Preparation method of transparent polypropylene

The transparent nucleating agent and ester-based group nucleating agent stabilizer generated by the reaction of undistilled dimethylbenzaldehyde with sorbitol, the problem of opacity and odor of polypropylene materials is solved, and cost reduction and transparency are achieved. promote.

CN119039704AActive Publication Date: 2024-11-29HUBEI NEW NANHUA TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411398471.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-29
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

The formation of large grains of polypropylene materials during cooling leads to opacity, and existing transparent nucleating agents are costly and have odor problems, limiting their use in high transparency applications.

Method used

The transparent nucleating agent produced by the reaction of undistilled dimethylbenzaldehyde and sorbitol, and the nucleating agent stabilizer of ester group is added to the polypropylene processing to reduce production costs and inhibit sorbitol acetal. Decompose, improve the transparency of polypropylene and reduce odor.

Benefits of technology

It effectively reduces the production cost of transparent nucleating agents, improves the transparency of polypropylene, and avoids the generation of odors. It is suitable for products that require high transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention relates to the field of polypropylene materials, in particular to a preparation method of transparent polypropylene. The invention relates to a preparation method of transparent polypropylene. The preparation method comprises the following steps: (1) preparing dimethyl benzaldehyde; (2) preparing a transparent nucleating agent; and (3) preparing polypropylene. According to the invention, 3, 4-dimethylbenzaldehyde with high purity is not adopted as a transparent nucleating agent raw material, and a nucleating agent stabilizer is added into a polypropylene processing raw material, so that the production cost of the transparent nucleating agent is reduced, and the finished polypropylene has excellent transparency and no obvious peculiar smell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polypropylene materials, and in particular to a method for preparing transparent polypropylene. Background Art

[0002] Polypropylene (PP) is a commonly used thermoplastic with excellent chemical stability and electrical insulation, as well as light weight, good strength and good heat resistance. Therefore, it is widely used in packaging, automotive industry, household appliances, medical devices and other fields. However, polypropylene is a crystalline polymer. When cooled under natural conditions, it will form larger grains, causing the material to appear milky white or opaque. This opacity limits the use of polypropylene in some applications, especially for products that require high transparency, such as transparent packaging materials, transparent containers, medical devices, etc. In order to overcome this limitation, adding a transparent nucleating agent during the processing of polypropylene helps to control the crystallization process, so that polypropylene forms finer grains during crystallization, reduces light scattering inside the material, and thus improves the transparency of the material. At present, the transparent nucleating agent on the market is mainly the third-generation sorbitol product 1,3,2,4-di(3,4-dimethyl)benzylidene sorbitol (DMDBS), which is prepared by the aldol condensation reaction of 3,4-dimethylbenzaldehyde and sorbitol.

[0003] However, in the preparation process of 3,4-dimethylbenzaldehyde, isomers are produced, and these by-products are mainly 3,5-dimethylbenzaldehyde, 2,3-dimethylbenzaldehyde, 2,5-dimethylbenzaldehyde and other substances. Since the sorbitol acetals obtained by the reaction of these isomers with sorbitol are easily decomposed, which makes the finished polypropylene produce odor, 3,4-dimethylbenzaldehyde with a purity of more than 99% is usually used in the preparation of DMDBS. However, since these isomers are extremely similar in nature to 3,4-dimethylbenzaldehyde, it is extremely difficult to purify them by distillation separation, which greatly increases the production cost of DMDBS, thereby limiting the further application of DMDBS in the market. And due to the bottleneck of distillation technology, it is very difficult to completely separate 3,4-dimethylbenzaldehyde and its isomers, which leads to the decomposition of trace amounts of isomers and sorbitol when DMDBS is used as a nucleating agent to prepare polypropylene, thereby releasing aldehyde substances to produce odor, which further limits the market of DMDBS. Summary of the invention

[0004] In order to solve the problems of high production cost of transparent nucleating agent and odor of polypropylene, the present application provides a method for preparing transparent polypropylene, which comprises (1) preparing dimethylbenzaldehyde; (2) preparing transparent nucleating agent; and (3) preparing polypropylene. The present application does not use 3,4-dimethylbenzaldehyde with a purity of more than 99% as the raw material of transparent nucleating agent and does not add nucleating agent stabilizer to the raw material of polypropylene processing, thereby reducing the production cost of transparent nucleating agent and preparing polypropylene with less odor and excellent transparency.

[0005] The first aspect of the present application provides a method for preparing transparent polypropylene, comprising the following steps: (1) Preparation of dimethylbenzaldehyde: o-xylene and 1,2-dichloroethane are mixed, aluminum chloride and hydrochloric acid are added, and the mixture is reacted in a carbon monoxide atmosphere; the reaction solution is washed with water, and the lower layer solution is removed after static stratification to obtain an upper layer oily substance, and the solvent in the oily substance is removed to prepare dimethylbenzaldehyde, wherein the dimethylbenzaldehyde includes 3,4-dimethylbenzaldehyde and 3,5-dimethylbenzaldehyde; (2) Preparation of a transparent nucleating agent: the dimethylbenzaldehyde is mixed with sorbitol, cyclohexane, methanol, and p-toluenesulfonic acid, and the mixture is reacted to prepare a transparent nucleating agent; (3) Preparation of polypropylene: the transparent nucleating agent, the compound shown in formula I, the auxiliary agent and the polypropylene matrix resin are mixed to obtain a polypropylene processing raw material, and the raw material is added into an extruder for extrusion to prepare polypropylene, Formula I Wherein, m, n, x, and y in Formula I are each independently an integer greater than or equal to 0.

[0006] The preparation of the transparent nucleating agent of the present application directly reacts the product of the o-xylene reaction with sorbitol, and the dimethylbenzaldehyde is used as a raw material to prepare the transparent nucleating agent without the need for a long time-consuming and precision equipment-required distillation and purification process, which greatly reduces the raw material cost of the transparent nucleating agent, thereby reducing the production cost of the transparent nucleating agent. Due to the presence of isomers of 3,4-dimethylbenzaldehyde in the dimethylbenzaldehyde prepared above, the sorbitol acetal obtained by reacting with sorbitol is easy to cause the oxygen atoms on its acetal bond to be attacked due to the acidity, moisture and other reasons in the reaction environment of preparing polypropylene, thereby forming a hemiacetal intermediate, ultimately causing the acetal bond to break, and decomposing and releasing the parent aldehyde. Based on this, the preparation method of the present application is further by adding the nucleating agent stabilizer shown in formula I in the raw material of preparing polypropylene, and the ester group in the nucleating agent stabilizer can consume water molecules and acidic substances in the reaction environment, thereby preventing its attack on the acetal bond of sorbitol acetal, playing a role in suppressing the decomposition of sorbitol acetal, thereby avoiding the production of peculiar smell in the finished polypropylene. And the alcohol substances produced by the nucleating agent stabilizer shown in Formula I due to the consumption of water molecules and the decomposition of acidic substances can further combine with trace aldehyde substances that may exist in the reaction environment, thereby further avoiding the odor caused by aldehyde substances. And the applicant unexpectedly found in the experiment that compared with the sorbitol acetal transparent nucleating agent generated by the reaction of 3,4-dimethylbenzaldehyde with a purity of more than 99% and sorbitol, the sorbitol acetal transparent nucleating agent generated by the reaction of dimethylbenzaldehyde and sorbitol without distillation and purification can further improve the transparency of polypropylene. Based on this phenomenon, the applicant found through experiments that the transparent nucleating agent obtained by the reaction of 3,5-dimethylbenzaldehyde and sorbitol has a better transmittance-enhancing effect than 3,4-dimethylbenzaldehyde, while the transparent nucleating agent obtained by the reaction of 2,3-dimethylbenzaldehyde and 2,5-dimethylbenzaldehyde with sorbitol has a transmittance-enhancing effect close to that of the transparent nucleating agent obtained by the reaction of 3,4-dimethylbenzaldehyde. Therefore, by adopting the preparation method of polypropylene of the present application, the production cost of the transparent nucleating agent is reduced, and the finished polypropylene has excellent transparency and no obvious odor.

[0007] In any embodiment, m, n, x, and y in Formula I are each independently greater than or equal to 10 and less than or equal to 15.

[0008] When m, n, x, and y in Formula I are independently greater than or equal to 10 and less than or equal to 15, the length of the alkyl chain of the nucleating agent stabilizer is within a suitable range, which can prevent the alkyl chain from being too short, reduce its compatibility and dispersibility with non-polar molten polypropylene, and make the addition of the nucleating agent stabilizer unfavorable to the transparency of polypropylene; it can also prevent the alkyl chain from being too long, resulting in its obvious steric effect, which is unfavorable for the uniform crystallization of the crystal nucleus, and also make the addition of the nucleating agent stabilizer have a negative impact on the transparency of polypropylene. When m, n, x, and y in Formula I are independently greater than or equal to 10 and less than or equal to 15, the nucleating agent stabilizer shown in Formula I can have good dispersibility, and is easy to form a homogeneous phase with the molten PP, which inhibits the decomposition of sorbitol acetal and reduces the odor of polypropylene. At the same time, as a nucleating agent stabilizer, when added in trace amounts, it has no negative effect on the transparency of polypropylene.

[0009] In any embodiment, in step (3), the amount of the compound represented by formula I is 0.1%-0.5%, based on the mass of the polypropylene matrix resin.

[0010] When the amount of the compound shown in Formula I is within the above range, it can not only consume water, acid and other substances present in the preparation process of polypropylene, avoid the decomposition of unstable sorbitol acetal in polypropylene to produce aldehyde substances, but also consume trace aldehyde substances that may exist in polypropylene, thereby avoiding the production of obvious odor in the finished polypropylene; it can also avoid the appearance of excessive amorphous regions in polypropylene due to excessive dosage, which is beneficial to reducing the scattering and refraction of light inside polypropylene, so that the addition of nucleating agent stabilizer has no obvious adverse effect on the transparency of polypropylene.

[0011] In any embodiment, step (1) specifically comprises: mixing o-xylene and 1,2-dichloroethane, adding aluminum chloride and hydrochloric acid, reacting for 2h-3h under a carbon monoxide atmosphere at a temperature of -10°C to -5°C; washing the reaction solution with water at -10°C to -5°C, removing the lower layer of solution after static stratification to obtain an upper layer of oily substance, adding an imidazole ionic liquid to the oily substance, performing a catalytic reaction, washing the reaction solution with water at -10°C to -5°C again, removing the lower layer of solution after static stratification to obtain an upper layer of liquid, removing the solvent in the liquid, and obtaining the prepared dimethylbenzaldehyde, wherein the dimethylbenzaldehyde includes 3,4-dimethylbenzaldehyde and 3,5-dimethylbenzaldehyde.

[0012] When the charge distribution of the aldehyde group and methyl group on dimethylbenzaldehyde on the benzene ring is uneven (such as 3,4-dimethylbenzaldehyde, 2,3-dimethylbenzaldehyde, 2,5-dimethylbenzaldehyde, etc.), they will tend to rearrange in the most stable way with the lowest energy structure (such as 3,5-dimethylbenzaldehyde). Based on the discovery that the transparent nucleating agent obtained by the reaction of 3,5-dimethylbenzaldehyde and sorbitol has better permeability-enhancing properties for polypropylene than other isomers, the applicant further used imidazole ionic liquids as catalysts to catalyze the electrophilic rearrangement reaction of dimethylbenzaldehyde, thereby increasing the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, and then improving the permeability-enhancing properties of the transparent nucleating agent for polypropylene, which is beneficial to further reduce the haze of polypropylene. The cation of the imidazole ionic liquid can show a certain acidity and can act as a proton donor to promote the conversion of the methyl group on the benzene ring into electrophilic CH3 + , and then rearranges with the benzene ring to form 3,5-dimethylbenzaldehyde with lower energy and more stable structure. The polar environment provided by imidazole ionic liquids also helps to stabilize the electrophilic intermediate. Compared with protonic acids such as hydrochloric acid, imidazole ionic liquids have the advantages of being green, recyclable, structurally designable, and mild, which can reduce the occurrence of side reactions and improve the selectivity of the target product.

[0013] In any embodiment, the imidazolium-based ionic liquid includes one or more of 1-methyl-3-butylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hexafluorophosphate, and 1-ethyl-3-methyltetrafluoroborate.

[0014] The anion of the above-mentioned imidazole ionic liquid is hydrogen sulfate HSO4 - , hexafluorophosphate PF6 ⁻ and tetrafluoroborate BF4 ⁻ , which further facilitates the conversion of the methyl group on the benzene ring into electrophilic CH3 + , which further facilitates the electrophilic rearrangement reaction of dimethylbenzaldehyde catalyzed by imidazole ionic liquids and improves the selectivity of the target product. - Since hydrogen ions can be dissociated, further protons are provided to promote the conversion of the methyl groups on the benzene ring into electrophilic CH3 + This makes the electrophilic rearrangement reaction of dimethylbenzaldehyde catalyzed by 1-methyl-3-butylimidazole hydrogen sulfate more effective, which is beneficial to further improve the transparency of polypropylene.

[0015] In any embodiment, the amount of the imidazolium ionic liquid used is 0.01%-0.1%, based on the total mass of the oil.

[0016] The amount of imidazole ionic liquid used within the above range can avoid the slow rate of catalytic electrophilic rearrangement reaction due to too little catalyst, and the low mass proportion of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, which is not conducive to the improvement of the transparency of polypropylene; it can also avoid the excessive reaction rate due to excessive catalyst or the impact on the normal progress of the reaction, resulting in too high a mass proportion of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde or too many side reactions. Since the amount of nucleating agent stabilizer added during the preparation of polypropylene needs to be controlled within a certain range, the presence of too much unstable sorbitol acetal will cause its decomposition to be unable to be inhibited, thereby causing the finished polypropylene to produce odor. The amount of imidazole ionic liquid used within the above range, polypropylene has excellent transparency and no odor.

[0017] In any embodiment, the temperature of the catalytic reaction is -10°C to -5°C, and the reaction time is 1h-6h.

[0018] When the temperature of the catalytic reaction is within the above range, it is conducive to the occurrence of electrophilic rearrangement reaction, so that the content of 3,5-dimethylbenzaldehyde in the prepared dimethylbenzaldehyde is increased; when the reaction time of the catalytic reaction is within the above range, the content of 3,5-dimethylbenzaldehyde in the prepared dimethylbenzaldehyde can be within an appropriate range, which can avoid the reaction time being too short and the content of 3,5-dimethylbenzaldehyde being too low, which is not conducive to the improvement of the transparency of polypropylene; it can also avoid the reaction time being too long and the content of 3,5-dimethylbenzaldehyde being too high or the side reactions being too many, which reduces the production efficiency and also causes the polypropylene to produce a noticeable odor. When the reaction time of the catalytic reaction is within the above range, the transparent nucleating agent makes the polypropylene have excellent transparency and no noticeable odor is produced.

[0019] In any embodiment, based on the total mass of the dimethylbenzaldehyde, the mass proportion of 3,5-dimethylbenzaldehyde in the dimethylbenzaldehyde is 8%-40%.

[0020] When the mass proportion of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde is 8%-40%, the transparent nucleating agent prepared by 3,5-dimethylbenzaldehyde and sorbitol makes the polypropylene have excellent transparency, and the nucleating agent stabilizer added to the raw material for preparing the polypropylene effectively inhibits the decomposition of sorbitol acetal. The polypropylene has excellent transparency and no obvious odor is generated.

[0021] In any embodiment, in step (3), the amount of the transparent nucleating agent is 0.1%-0.5%, based on the mass of the polypropylene matrix resin.

[0022] When the amount of the transparent nucleating agent is within the above range based on the mass of the polypropylene matrix resin, the polypropylene has excellent transparency and no obvious odor is generated.

[0023] In any embodiment, in step (3), the auxiliary agent includes one or more of antioxidant 1010, antioxidant 168, and calcium stearate.

[0024] The above additives are beneficial to improving the mechanical properties of polypropylene and extending the service life of polypropylene.

[0025] In summary, this application has the following beneficial effects: (1) The preparation of the transparent nucleating agent of the present application directly reacts the product of the reaction of o-xylene with sorbitol. The dimethylbenzaldehyde can be used as a raw material to prepare the transparent nucleating agent without going through a time-consuming and precision equipment-required distillation and purification process, which greatly reduces the raw material cost of the transparent nucleating agent, thereby reducing the production cost of the transparent nucleating agent. Further, by adding a nucleating agent stabilizer shown in Formula I to the raw material for preparing polypropylene, the ester group in the nucleating agent stabilizer can consume water molecules and acidic substances in the reaction environment, thereby preventing them from attacking the acetal bond of sorbitol acetal, playing a role in inhibiting the decomposition of sorbitol acetal, thereby avoiding the finished polypropylene from producing obvious odor. In addition, the applicant unexpectedly discovered in the experiment that compared with the sorbitol acetal transparent nucleating agent generated by the reaction of 3,4-dimethylbenzaldehyde with a purity of more than 99% and sorbitol, the sorbitol acetal transparent nucleating agent generated by the reaction of dimethylbenzaldehyde and sorbitol without distillation and purification can further improve the transparency of polypropylene. Therefore, by adopting the method for preparing polypropylene of the present application, the production cost of the transparent nucleating agent is reduced, and the prepared polypropylene has both low odor and excellent transparency.

[0026] (2) The applicant uses imidazole ionic liquid as a catalyst to catalyze the electrophilic rearrangement reaction of dimethylbenzaldehyde, thereby increasing the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, and then improving the transparency-enhancing performance of the transparent nucleating agent on polypropylene, which is beneficial to further reduce the haze of polypropylene. DETAILED DESCRIPTION

[0027] The present application is further described in detail below in conjunction with embodiments and comparative examples.

[0028] In the following examples, if no specific conditions are specified, the reaction was carried out according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources. Example Example 1

[0029] A method for preparing polypropylene comprises the following steps: (1) Preparation of dimethylbenzaldehyde Add 100 parts by weight of o-xylene and 200 parts by weight of 1,2-dichloroethane, start the agitator, pre-cool the materials in the reaction bottle to -20°C to -10°C, then add 3-4 drops of concentrated hydrochloric acid and 130 parts by weight of anhydrous AlCl3 as a catalyst in sequence, introduce nitrogen as replacement gas; control the operating temperature at -10°C to -5°C, introduce carbon monoxide, maintain the partial pressure of carbon monoxide at 1.0Mpa, and start timing reaction. After 2.5 hours of reaction, the reaction is terminated, the carbon monoxide vent valve is closed, stirring is continued, and then the above reactants are poured into a prepared ice brine flask at a temperature of -10°C to -5°C, stirred, placed in a separating funnel, extracted and shaken, allowed to stand for stratification, the lower layer of acid water is separated, the upper layer of oil is obtained, placed in a distillation flask for atmospheric distillation, and the solvent is removed to obtain the prepared dimethylbenzaldehyde. Through testing, it was calculated that the mass proportion of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde is 8%.

[0030] (2) Preparation of transparent nucleating agent 400 parts by mass of cyclohexane and 60 parts by mass of methanol were added, and then 30 parts by mass of sorbitol, 50 parts by mass of the above-prepared dimethylbenzaldehyde, and 3 parts by mass of p-toluenesulfonic acid catalyst were added in sequence, the temperature was raised to 70°C, and an aldol condensation reaction was carried out under a nitrogen atmosphere. A mixture of methanol and water was separated by a liquid-liquid separator. The reaction was continued for 6 hours and then cooled to 50°C. An alkaline solution was added to neutralize and remove the acid catalyst, the solvent was evaporated, filtered, and vacuum dried to obtain a transparent nucleating agent product.

[0031] (3) Preparation of polypropylene The prepared transparent nucleating agent, the compound shown in formula I, antioxidant 1010, antioxidant 168, calcium stearate and polypropylene matrix resin are uniformly mixed in a high-speed mixer according to a mass ratio of 2:3:0.5:1:0.5:1000, and the mixture is extruded through a twin-screw extruder to prepare polypropylene, wherein m, n, x and y of the compound shown in formula I are 12, and the compound shown in formula I is pentaerythritol tetramyristate. The temperatures of the extruder from the feed port to each zone of the die are 190°C, 200°C, 210°C, 218°C, 210°C, 200 and 190°C, respectively.

[0032] The prepared polypropylene was used to prepare standard specimens required for the haze test and the odor test by injection molding in an injection molding machine, and the temperature of the injection molding machine from the first stage to the head was 200°C-230°C.

[0033] Comparative Example 1 The preparation method of the polypropylene in Comparative Example 1 is basically similar to that in Example 1, the difference is that in step (2), the transparent nucleating agent is prepared by using commercially available 3,4-dimethylbenzaldehyde with a purity of more than 99%.

[0034] Comparative Example 2 The preparation method of the polypropylene in Comparative Example 2 is basically similar to that in Example 1, except that, in the preparation of the polypropylene in step (3), the compound represented by Formula I is not added.

[0035] Comparative Example 3 The preparation method of the polypropylene in Comparative Example 3 is basically similar to that in Example 1, except that, in the preparation of the polypropylene in step (3), the compound represented by formula I is not added, but pentaerythritol is added instead. Performance Testing

[0036] 1. Haze The specimens with the specification of 50 mm×50 mm×1 mm were prepared, and the test standard was carried out according to the ASTM D1003-07 standard.

[0037] 2. Smell According to the odor test standard VDA270-2018, a sample with a size of 50mm×50mm×20mm was prepared and placed in a 500ml glass bottle with the cap tightly closed. The glass bottle and the bottle cap were cleaned before use to keep them clean and the odor neutral. They were placed at ambient temperature for one day and then the odor was evaluated. Five people participated in the odor evaluation, and the odor evaluation adopted a 6-level evaluation standard: Level 1 means no odor, level 2 means there is an odor but it is not disturbing, level 3 means there is an obvious odor but it is still not disturbing, level 4 means there is a disturbing odor, level 5 means there is a strong disturbing odor, and level 6 means it is unbearable. The evaluation results can be described at half a level, and the average value is taken as the final odor level result. The lower the level, the smaller the odor.

[0038] 3. Content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde The prepared dimethylbenzaldehyde was detected by gas chromatography (GC), so as to calculate the mass proportion of 3,5-dimethylbenzaldehyde in the dimethylbenzaldehyde.

[0039] The performance of the polypropylene samples prepared in Example 1 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1.

[0040] Table 1 Performance test table of polypropylene of Example 1 and Comparative Examples 1-2 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 1 8% 8.7 1 Comparative Example 1 / 10.6 2 Comparative Example 2 8% 9.9 5 Comparative Example 3 8% 10.3 4 Referring to Table 1, it can be seen from the comparison between Comparative Example 1 and Comparative Examples 1, 2, and 3 that the preparation method of the present application, by directly using the dimethylbenzaldehyde after the reaction and adding the compound shown in Formula I, greatly reduces the production cost of the transparent nucleating agent, avoids the generation of odor, and further reduces the haze of polypropylene. Comparative Example 1 uses 3,4-dimethylbenzaldehyde with a purity of more than 99% with a relatively high cost as a raw material to prepare a transparent nucleating agent for the preparation of polypropylene. Since the raw material may also contain trace isomers that cannot be completely separated, the polypropylene of Comparative Example 1 has an odor when the compound shown in Formula I is not added. Comparative Example 2 uses the dimethylbenzaldehyde after the reaction directly as a raw material to prepare a transparent nucleating agent, but when the compound shown in Formula I is not added to inhibit the decomposition of sorbitol acetal and remove aldehyde substances, the polypropylene has a strong odor, which is not conducive to the application of polypropylene products in the fields of food, cosmetics, and medicines. In Comparative Example 3, the reacted dimethylbenzaldehyde is directly used as a raw material to prepare a transparent nucleating agent. Pentaerythritol is added to the reaction raw materials for preparing polypropylene. Although it has a certain effect of suppressing odor, the effect is weak and has a negative impact on the transparency of polypropylene.

[0041] Embodiment 2-5 The preparation method of the polypropylene in Examples 2-5 is basically similar to that in Example 1, except that the structure of the compound represented by Formula I added in step (3) is changed, as follows: Example 2: m, n, x, and y of the compound represented by formula I are 10, and the compound represented by formula I is pentaerythritol tetralaurate; In Example 3, m, n, x, and y of the compound represented by Formula I are 14, and the compound represented by Formula I is pentaerythritol tetrapalmitate; In Example 4, m, n, x, and y of the compound represented by Formula I are 5, and the compound represented by Formula I is pentaerythritol tetra-n-heptanoate; In Example 5, m, n, x, and y of the compound represented by Formula I are 16, and the compound represented by Formula I is pentaerythritol tetrastearate; The polypropylene samples of Examples 2-5 were tested for performance, and the test results are shown in Table 2.

[0042] Table 2 Performance test table of polypropylene of Example 1 and Example 2-5 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 1 8% 8.7 1 Example 2 8% 9.2 1 Example 3 8% 9.7 1 Example 4 8% 9.9 1 Example 5 8% 10.4 1 Referring to Table 2, it can be seen from the comparison between Examples 1-3 and 4-5 that when m, n, x, and y of the compound shown in Formula I are greater than or equal to 10 and less than or equal to 15, it is beneficial to further reduce the haze of polypropylene. This may be because when the length of the carbon chain connected to the ester group of the compound shown in Formula I is in an appropriate range, it is easy to form a homogeneous phase with the molten PP and will not affect the crystallization of polypropylene, thereby avoiding the odor of polypropylene and having excellent transparency. When m, n, x, and y of the compound shown in Formula I are less than 10 and greater than 15, the transparency of polypropylene may be reduced because the carbon chain is too short and is not conducive to its dispersion, and the carbon chain is too long and is not conducive to the crystallization of polypropylene.

[0043] Embodiment 6-9 The preparation methods of polypropylene in Examples 6-9 are basically similar to those in Example 1, except that the amount of the compound represented by Formula I in step (3) is changed, as follows: The amount of the compound represented by formula I in Example 6 is 0.1%, based on the mass of the polypropylene base resin; The amount of the compound represented by formula I in Example 7 is 0.5%, based on the mass of the polypropylene base resin; The dosage of the compound represented by formula I in Example 8 is 0.05%, based on the mass of the polypropylene matrix resin; The amount of the compound represented by formula I in Example 9 is 0.8%, based on the mass of the polypropylene base resin; The polypropylene samples of Examples 6-9 were tested for performance, and the test results are shown in Table 3.

[0044] Table 3 Performance test table of polypropylene in Example 1 and Examples 6-9 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 1 8% 8.7 1 Example 6 8% 8.3 2 Example 7 8% 9.8 1 Example 8 8% 8.1 3 Example 9 8% 10.3 1 Referring to Table 3, it can be seen from the comparison between Examples 1, 6, 7 and Examples 8 and 9 that when the amount of the compound shown in Formula I is 0.1%-0.5%, it is beneficial to suppress the odor of polypropylene and also make the polypropylene have excellent transparency. When the addition amount of the compound shown in Formula I is less than 0.1%, the inhibition of the decomposition of sorbitol acetal is limited, so that the prepared polypropylene is prone to produce obvious odor; when the addition amount of the compound shown in Formula I is greater than 0.5%, too many amorphous regions will appear in the polypropylene, thereby reducing the transparency of the polypropylene. Example 10

[0045] The preparation method of the polypropylene in Example 10 is basically similar to that in Example 1, except that an imidazole ionic liquid is further added in step (1). The specific preparation method of step (1) is as follows: Add 100 parts by weight of o-xylene and 200 parts by weight of 1,2-dichloroethane, start the agitator, pre-cool the materials in the reaction bottle to -20°C to -10°C, then add 3 to 4 drops of concentrated hydrochloric acid and 130 parts by weight of catalyst anhydrous AlCl3 in sequence, and introduce nitrogen as replacement gas; control the operating temperature at -10°C to -5°C, introduce carbon monoxide, maintain the partial pressure of carbon monoxide at 1.0 MPa, and start the timing reaction. After 2.5 hours of reaction, the reaction was terminated, the carbon monoxide vent valve was closed, stirring was continued, and then the above reactants were poured into a prepared ice-salt water flask at a temperature of -10°C to -5°C, and after stirring, placed in a separatory funnel, extracted and shaken, allowed to stand for stratification, and the lower layer of acid water was separated to obtain an upper layer of oil; 1-methyl-3-butyl imidazole hydrogen sulfate accounting for 0.05% of the total mass of the oil was added to the oil, and the catalytic reaction was carried out at -5°C for 4 hours, and then the above reactants were poured into a prepared ice-salt water flask at a temperature of -10°C to -5°C, and after stirring, placed in a separatory funnel, extracted and shaken, allowed to stand for stratification, and the lower layer of solution was separated to obtain an upper layer of solution; the upper layer of solution was placed in a distillation flask for atmospheric distillation, and the solvent was removed to obtain the prepared dimethylbenzaldehyde. The test showed that the mass proportion of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde was 24%.

[0046] In the preparation of polypropylene in step (3), the mass ratio of the compound represented by formula I to the polypropylene matrix resin is 5:1000.

[0047] Examples 11-14 The preparation methods of polypropylene in Examples 11-14 are basically similar to that in Example 10, except that the amount of 1-methyl-3-butylimidazole hydrogen sulfate in step (1) is changed, as follows: In Example 11, the amount of 1-methyl-3-butylimidazole hydrogen sulfate used is 0.01% of the total mass of the oil; In Example 12, the amount of 1-methyl-3-butylimidazole hydrogen sulfate used is 0.1% of the total mass of the oil; In Example 13, the amount of 1-methyl-3-butylimidazole hydrogen sulfate used is 0.005% of the total mass of the oil; In Example 14, the amount of 1-methyl-3-butylimidazole hydrogen sulfate used is 0.2% of the total mass of the oil; The polypropylene samples of Examples 10-14 were tested for performance, and the test results are shown in Table 4.

[0048] Table 4 Performance test table of polypropylene of Example 1 and Examples 10-14 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 1 8% 8.7 1 Example 10 24% 7.1 1 Embodiment 11 16% 7.7 1 Example 12 38% 6.8 2 Embodiment 13 12% 8.2 1 Embodiment 14 43% 6.6 4 Referring to Table 4, it can be seen from the comparison between Example 1 and Example 10 that further adding imidazole ionic liquid to catalyze electrophilic rearrangement reaction is beneficial to increase the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde. When used to prepare a transparent nucleating agent for the preparation of polypropylene, the compound shown in Formula I has an inhibitory effect on the decomposition of sorbitol acetal, so that the haze of polypropylene is further reduced without generating odor. From the comparison between Examples 10-12 and Examples 13 and 14, it can be seen that when the amount of the imidazole ionic liquid is 0.01% to 0.1% of the total mass of the oil, the polypropylene has excellent transparency and no obvious odor is generated. When the amount of the imidazole ionic liquid is less than 0.01%, the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde is too small, which is not conducive to improving the transparency of the polypropylene; when the amount of the imidazole ionic liquid is greater than 0.1%, due to the excessive content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, the content of unstable sorbitol acetal in the transparent nucleating agent is excessive, resulting in the generation of odor in the polypropylene.

[0049] Examples 15-18 The preparation methods of polypropylene in Examples 15-18 are basically similar to those in Example 10, except that the time of the catalytic reaction in step (1) is changed, as follows: The catalytic reaction time of Example 15 is 1 h; The catalytic reaction time of Example 16 is 6 h; The catalytic reaction time of Example 17 is 0.5h; The catalytic reaction time of Example 18 is 8h; The polypropylene samples of Examples 15-18 were tested for performance, and the test results are shown in Table 5.

[0050] Table 5 Performance test table of polypropylene of Example 10 and Examples 15-18 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 10 24% 7.1 1 Embodiment 15 17% 7.6 1 Example 16 35% 6.9 2 Embodiment 17 10% 8.6 1 Embodiment 18 33% 7.0 3 Referring to Table 5, from the comparison of Examples 10, 15-18, it can be seen that the time of the catalytic electrophilic rearrangement reaction is 1h-6h, which is conducive to controlling the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde within a suitable range, and the polypropylene has excellent transparency without obvious odor. When the time of the catalytic electrophilic rearrangement reaction is less than 1h, the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde is too little, which is not conducive to improving the transparency of polypropylene; when the time of the catalytic electrophilic rearrangement reaction is greater than 6h, it is not conducive to further improving the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, and may lead to the generation of by-products, thereby causing the polypropylene to produce odor. Embodiment 19

[0051] The preparation method of polypropylene in Example 19 is basically similar to that in Example 10, except that the type of imidazole ionic liquid in step (1) is changed. The imidazole ionic liquid used in Example 19 is 1-butyl-3-methylimidazolium hexafluorophosphate.

[0052] Comparative Example 4 The preparation method of the polypropylene in Comparative Example 4 is substantially similar to that in Example 10, except that concentrated hydrochloric acid is used as a catalyst in Comparative Example 4.

[0053] The polypropylene samples of Example 19 and Comparative Example 4 were tested for performance, and the test results are shown in Table 6 respectively.

[0054] Table 6 Performance test table of polypropylene of Example 19 and Comparative Example 4 Serial number Mass proportion of 3,5-dimethylbenzaldehyde Haze / % odor Example 10 24% 7.1 1 Embodiment 19 17% 7.7 1 Comparative Example 4 37% 6.8 5 Referring to Table 6, from the comparison between Example 10 and Example 19, it can be seen that when the imidazole ionic liquid uses 1-methyl-3-butyl imidazole hydrogen sulfate, it is more conducive to catalyzing the electrophilic rearrangement reaction, which is conducive to increasing the content of 3,5-dimethylbenzaldehyde in dimethylbenzaldehyde, thereby reducing the haze of polypropylene. From the comparison between Examples 10 and 19 and Comparative Example 4, it can be seen that when hydrochloric acid is used as a catalyst, the rate of catalyzing the electrophilic rearrangement reaction is too intense and by-products are easily produced, resulting in a significant odor in polypropylene. Compared with hydrochloric acid, the use of imidazole ionic liquids as catalysts is mild, can reduce the occurrence of side reactions, improve the transparency of polypropylene, and polypropylene does not produce odor.

[0055] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for preparing transparent polypropylene, characterized in that: The following steps are involved: (1) Preparation of dimethylbenzaldehyde: o-xylene and 1,2-dichloroethane are mixed, aluminum chloride and hydrochloric acid are added, and the mixture is reacted under a carbon monoxide atmosphere; the solution after the reaction is washed with water, the lower layer of the solution is removed after static stratification to obtain an oily substance on the upper layer, and the solvent in the oily substance is removed to prepare dimethylbenzaldehyde, wherein the dimethylbenzaldehyde includes 3,4-dimethylbenzaldehyde and 3,5-dimethylbenzaldehyde; (2) Preparation of a transparent nucleating agent: mixing the dimethylbenzaldehyde with sorbitol, cyclohexane, methanol, and p-toluenesulfonic acid, and reacting the mixture to prepare a transparent nucleating agent; (3) Preparation of polypropylene: The transparent nucleating agent, the compound represented by formula I, the auxiliary agent and the polypropylene matrix resin are mixed to obtain a polypropylene processing raw material, and the raw material is added into an extruder for extrusion to prepare polypropylene. Formula I Wherein, m, n, x, and y in Formula I are each independently an integer greater than or equal to 0.

2. The preparation method according to claim 1, characterized in that: In the formula (I), m, n, x and y are each independently greater than or equal to 10 and less than or equal to 15.

3. The preparation method according to claim 1, characterized in that: In step (3), the amount of the compound represented by formula I is 0.1%-0.5%, based on the mass of the polypropylene matrix resin.

4. The preparation method according to claim 1, characterized in that: Step (1) specifically includes: Mix o-xylene and 1,2-dichloroethane, add aluminum chloride and hydrochloric acid, and react for 2h-3h at a temperature of -10°C to -5°C under a carbon monoxide atmosphere; wash the solution after the reaction with water at -10°C to -5°C, remove the solution of the lower layer after static stratification to obtain an oily substance on the upper layer, add an imidazole ionic liquid to the oily substance, perform a catalytic reaction, wash the solution after the reaction with water at -10°C to -5°C again, remove the solution of the lower layer after static stratification to obtain a liquid on the upper layer, remove the solvent in the liquid, and obtain the prepared dimethylbenzaldehyde, wherein the dimethylbenzaldehyde includes 3,4-dimethylbenzaldehyde and 3,5-dimethylbenzaldehyde.

5. The preparation method according to claim 4, characterized in that: The imidazolium ionic liquid includes one or more of 1-methyl-3-butylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hexafluorophosphate, and 1-ethyl-3-methyltetrafluoroborate.

6. The preparation method according to claim 4, characterized in that: The amount of the imidazole ionic liquid used is 0.01%-0.1%, based on the total mass of the oil.

7. The preparation method according to claim 4, characterized in that: The temperature of the catalytic reaction is -10°C to -5°C, and the reaction time is 1h-6h.

8. The preparation method according to any one of claims 1 to 7, characterized in that Based on the total mass of the dimethylbenzaldehyde, the mass proportion of 3,5-dimethylbenzaldehyde in the dimethylbenzaldehyde is 8%-40%.

9. The preparation method according to claim 1, characterized in that: In step (3), the amount of the transparent nucleating agent is 0.1%-0.5%, based on the mass of the polypropylene matrix resin.

10. The preparation method according to claim 1, characterized in that: In step (3), the auxiliary agent includes one or more of antioxidant 1010, antioxidant 168, and calcium stearate.

Citation Information

Patent Citations

  • Polyolefine nucleating agent and preparation as well as application thereof

    CN102250398A

  • 3,5-dimethylbenzaldehyde preparation method

    CN103524313A

  • Polyolefin resin composition and preparation method thereof

    CN104163984A

  • Method for reducing melting point of polypropylene transparent nucleating agent

    CN104558823A

  • Synthesis method for 3,5-dimethyl benzaldehyde

    CN105753672A