Method for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as raw material
By using iron scales to prepare iron oxide red and hydrothermal complex precipitation technology in the metallurgical industry, the high temperature, high cost and complex process problems in solid waste treatment in the metallurgical industry are solved, and the high value-added lithium battery positive electrode material lithium iron phosphate is achieved The resource utilization of the company reduces production costs and wastewater discharge, and is suitable for industrial production.
Patent Information
- Application Number
- CN202210836286.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-15
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-07-15
AI Technical Summary
Traditional process treatment of metallurgy industry rich iron solid waste has problems such as high roasting temperature, low product added value, complex process flow, large amount of waste slag and waste liquid, and high production costs.
Iron oxide red is prepared by oxidation and roasting, water-thermal complexing leaching and hydrothermal reduction complexing precipitation, and lithium iron phosphate, which has good physical and chemical properties, simplifies the process flow, reduces the reaction temperature, and reduces the Waste residue is generated to improve product purity and added value.
It has realized the resource utilization and high-value utilization of bulk iron-containing solid waste in the metallurgical industry, reduced the production cost of lithium battery positive electrode materials, improved product purity and added value, simplified the process flow, reduced wastewater emissions, and was suitable for industrial scale production.
Smart Images

Figure CN115532770B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of comprehensive utilization of solid wastes in the steel industry, and specifically relates to a method for preparing lithium iron phosphate, a positive electrode material for lithium batteries with high added value, using iron oxide scraps - iron scales from steel mills as raw materials. Background Art
[0002] As non-renewable resources such as oil, coal, and natural gas are gradually exhausted, the development and utilization of new energy sources, such as nuclear energy, solar energy, and electric energy, are gradually becoming a research hotspot for scientific researchers and a key development direction for industry layout. Taking cheap and convenient electrochemical energy storage devices as an example, lithium-ion batteries have been rapidly developed due to their long cycle life, high safety, and more environmentally friendly characteristics. In 2020, my country's lithium battery production reached nearly 50 billion, an increase of more than 150% year-on-year; power battery production reached 217GWh, which has become the largest consumer end, and it is expected to even reach more than 1000GWh in 2025. This not only provides huge market application prospects for the development of lithium battery production technology, but also puts forward higher requirements and challenges for the improvement of lithium battery material performance and the optimization and control of costs.
[0003] Taking lithium-ion batteries as an example, their positive electrode materials often account for a larger proportion than negative electrode materials. Therefore, the properties of lithium battery positive electrode materials directly affect the performance of lithium-ion batteries, and their cost also directly determines the cost of the entire battery. Among a number of lithium battery positive electrode materials that have emerged in recent years, lithium iron phosphate has been widely used in various large-capacity energy storage components and high-power power battery equipment due to its advantages such as large capacity, high temperature resistance, long life, and low price. It is currently the energy storage material with the best comprehensive performance and the most promising application prospects. With the vigorous development and utilization of lithium iron phosphate materials in electric vehicles and energy storage batteries, its market scale and market capacity will be further expanded, and the prospects for promotion and application are very broad. Expanding the applicable scope of iron sources in the preparation of lithium iron phosphate materials and optimizing the preparation process of lithium iron phosphate are the key to solving its market and cost problems. Most of the solid waste resources generated by metallurgical enterprises are rich in Fe resources. If they can be used as raw materials for synthesizing lithium iron phosphate, it can not only solve the imminent solid waste treatment problem for steel enterprises, but also greatly reduce the production cost of lithium iron phosphate from the source, and the social and economic benefits are very obvious. Take the scales, iron oxide scraps and iron scales that fall off during the heating and rolling process of steel ingots and billets in steel mills as an example. The amount of scales in steel mills is about 2% to 3% of steel production, and my country produces 2 million to 10,000 tons of scales each year. Scales generally contain 70% to 75% iron, and the fine powder scales cleaned from the sedimentation tank of the rolling mill also contain about 60% iron; its SiO2, CaO, Al2O3 and MgO content are about 1% to 2%. At present, scales are mainly used as auxiliary raw materials for sintered ore and have not been used at a high value. There are also red iron oxide or reduced iron powder prepared from scales, but because the scales contain some impurities, the purity of the prepared red iron oxide products or reduced iron powder is not high, and the added value of the products is low. It is often necessary to remove impurities before producing red iron oxide or processing reduced iron powder.
[0004] The patent "A method for preparing red iron oxide from iron-containing waste and red iron oxide pigment" (CN201810770162.1) provides a method for preparing red iron oxide from iron-containing waste. The method first uses excess sodium hydroxide to convert the iron element in the iron-containing waste into ferric hydroxide or ferrous hydroxide, and then prepares γ-Fe2O3 by two-step drying in a closed environment at 400-800°C. However, the alkali consumption is high, the process flow is long, and the product purity is low, so enterprises are not very active in making technical improvements.
[0005] The article "Comprehensive Utilization Technology of Rolled Iron Scale" published in the 5th issue of the Chinese journal "Shandong Metallurgy" in 2013 gives various ways to utilize rolled iron scale, including: using rolled iron scale to make permanent ferrite materials, using rolled iron scale to make reduced iron powder, steel smelting recycling, iron scale for the chemical industry, and iron scale for the manufacture of ferrosilicon alloy. But in general, the production process is extremely complicated. Taking the process of manufacturing reduced iron powder as an example, its process flow is: primary reduction, rolled iron scale - drying - magnetic separation - crushing - screening - canning - tunnel kiln reduction - sponge iron; secondary reduction, sponge iron - cleaning - crushing - magnetic separation - hydrogen reduction furnace - powder block - crushing - magnetic separation - screening - classification - mixing - packaging - product.
[0006] In view of this, in order to address the technical difficulties faced by existing steel enterprises in the high-value utilization technology of iron scale, the present invention proposes a method for high-value utilization of iron scale, namely, a method for preparing lithium iron phosphate, a positive electrode material for lithium batteries. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects of high roasting temperature, low product added value, complex process flow, large amount of waste slag and waste liquid generated, and high production cost in traditional processes for treating iron-rich solid waste in the metallurgical industry, and provide a method for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as a raw material, which has the advantages of short process flow, simple equipment, low reaction temperature, milder reaction conditions, higher product added value, and less lithium source usage. The method prepares red iron oxide by oxidative roasting, prepares ferrous oxalate by hydrothermal complexation of red iron oxide, and synthesizes lithium iron phosphate, a positive electrode material for lithium batteries with good physical and chemical properties by solid phase reaction, thereby finally achieving the purpose of resource utilization and high-value utilization of large amounts of iron-containing solid waste in the metallurgical industry.
[0008] To achieve the above-mentioned purpose of the present invention, the present invention uses iron scale produced in the actual production activities of steel enterprises as raw materials to prepare red iron oxide, selects oxalic acid as a leaching agent and iron powder as a reducing agent, and transforms the abundant iron therein into high-purity ferrous oxalate through hydrothermal complex leaching and hydrothermal reduction complex precipitation, and uses the obtained ferrous oxalate as the main raw material to prepare lithium iron phosphate, a positive electrode material for lithium batteries with good physical and chemical properties. The method of the present invention for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as raw materials is specifically implemented by the following steps:
[0009] 1) Raw material preparation: Using iron scale, a solid waste of steel enterprises, as raw material, after ultra-fine grinding, obtains fine iron scale powder with a particle size of -0.074 mm and a content of ≥80.0%, preferably with a particle size of -0.074 mm and a content of ≥90.0%. Before preparing red iron oxide, the present invention does not need to remove impurities from the iron scale.
[0010] 2) Oxidation roasting to prepare red iron oxide: The fine iron scale powder obtained in step 1) is added into a rotary kiln for oxidation roasting to prepare red iron oxide, and the temperature in the rotary kiln is controlled in the range of 550° C. to 680° C. In this step of the present invention, the oxidant is natural air.
[0011] Since the final product of the present invention is not red iron oxide, the temperature in the rotary kiln is relatively low in this step, 20 to 150°C lower than the temperature of conventional rotary kiln for preparing red iron oxide, and the energy saving effect is obvious. Under this condition, 95% or more of the Fe in the iron scale is converted into Fe2O3.
[0012] 3) Hydrothermal complex leaching and iron extraction: The red iron oxide prepared in step 2) is added to the oxalic acid solution of designed concentration according to the calculated liquid-solid ratio, mixed thoroughly, and placed in a constant temperature reaction device, and the reaction temperature and reaction time are adjusted to make the iron oxide in the fine iron scale powder undergo hydrothermal complex reaction to generate Fe(C2O4)3 which is easily soluble in water and acid solution. 3- , and is free in the solution; after the hydrothermal complex reaction is completed, the reaction product is separated into solid and liquid, and after multiple filtration, washing and purification, an iron-rich complex ion leaching solution I is obtained.
[0013] The multiple times mentioned above refers to 3 times or more. Since iron scale is used as raw material in step 1), the impurity content of SiO2, CaO, Al2O3 and MgO in the iron scale is only 1% to 2%, and the impurity content of SiO2, CaO, Al2O3 and MgO in the prepared iron red is less than 1.5%, therefore, the amount of residual slag after solid-liquid separation of the reaction product in step 3) is very small, and can be directly mixed into the smelting charge as a batching.
[0014] 4) preparing ferrous oxalate by hydrothermal reduction of complex iron precipitation: using the iron-rich complex ion leaching solution I obtained in step 3) as a raw material, oxalic acid and reduced Fe powder as additives, controlling the reaction temperature, raw material ratio and reaction time, and precipitating ferrous oxalate crystals from the solution at normal temperature and pressure; the precipitated ferrous oxalate crystals are subjected to solid-liquid separation and vacuum drying to obtain high-purity ferrous oxalate powder with a purity of ≥99.0%.
[0015] 5) Synthesis of lithium iron phosphate by solid phase reaction: using the high-purity ferrous oxalate powder obtained in step 4) as the iron source for synthesizing lithium iron phosphate, lithium carbonate / lithium hydroxide as the lithium source, ammonium dihydrogen phosphate as the phosphorus source, and anhydrous ethanol as the medium to prepare a lithium iron phosphate precursor; after obtaining the lithium iron phosphate precursor, a two-step solid phase synthesis method is adopted in a reducing roasting atmosphere, and the mixture is kept warm at two different roasting temperatures of 350-500° C. and 650-900° C., and the holding time is 10-20 h and 20-32 h, respectively, to finally obtain a lithium iron phosphate product that meets the performance requirements of the lithium battery positive electrode material.
[0016] Furthermore, the liquid-to-solid ratio (ml / g) of oxalic acid to fine-grained iron scale powder in step 3) is preferably (12-35):1, preferably (15-20):1; the mass concentration of the oxalic acid solution is preferably 15-40%, preferably 20-25%; the reaction temperature is 50-95°C, preferably 70-85°C; the reaction time is 1-5h, preferably 1.5-2.5h.
[0017] Furthermore, the mass ratio of oxalic acid added in step 4) to the mass ratio of Fe in the iron-rich complex ion leachate I is (0.8-2.2):1, preferably (1.0-2.0):1; the mass ratio of reduced iron powder to Fe in the iron-rich complex ion leachate I is (3-4):1, (3.2-3.8):1; the reaction temperature is 60-90°C, preferably 75-85°C; the stirring speed is 300-400r / min, and the reaction time is 2-3h.
[0018] Furthermore, in step 4), the vacuum drying temperature of the vacuum drying treatment operation is 50-80°C, preferably 60-70°C; the vacuum degree is 10.13-30.39 kPa, preferably 10.13-20.26 kPa; and the drying time is 5-20 h, preferably 8-12 h.
[0019] As a further preferred embodiment of the present invention, in step 5), the mass ratio of high-purity ferrous oxalate powder, lithium carbonate / lithium hydroxide, and ammonium dihydrogen phosphate is preferably (2.0-2.5):1:(2.0-2.5); a two-step solid phase synthesis method is adopted, and the lithium iron phosphate synthesis is divided into two stages under a reducing roasting atmosphere: the first stage is preferably kept warm at a roasting temperature of 400-450°C for 12-15h; on the basis of completing the first stage reaction, the temperature is continued to be raised to 700-900°C to enter the second stage, and the second stage is preferably kept warm at a roasting temperature of 750-800°C for 24-28h.
[0020] Compared with the prior art, the method of preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as a raw material has the following advantages:
[0021] (1) The present invention provides a method for preparing lithium iron phosphate, a positive electrode material for lithium batteries with high added value, using iron scale, a bulk solid waste of the steel industry, such as rolled steel skin and iron filings, as raw materials. This is an unprecedented technical concept. Through the mutual coordination and comprehensive integration of five steps, lithium iron phosphate, a positive electrode material for lithium batteries with extremely high added value, is prepared from iron scale, a bulk, low-value solid waste of steel enterprises. This is a typical original innovation technology.
[0022] (2) Since the impurity content in the iron scale is low, less than 2%, the yield of the final product, lithium iron phosphate, anode material for lithium battery, is as high as 98.0% or more. The entire process only produces a small amount of solid-liquid separation residue in step 3). The components of the residue are mainly calcium, magnesium, silicon, and aluminum. The ingredients are directly mixed into the smelting furnace charge, so that the iron scale raw materials are 100% utilized, eliminating its pollution to the ecological environment while reducing the raw material cost of lithium iron phosphate, anode material for lithium battery. Considering the overall technical process, it can reduce the unit production cost by more than 60%, with obvious economic advantages.
[0023] (3) The present invention provides a method for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as a raw material. Compared with conventional technologies, the reaction mother liquor is returned to the pre-reaction process for recycling, and there is no need to neutralize the by-products, which saves a large amount of alkali solution required for the neutralization reaction and greatly reduces the discharge of wastewater. The overall environmental protection cost can be reduced by more than 60%; the process route is simple and controllable, and the yield can reach more than 90%, which is suitable for industrial-scale production;
[0024] (4) The present invention provides a method for resource-based and high-value utilization of large-scale solid waste iron scale in the metallurgical industry. In combination with the characteristics of lithium iron phosphate materials, iron-containing solid waste in the metallurgical industry is used as raw material, and different reaction conditions are selected to prepare ferrous oxalate powder with a particle size of 0.5 to 10 μm. The particle size is fully controllable; the product purity is greater than 99.0%, and can reach up to 99.8%, which is more in line with the product quality requirements of downstream battery manufacturers, with higher product added value and more competitiveness in the market;
[0025] (5) The present invention provides a method for using large-scale solid waste iron scale from the metallurgical industry as raw material, recycling it and making high-value use of it, and finally producing high-value-added product lithium iron phosphate. From the perspective of the overall production process of lithium iron phosphate, the preparation cost can be reduced by 60-70%, the technical and economic value is high, and it has a better industrialization prospect than traditional processes; the reaction conditions are mild, and some traditional production processes are simplified, which is conducive to saving investment, and the direct economic benefits are more obvious.
[0026] (6) The first reversible specific capacity of lithium iron phosphate, a positive electrode material for lithium batteries prepared by the method of the present invention, is 158.68 mAh g -1 After 25 cycles, it still maintains 158.65mAh·g -1 The reversible specific capacity and capacity retention rate are basically 100%, which indicates that it has excellent cycle stability.
[0027] (7) Electrochemical testing of the assembled 2025 button cell: The three charge and discharge curves basically overlap, indicating that LiFePO4 has good cycle stability during the charge and discharge process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a process flow chart of the principle of the method for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as a raw material according to the present invention;
[0029] Figure 2 The XRD diffraction pattern of ferrous oxalate powder prepared according to the method of the present invention adopts Cu-Kα target radiation, the diffraction angle 2θ is 10-90°C, and the X-ray wavelength λ is 0.15416nm;
[0030] Figure 3 The XRD diffraction spectrum of lithium iron phosphate powder prepared according to the method of the present invention adopts Cu-Kα target radiation, the diffraction angle 2θ is 10-90°C, and the X-ray wavelength λ is 0.15416nm. DETAILED DESCRIPTION
[0031] To describe the present invention, the method for preparing lithium iron phosphate, a positive electrode material for a lithium battery, using iron scale as a raw material is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0032] like Figure 1 As shown in the process flow chart of the method for preparing lithium iron phosphate, a positive electrode material of a lithium battery, from iron scale as a raw material, the method for preparing lithium iron phosphate, a positive electrode material of a lithium battery, from iron scale as a raw material, is implemented by the following steps:
[0033] 1) Raw material preparation: Using the solid waste iron scale of steel enterprises as raw material, after ultra-fine crushing, obtain fine iron scale powder with a particle size of -0.074mm and a content of ≥90.0%.
[0034] 2) Oxidation roasting to prepare red iron oxide: the fine iron scale powder obtained in step 1) is added into a rotary kiln for oxidation roasting to prepare red iron oxide, and the temperature of the rotary kiln is controlled in the range of 600°C to 650°C.
[0035] 3) Hydrothermal complex leaching and iron extraction: The red iron oxide prepared in step 2) is added to the oxalic acid solution of designed concentration according to the calculated liquid-solid ratio, mixed thoroughly, and placed in a constant temperature reaction device, and the reaction temperature and reaction time are adjusted to make the iron oxide in the fine iron scale powder undergo hydrothermal complex reaction to generate Fe(C2O4)3 which is easily soluble in water and acid solution. 3- , and free in the solution; after the hydrothermal complex reaction is completed, the reaction product is separated into solid and liquid, and after multiple filtration, washing and purification, an iron-rich complex ion leaching solution I is obtained. The liquid-solid ratio (ml / g) of oxalic acid to fine iron scale powder in this step is (15-20):1, the mass concentration of oxalic acid solution is 20-25%, the reaction temperature is 70-85°C, and the reaction time is 1.5-2.5h.
[0036] 4) preparing ferrous oxalate by hydrothermal reduction of complex iron precipitation: using the iron-rich complex ion leaching solution I obtained in step 3) as a raw material, oxalic acid and reduced Fe powder as additives, controlling the reaction temperature, raw material ratio and reaction time, and precipitating ferrous oxalate crystals from the solution at normal temperature and pressure; the precipitated ferrous oxalate crystals are subjected to solid-liquid separation and vacuum drying to obtain high-purity ferrous oxalate powder with a purity of ≥99.0%.
[0037] The mass ratio of oxalic acid added in this step to the mass ratio of Fe in the iron-rich complex ion leachate I is (1.0-2.0):1, the mass ratio of reduced iron powder to Fe in the iron-rich complex ion leachate I is (3.2-3.8):1, the reaction temperature is 75-85°C, the stirring speed is 300-400r / min, and the reaction time is 2-3h; the vacuum drying temperature of the vacuum drying treatment operation is 60-70°C, the vacuum degree is 10.13-20.26kPa, and the drying time is 8-12h.
[0038] 5) Solid phase reaction synthesis of lithium iron phosphate: using the high-purity ferrous oxalate powder obtained in step 4) as the iron source for synthesizing lithium iron phosphate, lithium carbonate / lithium hydroxide as the lithium source, ammonium dihydrogen phosphate as the phosphorus source, and anhydrous ethanol as the medium to prepare a lithium iron phosphate precursor; after obtaining the lithium iron phosphate precursor, a two-step solid phase synthesis method is used in a reducing roasting atmosphere, and the heat is maintained at two different roasting temperatures of 400-450°C and 750-800°C, and the heat preservation time is 12-15h and 24-28h, respectively, to finally obtain a lithium iron phosphate product that meets the performance requirements of lithium battery positive electrode materials. In this step, the mass ratio of high-purity ferrous oxalate powder, lithium carbonate / lithium hydroxide, and ammonium dihydrogen phosphate is (2.0-2.5):1:(2.0-2.5).
[0039] The invention will be described in detail below in conjunction with specific embodiments. The method for preparing lithium iron phosphate, a positive electrode material for a lithium battery, using iron scale as a raw material is specifically implemented using the following process steps:
[0040] (1) Solid waste iron scale from Maanshan Iron and Steel Rolling Mill was used as raw material, and after ultra-fine grinding, fine iron scale powder with a particle size of -0.074 mm and a content of ≥90.0% was obtained; red iron oxide was prepared in the laboratory using the obtained fine iron scale powder as raw material; 1 g of red iron oxide was weighed.
[0041] (2) The red iron oxide sample obtained in step (1) was mixed with 20% oxalic acid solution at a liquid-to-solid ratio of 20:1. After being fully mixed to form a uniform slurry, it was placed in a constant temperature water bath. The reaction conditions were specifically set as follows: leaching temperature of 85°C, reaction time of 2h, and stirring speed of 400r / min. After the hydrothermal complex reaction was completed, the reaction product was separated into solid and liquid to obtain an iron-rich complex ion leaching solution I and the volume was fixed to 250mL. At this time, ICP-AES analysis showed that the concentration of Fe in the leaching solution I was 2572mg / L.
[0042] (3) Using the leachate I in the above arrangement as the reaction raw material, high-purity ferrous oxalate powder was prepared. The specific reaction conditions were: adding 1.08g oxalic acid, 2.02g reduced iron powder, leaching temperature of 85°C, reaction time of 2h, stirring speed of 400r / min. After the reaction was completed, the solution was cooled to room temperature for solid-liquid separation, and the solid obtained by the filtration reaction was vacuum dried at 65°C and a vacuum degree of 10.13kPa for 12h to finally obtain high-purity ferrous oxalate powder. The XRD diffraction pattern of the reaction product is as follows: Figure 2 shown by Figure 2 It can be seen that the Cu-Kα target radiation used has a diffraction angle 2θ of 10 to 90°C and an X-ray wavelength λ of 0.15416nm. Figure 2 It can be seen that compared with the ferrous oxalate standard card, the ferrous oxalate powder prepared using red iron oxide has good crystallization performance, high strength, and does not contain any impurity peaks. The prepared ferrous oxalate powder has a purity of 98.75% after analysis and testing.
[0043] (4) The ferrous oxalate obtained in the above step was used as a raw material, and lithium iron phosphate was prepared by a two-step method using a solid phase reaction method. The specific experimental conditions were as follows: 1.8 g of ferrous oxalate, 0.37 g of lithium carbonate and 1.5 g of ammonium dihydrogen phosphate were weighed respectively, and alcohol was used as a medium to fully grind and prepare a precursor; under reducing roasting conditions, first, the temperature was kept at 400°C for 12 hours; after the temperature was kept at 750°C, the temperature was immediately raised and the temperature was continued to be kept at 750°C for 24 hours; after the reaction was completed, the system was cooled, and the sample was taken out after the furnace was cooled. The XRD diffraction pattern of the reaction product is as follows: Figure 3 As shown. Figure 3 It can be seen that the Cu-Kα target radiation used has a diffraction angle 2θ of 10 to 90°C and an X-ray wavelength λ of 0.15416nm. Figure 3 It can be seen that compared with the lithium iron phosphate standard card, the lithium iron phosphate powder prepared using red iron oxide has good crystallization performance, high peak intensity, and does not contain any impurity peaks; through further experimental testing, it can be seen that the purity of the lithium iron phosphate powder at this time is 99.10%.
[0044] The lithium iron phosphate cathode material of the lithium battery prepared by the method embodiment of the present invention was subjected to constant current charge and discharge test at a current density of 0.1C. The first charge and discharge specific capacities of the synthesized lithium iron phosphate material were 158.68 mAh·g -1 and 165.03mAh·g -1 The first coulombic efficiency reached 104.0%. After 25 cycles, it still maintained 158.65mAh·g -1 The reversible specific capacity of LiFePO4 is 100%, and the capacity retention rate is basically 100%, which shows that it has excellent cycle stability. The electrochemical test of the assembled 2025 button battery shows that the three charge and discharge curves are basically the same, indicating that LiFePO4 has good cycle stability during the charge and discharge process.
[0045] The upper and lower limits and interval values of the raw materials and process parameters involved in the present invention can all achieve the product of the present invention, and are not listed here one by one.
Claims
1. A method for preparing lithium iron phosphate, a positive electrode material for lithium batteries, using iron scale as raw material, characterized in that This is done using the following steps: 1) Raw material preparation: solid waste scale from steel enterprises is used as raw material, and after ultra-fine crushing, fine-grained scale powder with a particle size of -0.074 mm and a content of ≥80.0% is obtained; 2) Oxidation roasting to prepare red iron oxide: the fine iron scale powder obtained in step 1) is added into a rotary kiln for oxidation roasting to prepare red iron oxide, and the temperature in the rotary kiln is controlled in the range of 550° C. to 650° C.; 3) Hydrothermal complex leaching and iron extraction: The red iron oxide prepared in step 2) is added to the oxalic acid solution of designed concentration according to the calculated liquid-solid ratio, mixed thoroughly, and placed in a constant temperature reaction device, and the reaction temperature and reaction time are adjusted to make the iron oxide in the fine iron scale powder undergo hydrothermal complex reaction to generate Fe(C2O4)3 which is easily soluble in water and acid solution. 3- , and free in the solution; After the hydrothermal complex reaction is completed, the reaction product is subjected to solid-liquid separation, and after multiple filtration, washing and purification, an iron-rich complex ion leaching solution I is obtained; the liquid-solid ratio (ml / g) of oxalic acid to fine iron scale powder in this step is (12-35):1, the mass concentration of the oxalic acid solution is 15-40%, the reaction temperature is 50-95°C, and the reaction time is 1-5h; 4) preparing ferrous oxalate by hydrothermal reduction of complex iron precipitation: using the iron-rich complex ion leachate I obtained in step 3) as a raw material, oxalic acid and reduced Fe powder as additives, controlling the reaction temperature, raw material ratio and reaction time, and precipitating ferrous oxalate crystals from the solution at room temperature and pressure; the precipitated ferrous oxalate crystals are subjected to solid-liquid separation and vacuum drying to obtain high-purity ferrous oxalate powder with a purity of ≥99.0%; the mass ratio of oxalic acid added in this step to the mass ratio of Fe in the iron-rich complex ion leachate I is (0.8-2.2):1, the mass ratio of reduced iron powder to Fe in the iron-rich complex ion leachate I is (3-4):1, the reaction temperature is 60-90°C, the stirring speed is 300-400r / min, and the reaction time is 2-3h; 5) Synthesis of lithium iron phosphate by solid phase reaction: using the high-purity ferrous oxalate powder obtained in step 4) as the iron source for synthesizing lithium iron phosphate, lithium carbonate / lithium hydroxide as the lithium source, ammonium dihydrogen phosphate as the phosphorus source, and anhydrous ethanol as the medium to prepare a lithium iron phosphate precursor; After obtaining the lithium iron phosphate precursor, a two-step solid-phase synthesis method is used under a reducing calcination atmosphere, and the calcination is carried out at two different calcination temperatures of 350-500°C and 650-900°C, with the insulation time being 10-20h and 20-32h respectively, to finally obtain a lithium iron phosphate product that meets the performance requirements of lithium battery positive electrode materials.
2. The method for preparing lithium iron phosphate as a positive electrode material for a lithium battery using iron scale as a raw material according to claim 1, characterized in that: The liquid-to-solid ratio (ml / g) of oxalic acid to fine iron scale powder in step 3) is (15-20):1, the mass concentration of the oxalic acid solution is 20-25%, the reaction temperature is 70-85°C, and the reaction time is 1.5-2.5h.
3. The method for preparing lithium iron phosphate as a positive electrode material for a lithium battery using iron scale as a raw material according to claim 1 or 2, characterized in that: The mass ratio of oxalic acid added in step 4) to the mass ratio of Fe in the iron-rich complex ion leaching solution I is (1.0-2.0):1, the mass ratio of reduced iron powder to Fe in the iron-rich complex ion leaching solution I is (3.2-3.8):1, and the reaction temperature is 75-85°C.
4. The method for preparing lithium iron phosphate as a positive electrode material for a lithium battery using iron scale as a raw material as claimed in claim 3, characterized in that: In step 4), the vacuum drying temperature of the vacuum drying treatment operation is 50-80° C., the vacuum degree is 10.13-30.39 kPa, and the drying time is 5-20 hours.
5. The method for preparing lithium iron phosphate as a positive electrode material for lithium batteries using iron scale as a raw material according to claim 4, characterized in that: In step 4), the vacuum drying temperature of the vacuum drying treatment operation is 60-70° C., the vacuum degree is 10.13-20.26 kPa, and the drying time is 8-12 hours.
6. The method for preparing lithium iron phosphate as a positive electrode material for lithium batteries using iron scale as a raw material according to claim 5, characterized in that: In step 5), the mass ratio of high-purity ferrous oxalate powder, lithium carbonate / lithium hydroxide, and ammonium dihydrogen phosphate is (2.0-2.5):1:(2.0-2.5); the first stage is kept warm at a roasting temperature of 400-450°C for 12-15 hours, and the second stage is kept warm at a roasting temperature of 750-800°C for 24-28 hours.
Citation Information
Patent Citations
Method for preparing iron oxide red by utilizing iron-containing wastes and iron oxide red pigment
CN108793263A
Lithium iron phosphate / carbon composite anode material prepared by catalytic graphitization method, and preparation method thereof
CN102347476A
Method for preparing lithium ferrous silicate positive pole material from ilmenite
CN103326022A
Method for recycling positive material from water-system waste lithium iron phosphate battery
CN103449395A
Method of manufacturing cathode active material for lithium battery cell
KR1020160027754A