize blast furnace bag ash comprehensively, improve its utilization efficiency, and reduce pollutant emissions is of great significance to the sustainable development of enterprises. Summary of the invention

[0004] The purpose of the present invention is to purify iron, carbon and zinc from blast furnace bag ash, improve the grade of iron concentrate, separate zinc mud and carbon powder as products, increase the added value of blast furnace bag ash, and realize efficient and comprehensive resource utilization of blast furnace bag ash.

[0005] The objective of the present invention is achieved through the following technical solutions: A method for purifying iron, carbon and zinc from blast furnace bag ash of the present invention is characterized by comprising the following steps: Step 1, mixing blast furnace bag ash with water to make pulp, adjusting the pulp mass concentration to 25%, and then feeding it into a primary cyclone for classification treatment to obtain primary sedimentation and primary overflow products, the zinc content of the primary overflow product is greater than 8%, and it enters a zinc mud sedimentation tank; Step 2: Feed the primary sand settling in step 1 into the primary spiral chute for gravity separation to obtain an inner ring product with an iron content of more than 30% and an outer ring product with a carbon content of more than 6%. The outer ring product enters the carbon powder sedimentation tank; Step 3, adding inhibitor, collector and frother to the inner ring product with iron content greater than 30% in step 2, stirring, and feeding into flotation operation for primary flotation and secondary flotation operation; selecting the iron-containing coarse concentrate and carbon-containing tailings slurry through the primary flotation operation, the carbon-containing tailings slurry of the primary flotation operation enters the carbon powder sedimentation tank, the iron-containing coarse concentrate selected by the primary flotation operation is fed into the secondary flotation operation, and the tailings slurry of the secondary flotation operation returns to the primary flotation operation; Step 4: add water to the coarse concentrate after the secondary flotation operation in step 3 to adjust the concentration to 25% slurry, feed it into the secondary cyclone for gravity separation, and obtain the secondary sedimentation product with iron content greater than 35% and the secondary overflow product with zinc content greater than 6%. The secondary overflow product enters the zinc mud sedimentation tank; Step 5, the secondary sedimentation product obtained in step 4 is subjected to primary magnetic separation and secondary magnetic separation to separate the first magnetic concentrate and the third tailings, the first magnetic concentrate is fed into the secondary magnetic separation to carry out secondary magnetic separation, and the final iron concentrate and the fourth tailings are obtained, and the final iron concentrate enters the iron concentrate sedimentation tank; the third tailings and the fourth tailings are combined and enter the second-stage spiral chute for re-selection to obtain the inner circle product tailings and the outer circle product carbon powder, the outer circle carbon-containing product enters the carbon powder sedimentation tank, and the inner circle product enters the tailings sedimentation tank; Step 6: After the products in the zinc mud sedimentation tank, the iron ore concentrate sedimentation tank, the carbon powder sedimentation tank and the tailings sedimentation tank are concentrated, zinc mud, final iron ore concentrate, carbon powder and tailings are obtained respectively. The water separated from each sedimentation tank is pumped into a centralized water tank and then filtered through a filtration tank to obtain clean water for slurry making and recycling. Concentrating the products in the zinc mud sedimentation tank, the iron ore concentrate sedimentation tank, the carbon powder sedimentation tank and the tailings sedimentation tank is a prior art and will not be described in detail here.

[0006] Preferably, in step 1, the feed concentration of the primary cyclone is 25%, the feed pressure is 0.15 MPa, and the feed flow rate is 50 m 3 / h cyclone zinc selection.

[0007] Preferably, the inhibitor in step 3 is zinc sulfate, and its dosage is 500-700 g / t dry ore, the collector is a compound of light diesel and oleic acid in a weight ratio of 7:1, and its dosage is 1500-2000 g / t dry ore, and the foaming agent is 2-octanol, and its dosage is 100-400 g / t dry ore. The processing time of the primary operation and the secondary flotation operation is 18 minutes.

[0008] Preferably, the first spiral chute and the second spiral chute are spiral chutes of Φ1.3m for gravity selection.

[0009] Preferably, the feed pressure of the secondary cyclone in step 4 is 0.15 MPa and the feed flow rate is 50 m 3 / h cyclone zinc selection.

[0010] Preferably, the primary magnetic separation in step 5 is performed using a 120mT~200mT drum magnetic separator, and the secondary magnetic separation is performed using an 800mT~1000mT drum magnetic separator.

[0011] Preferably, the final iron concentrate in step 6 has an iron content of 57.80-60.23%, a recovery rate of 72.17-78.21%, zinc mud contains 8.24-9.02% zinc, a recovery rate of 38.54-41.35%, and carbon powder contains 12.56-19.62% carbon, with a recovery rate of 43.28-50.34%.

[0012] 1. The present invention adds cyclone classification and spiral chute separation before flotation treatment, reduces the use of flotation reagents, and greatly reduces production costs. Cyclone classification re-selection is added between flotation and magnetic separation, further improving the iron grade and reducing the workload of magnetic separation.

[0013] 2. Before selecting iron and carbon, the present invention first uses a cyclone to separate most of the zinc overflow, reduces the zinc content in the iron ore concentrate and carbon powder, uses two-stage flotation to separate the carbon powder to the greatest extent, and then uses two-stage magnetic separation to further improve the grade of the iron ore concentrate. Selecting zinc and carbon first can separate iron, carbon, and zinc to the greatest extent.

[0014] 3. The iron concentrate selected by the present invention has a high grade. The iron concentrate powder can be directly supplied to the sintering plant as a batching material, and the carbon powder can be directly supplied to the ironmaking plant as a coal injection material, further reducing the cost of ironmaking. The zinc mud contains a small amount of unselected iron powder, which can be used in rotary kilns to extract secondary zinc oxide or prepare zinc-containing catalysts and other high-end products. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 The present invention is a flow chart of a method for purifying iron, carbon and zinc from blast furnace bag ash. DETAILED DESCRIPTION

[0015] The specific implementation of the present invention is further described below with reference to specific examples. The blast furnace bag ash used in the test is from a steel plant, and its chemical composition is shown in Table 1.

[0016] Table 1 Chemical composition of blast furnace bag ash from a steel plant Example

[0017] Add water to the blast furnace bag ash to make slurry, adjust the slurry mass concentration to 25%, and let the slurry enter the primary cyclone. 3 / h, and the first overflow product with zinc content>8% is fed into the zinc mud sedimentation tank, and the sedimentation product is difficult to enter the spiral chute 1 of Φ1.3m for reselection, and the inner ring product with iron content>30% and the outer ring product with carbon content>6% are obtained. The outer ring product has a high carbon powder content and is fed into the carbon powder sedimentation tank. Subsequently, an inhibitor, a collector, and a foaming agent are added to the inner ring product. The inhibitor is zinc sulfate, and the amount of the inhibitor is 500g / t dry ore. The collector is a composite of light diesel and oleic acid, and the weight ratio of light diesel to oleic acid is 7:1. The amount of the collector is 1500g / t dry ore. The foaming agent is 2-octanol, and the amount of the foaming agent is 100g / t dry ore. The first flotation treatment is carried out for 18 minutes to obtain the first coarse concentrate and the first tailings. The first tailings enter the carbon powder sedimentation tank. The first rough concentrate is fed into the secondary flotation operation to obtain the second rough concentrate and the second tailings, and the second tailings of the secondary flotation operation are returned to the primary flotation operation; The second coarse concentrate product was adjusted to a concentration of 25% with water and fed into the secondary cyclone for gravity separation. At a feed pressure of 0.15 MPa and a feed flow rate of 50 m 3 / h, a secondary grit product with an iron content of >35% and a secondary overflow product with a zinc content of >6% are obtained, and the secondary overflow product enters the zinc mud sedimentation tank; the grit product is fed into a drum magnetic separator with a field strength of 120mT for primary magnetic separation to obtain a first magnetic concentrate and a third tailings, and the first magnetic concentrate is fed into a drum magnetic separator with a field strength of 800mT for secondary magnetic separation to obtain a final iron concentrate and a fourth tailings, and the final iron concentrate enters the iron concentrate sedimentation tank, and the third tailings and the fourth tailings are combined and fed into a Φ1.3m spiral chute 2 for re-selection to obtain an inner circle tailings product and an outer circle carbon-containing product, and the outer circle carbon-containing product enters the carbon powder sedimentation tank, and the inner circle product enters the tailings mud sedimentation tank. After the above scheme, the iron concentrate finally obtained has an iron grade of 57.80% and a recovery rate of 72.17%. The zinc mud contains 8.24% zinc and a recovery rate of 40.24%. The carbon powder contains 12.56% carbon and a recovery rate of 45.32%.

[0018] Example 2-Example 10 The steps of Example 2 to Example 10 are the same as those of Example 1. The specific process parameters are shown in Table 2. The separation results of each example are shown in Table 3.

[0019] Table 2 Process parameters and data of each embodiment .

[0020] Table 3 Separation results of various examples 。

Claims

1. A method for purifying iron, carbon and zinc from blast furnace bag ash, characterized in that: The following steps are involved: Step 1: Mix blast furnace bag ash with water to make pulp, adjust the pulp concentration to 25%, and then feed it into a primary cyclone for classification treatment to obtain a primary sand settling product and a primary overflow product. The zinc content of the primary overflow product is greater than 8%, and it enters a zinc mud sedimentation tank; Step 2: Feed the primary sand settling in step 1 into the primary spiral chute for gravity separation to obtain an inner ring product with an iron content of more than 30% and an outer ring product with a carbon content of more than 6%. The outer ring product enters the carbon powder sedimentation tank; Step 3, adding inhibitor, collector and frother to the inner ring product with iron content greater than 30% in step 2, stirring, and feeding into flotation operation for primary flotation and secondary flotation operation; the first rough concentrate and the first tailings are separated by the primary flotation operation, the first tailings of the primary flotation operation enter the carbon powder sedimentation tank, the first rough concentrate separated by the primary flotation operation is fed into the secondary flotation operation to obtain the second rough concentrate and the second tailings, and the second tailings of the secondary flotation operation are returned to the primary flotation operation; Step 4, adding water to the second coarse concentrate after the secondary flotation operation in step 3 to adjust the concentration to 25% slurry, feeding it into the secondary cyclone for gravity separation, obtaining a secondary sedimentation product with an iron content of more than 35% and a secondary overflow product with a zinc content of more than 6%, and the secondary overflow product enters the zinc mud sedimentation tank; Step 5, the secondary sedimentation product obtained in step 4 is subjected to primary magnetic separation and secondary magnetic separation to separate the first magnetic concentrate and the third tailings, the first magnetic concentrate is fed into the secondary magnetic separation to carry out secondary magnetic separation, and the final iron concentrate and the fourth tailings are obtained, and the final iron concentrate enters the iron concentrate sedimentation tank; the third tailings and the fourth tailings are combined and enter the second-stage spiral chute for re-selection to obtain the inner circle product tailings and the outer circle product carbon powder, the outer circle carbon-containing product enters the carbon powder sedimentation tank, and the inner circle product enters the tailings sedimentation tank; Step 6: Concentrate the products in the zinc mud sedimentation tank, the iron concentrate sedimentation tank, the carbon powder sedimentation tank and the tailings sedimentation tank to obtain zinc mud, final iron concentrate, carbon powder and tailings respectively. The water separated from each sedimentation tank is pumped into a centralized water tank and then filtered through a filtration tank to obtain clean water for pulping and recycling.

2. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: In step 1, the feed concentration of the primary cyclone is 25%, the feed pressure is 0.15 MPa, and the feed flow rate is 50 m 3 / h cyclone zinc selection.

3. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: The inhibitor in step 3 is zinc sulfate, and its dosage is 500-700 g / t dry ore. The collector is a compound of light diesel and oleic acid in a weight ratio of 7:1, and its dosage is 1500-2000 g / t dry ore. The foaming agent is octanol, and its dosage is 100-400 g / t dry ore. The processing time of the primary operation and the secondary flotation operation is 18 minutes.

4. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: The first-stage spiral chute and the second spiral chute adopt Φ1.3m spiral chute for gravity selection.

5. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: The feed pressure of the secondary cyclone in step 4 is 0.15 MPa and the feed flow rate is 50 m 3 / h cyclone zinc selection.

6. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: The first-level magnetic separation in step 5 adopts a 120mT~200mT drum magnetic separator for magnetic separation, and the second-level magnetic separation adopts a 800mT~1000mT drum magnetic separator for magnetic separation.

7. The method for purifying iron, carbon and zinc from blast furnace bag ash according to claim 1, characterized in that: The final iron concentrate in step 6 has an iron grade of 57.80-60.23% and a recovery rate of 72.17-78.21%. The zinc mud contains 8.24-9.02% zinc and a recovery rate of 38.54-41.35%. The carbon powder contains 12.56-19.62% carbon and a recovery rate of 43.28-50.34%.