High-flexibility display film and preparation method and application thereof

Through the combination of modified PVB resin and modified particles, heterojunction structure and composite skeleton particles are formed, which solves the shortcomings of traditional display films in terms of flexibility, electrical and high temperature stability, significantly improves the performance of the display film, and is suitable for electronics Display membrane equipment.

CN119039726AInactive Publication Date: 2024-11-29SHENZHEN SHENKUN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036447.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional projection display films have shortcomings in flexibility, electrical properties and high temperature stability, which limits the development of high-performance display films.

Method used

Using modified PVB resin and modified particle composition, heterojunction structure and composite skeleton particles are formed by sulfonating carbon nanotubes and zinc oxide, thereby improving the mechanical, electrical and waterproof properties of the display film, and through the modified particles Light energy excitation forms an electron circulation system, enhancing the electron flow and heat dissipation capabilities.

Benefits of technology

It significantly improves the flexibility, mechanical, electrical and high-temperature stability of the display film, enhances its performance in high-temperature environment, and is suitable for the use of electronic display film equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971206960000141
    Figure BDA0004971206960000141
Patent Text Reader

Abstract

The invention relates to the field of display films, in particular to a high-flexibility display film and a preparation method and application thereof. The high-flexibility display film comprises the following raw materials in parts by mass: 60-80 parts of PVB resin, 1-10 parts of scattering particles, 5-10 parts of modified particles, 1-5 parts of a blue light absorbent, 1-5 parts of a dispersing agent, 1-5 parts of a curing agent, 10-20 parts of a plasticizer and 60-120 parts of an organic solvent. The display film prepared in the invention keeps good flexibility on the basis of having excellent mechanical properties, and the electrical properties, high-temperature stability and waterproofness of the display film are further improved, so that the display film can meet the use requirements of existing electronic display film equipment, and has very excellent market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display films, and in particular to a highly flexible display film and a preparation method and application thereof. Background Art

[0002] In recent years, with the rapid development of information technology, projection equipment, computers, vehicle-mounted equipment and various intelligent devices have become an indispensable part of people's daily life and work. Among them, the display of the above-mentioned equipment is an important interface for interaction between people and machines, and its performance is closely related to the user's visual experience. Therefore, with the continuous development and improvement of the above-mentioned equipment, traditional display devices face more and more challenges in the above-mentioned application scenarios, including but not limited to technical problems such as flexibility problems (for projection systems, etc.), visual fatigue (for computers, etc.), and easy screen dirtiness. Especially in recent years, under the premise that interactive projection, electronically controlled projection and other projection equipment are widely favored by consumers, the performance requirements for projection display films have also increased.

[0003] Projection display film (also called projection display film) is a new type of projection imaging film. It has high visible light transmittance and can be attached to transparent glass or substrate (fiber curtain, etc.) for use. Based on the requirements for visible light transmittance and transparency, polyvinyl butyral resin (PVB) is used in the preparation of display film because of its excellent transparency, film-forming properties, adhesion and impact resistance. However, PVB has its own problems of electrical mismatch, poor flexibility and poor high-temperature stability, which further limits the research and development of high-performance display films.

[0004] Because, in order to effectively solve the above problems, the applicant provides a highly flexible display film and a method for preparing the same, and applies the prepared highly flexible display film to the preparation of electronic display film equipment (projection display film, etc.). The display film prepared in this application has excellent mechanical properties while maintaining good flexibility, and further improves its own electrical properties, high temperature stability and waterproofness, so that it can be applied to the use requirements of existing electronic display film equipment and has a very excellent market prospect. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present application provides a highly flexible display film, in which the raw materials include, by mass: 60 to 80 parts of PVB resin, 1 to 10 parts of scattering particles, 5 to 10 parts of modified particles, 1 to 5 parts of blue light absorbers, 1 to 5 parts of dispersants, 1 to 5 parts of curing agents, 10 to 20 parts of plasticizers, and 60 to 120 parts of organic solvents.

[0006] As a preferred solution, the PVB resin is a composition of PVB and modified PVB.

[0007] As a preferred solution, the refractive index of the PVB resin is 1.48-1.49.

[0008] As a preferred solution, the mass ratio of the PVB to the modified PVB is (6-7): (1-1.5).

[0009] As a preferred solution, the mass ratio of the PVB to the modified PVB is (6-6.5):(1-1.2).

[0010] As a preferred scheme, the preparation method of the modified PVB includes the following steps: S1: dispersing sulfonated carbon nanotubes in deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving PVA in deionized water to obtain a PVA solution for standby use; S2: maintaining the temperature of the PVA solution at 40-50°C, adding butyraldehyde and stirring for 0.5-1h, then adding the sulfonated carbon nanotube dispersion and mixing and stirring evenly, heating to 60-80°C, keeping warm and stirring for 2-3h, and after completion, filtering and washing the product, and vacuum drying at 40-50°C to obtain the product.

[0011] As a preferred solution, the mass ratio of the sulfonated carbon nanotubes, PVA and butyraldehyde is (0.4-0.8):(12-16):(6-8).

[0012] As a preferred solution, the mass ratio of the sulfonated carbon nanotubes, PVA and butyraldehyde is (0.5-0.7): (14-16): (6.5-7.5).

[0013] As a preferred solution, the average particle size of the sulfonated carbon nanotubes is 5 to 20 nm.

[0014] As a preferred solution, the average particle size of the sulfonated carbon nanotubes is 8 to 15 nm.

[0015] In this application, by adding modified PVB raw materials, the thermal stability, mechanical and waterproof properties of the display film can be greatly improved. The modified PVB raw materials can form a certain degree of heterojunction structure with the subsequent modified particles through the added sulfonated carbon nanotubes. The existence of this structure can greatly improve the flow activity and speed of electrons and carriers, thereby providing good photoelectric performance and facilitating electron transmission; on the other hand, the connection structure formed by it can effectively form a heat conduction path, thereby forming a good heat dissipation path under high temperature environment, thereby avoiding the excessive activity of internal molecules under high temperature environment, avoiding the probability of direct reaction between them, and reducing the yellowing phenomenon under high temperature; the particle connection structure finally formed can have good self-connection strength and form composite particle holes, which can serve as an internal connection bridge of the display film when external force acts, and dissipate external stress through the action of holes, so that the cracks that are about to be formed are converted back into silver streaks, thereby effectively improving its mechanical and flexibility properties.

[0016] As a preferred solution, the mass ratio of the PVB resin, scattering particles and modified particles is (7-8): (0.3-0.5): (0.6-1).

[0017] As a preferred solution, the mass ratio of the PVB resin, scattering particles and modified particles is (7-8): (0.4-0.5): (0.6-0.8).

[0018] As a preferred solution, the scattering particles are at least one of aluminum oxide, zinc oxide, titanium dioxide, zirconium oxide, antimony oxide, and cesium oxide.

[0019] As a preferred solution, the scattering particles are a composition of aluminum oxide and zirconium oxide.

[0020] As a preferred solution, the mass ratio of aluminum oxide to zirconium oxide is (5-7):(3-4).

[0021] As a preferred solution, the mass ratio of aluminum oxide to zirconium oxide is (6-6.5): (3.5-4).

[0022] As a preferred solution, the average particle size of the aluminum oxide is 100-150 nm.

[0023] As a preferred solution, the average particle size of the zirconium oxide is 800-1400 nm.

[0024] As a preferred solution, the preparation method of the modified particles includes the following steps: S1: zinc oxide, sodium dodecyl sulfate, silane coupling agent and succinic anhydride are mixed uniformly in deionized water, heated to 40-60°C, kept warm and stirred for 3-4 hours to obtain pretreated zinc oxide; S2: the pretreated zinc oxide is added to the DMF solution and trimesic acid is added to mix uniformly, and then the DMF solution containing copper acetate is added dropwise, the dropping temperature is 60-65°C, the dropping time is 1-1.5 hours, and after the dropwise addition is completed, the temperature is kept for 2-4 hours, and the particle size is sampled during the period; S3: when the particle size reaches the desired range, triethanolamine is added to adjust the pH to 6.8-7.2, and the pH is naturally reduced to room temperature, the product is centrifuged and filtered, and vacuum dried at 60-70°C to obtain.

[0025] As a preferred solution, the average particle size of the zinc oxide is 10 to 20 nm.

[0026] As a preferred solution, the average particle size of the modified particles is 500-600 nm.

[0027] As a preferred solution, the mass ratio of zinc oxide to sodium dodecyl sulfate, silane coupling agent and succinic anhydride is (2-3): (0.5-1.2): (0.2-0.4): (1-1.5).

[0028] As a preferred solution, the mass ratio of the pretreated zinc oxide, trimesic acid and cupric acetate is (0.8-1): (1.5-1.8): (3.5-4).

[0029] As a preferred solution, the mass ratio of the pretreated zinc oxide, trimesic acid and cupric acetate is 1:1.6:3.8.

[0030] In this application, by adding the above-mentioned modified particles as the raw materials for preparing the highly flexible display film, the high temperature stability, flexibility / mechanical properties and waterproofness of the display film can be greatly improved. First, the added modified particles can not only form a good scattering / diffusion effect with the scattering particles through their specific particle size, but more importantly, the prepared specific modified particles can be excited by the light energy of the irradiation effect, forming a good electron flow system, thereby enhancing its electron flow promotion effect to give the display film good electrical properties; secondly, the skeleton particles formed in the modified particles can be coordinated and combined with the active zinc oxide particles to form a composite skeleton particle wrapped with zinc oxide. The presence of the particles can form an excellent connection with the PVB resin system through the active groups on the surface of zinc oxide, thereby playing an excellent internal connection and barrier role respectively when external forces act and water molecules invade, thereby greatly improving the mechanics and flexibility of the display film, and adsorbing and storing excess water molecules inside, reducing the attraction of internal water molecules to external moisture, and improving waterproof performance, and the excellent high temperature stability of the modified particles themselves can maintain the stability of internal molecules in a high temperature environment, reduce the collision and contact probability between active molecules in a high temperature environment, and thus reduce the occurrence of active reactions, greatly improving stability.

[0031] As a preferred solution, the mass ratio of the blue light absorber to the plasticizer is (0.3-0.5):(1.2-1.8).

[0032] As a preferred solution, the mass ratio of the blue light absorber to the plasticizer is (0.4-0.45):(1.4-1.8).

[0033] As a preferred solution, the curing agent is at least one of isocyanate, anhydride curing agent, benzophenone, and benzoin ether.

[0034] As a preferred solution, the curing agent is isocyanate.

[0035] As a preferred solution, the plasticizer is at least one of aliphatic diesters and D-380.

[0036] As a preferred solution, the plasticizer is an aliphatic diester; the aliphatic diester is at least one of 3GH, 3G7, 3G8, and 4G7.

[0037] As a preferred solution, the organic solvent is a combination of methanol and isopropanol.

[0038] As a preferred solution, the mass ratio of methanol to isopropanol is (4-5):1.

[0039] The second aspect of the present application provides a method for preparing the above-mentioned high-flexibility display film, and the preparation method comprises the following steps: S1: adding PVB resin to an organic solvent and stirring evenly to obtain a resin base liquid for use; S2: mixing the scattering particles and the modified particles evenly and mixing them with a plasticizer and adding them to the resin base liquid, heating the temperature to 50-60°C, then adding a blue light absorber, a dispersant and a curing agent in sequence and stirring evenly in a high-speed stirrer to obtain a pre-product; S3: then dehydrating the pre-product and extruding it into a film, heating it at 60-65°C until it is completely cured into a film, and obtaining the pre-product.

[0040] A third aspect of the present application provides an application of the above-mentioned highly flexible display film in the preparation of an electronic display film device.

[0041] The beneficial effects of this application are:

[0042] 1. A highly flexible display film provided in the present application has excellent mechanical properties while maintaining good flexibility, and further improves its own electrical properties, high temperature stability and waterproofness, so that it can be suitable for the use requirements of existing electronic display film equipment and has very excellent market prospects.

[0043] 2. A highly flexible display film provided in the present application, which adds modified PVB raw materials, can greatly improve the thermal stability, mechanical and waterproof properties of the display film. The modified PVB raw materials can form a certain degree of heterojunction structure with the subsequently modified particles through the added sulfonated carbon nanotubes. The existence of this structure can greatly improve the flow activity and speed of electrons and carriers; on the other hand, the connection structure formed by it can effectively form a heat conduction path, and then form a good heat dissipation path under a high temperature environment, thereby avoiding the excessive activity of internal molecules under a high temperature environment, avoiding the probability of direct reaction between them, and reducing the yellowing phenomenon under high temperature; the particle connection structure finally formed can have good self-connection strength and form composite particle holes, which can serve as an internal connection bridge of the display film when an external force acts, and dissipate external stress through the action of holes.

[0044] 3. A highly flexible display film provided in the present application, wherein the modified particles added thereto can provide the display film with suitable optoelectronic properties and mechanical / flexibility properties. The added modified particles can not only form a good scattering / diffusion effect with the scattering particles through their specific particle size, but more importantly, the prepared specific modified particles can be excited by light energy under irradiation to form a good electron flow system, and the skeleton particles formed in the modified particles can coordinate and combine with the active zinc oxide particles to form composite skeleton particles wrapped with zinc oxide. The presence of the particles can form an excellent connection with the PVB resin system through the active groups on the surface of zinc oxide, thereby playing an excellent internal connection and barrier role respectively when external forces act and water molecules invade.

[0045] 4. A highly flexible display film provided in the present application, the added modified particles can also effectively improve the waterproof performance and high-temperature stability of the display film. The modified particles can absorb and store excess water molecules inside, reduce the attraction of internal water molecules to external moisture, and improve the waterproof performance. The excellent high-temperature stability of the modified particles themselves can maintain the internal molecular stability in a high-temperature environment, reduce the collision and contact probability between active molecules in a high-temperature environment, thereby reducing the occurrence of active reactions and greatly improving stability. DETAILED DESCRIPTION

[0046] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.

[0047] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.

[0048] Example 1

[0049] Embodiment 1 The first aspect provides a highly flexible display film, in which the raw materials include, by mass: 75 parts of PVB resin, 5 parts of scattering particles, 6.5 parts of modified particles, 4.2 parts of blue light absorber, 4 parts of dispersant, 2.5 parts of curing agent, 15 parts of plasticizer, and 100 parts of organic solvent.

[0050] PVB resin is a composition of PVB and modified PVB, with a mass ratio of 6.5: 1. PVB was purchased from an industrial-grade PVB product sold by Jinan Huijinchuan Trading Co., Ltd., with a refractive index of 1.485.

[0051] The preparation method of modified PVB includes the following steps, calculated by mass: S1: dispersing 0.65 parts of sulfonated carbon nanotubes in 50 parts of deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving 12 parts of PVA in 150 parts of deionized water to obtain a PVA solution for standby use; S2: maintaining the temperature of the PVA solution at 45°C, adding 7 parts of butyraldehyde and stirring for 0.6h, then adding the sulfonated carbon nanotube dispersion and mixing and stirring evenly, heating to 65°C, keeping warm and stirring for 3h, and after completion, filtering and washing the product, and vacuum drying at 50°C to obtain the product.

[0052] PVA was purchased from the AX-600 product sold by Japan Synthetic Chemical Industry; sulfonated carbon nanotubes were purchased from the products sold by Xi'an Qiyue Biological, with an average particle size of 10 nm.

[0053] The scattering particles are a combination of aluminum oxide and zirconium oxide, with a mass ratio of 6.5:3.5. The average particle size of the aluminum oxide is 120 nm, and the average particle size of the zirconium oxide is 1000 nm.

[0054] The preparation method of modified particles includes the following steps, calculated by mass: S1: 2.6 parts of zinc oxide, 0.8 parts of sodium dodecyl sulfate, 0.38 parts of γ-aminopropyltriethoxysilane and 1.42 parts of succinic anhydride are mixed evenly in 60 parts of deionized water, heated to 55°C and stirred for 3.2 hours to obtain pretreated zinc oxide; S2: 1 part of pretreated zinc oxide is added to 50 parts of DMF solution and 1.6 parts of trimesic acid are added to mix evenly, and then a DMF solution containing 3.8 parts of copper acetate (30 parts in total) is added dropwise, the dropping temperature is 60°C, the dropping time is 1.2 hours, and after the dropping is completed, the temperature is kept for 3.4 hours, and the particle size is sampled and detected during the period; S3: when the particle size reaches the desired range, triethanolamine is added to adjust the pH to 7, and the pH is naturally reduced to room temperature. The product is centrifuged and filtered, and vacuum dried at 65°C to obtain.

[0055] The average particle size of zinc oxide was 15 nm, and the average particle size of the modified particles was 580 nm.

[0056] The blue light absorber is the JEDEC 1227 model product of Qingdao Jiebaiao.

[0057] The dispersant is BYK-162; the curing agent is isocyanate; and the plasticizer is 3G7.

[0058] The organic solvent is a combination of methanol and isopropanol, and the mass ratio of the two is 4:1.

[0059] The second aspect of the present embodiment provides a method for preparing the above-mentioned high-flexibility display film, and the preparation method includes the following steps: S1: adding PVB resin to an organic solvent and stirring evenly to obtain a resin base liquid for use; S2: mixing the scattering particles and modified particles evenly and mixing them with a plasticizer and adding them to the resin base liquid, heating to 55°C, and then adding a blue light absorber, a dispersant and a curing agent in turn and stirring evenly in a high-speed stirrer to obtain a pre-product; S3: then dehydrating the pre-product and extruding it into a film, heating it at 65°C until it is completely cured into a film, and obtaining the product.

[0060] Example 2

[0061] Embodiment 2 The first aspect provides a highly flexible display film, in which the raw materials include, by mass: 72 parts of PVB resin, 3.5 parts of scattering particles, 7.2 parts of modified particles, 4.5 parts of blue light absorber, 4 parts of dispersant, 2.5 parts of curing agent, 16 parts of plasticizer, and 90 parts of organic solvent.

[0062] PVB resin is a composition of PVB and modified PVB, with a mass ratio of 6:1.2. PVB was purchased from the industrial-grade PVB product sold by Jinan Huijinchuan Trading Co., Ltd., with a refractive index of 1.485.

[0063] The preparation method of modified PVB includes the following steps, calculated by mass: S1: dispersing 0.65 parts of sulfonated carbon nanotubes in 50 parts of deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving 12 parts of PVA in 150 parts of deionized water to obtain a PVA solution for standby use; S2: maintaining the temperature of the PVA solution at 45°C, adding 7 parts of butyraldehyde and stirring for 0.6h, then adding the sulfonated carbon nanotube dispersion and mixing and stirring evenly, heating to 65°C, keeping warm and stirring for 3h, and after completion, filtering and washing the product, and vacuum drying at 50°C to obtain the product.

[0064] PVA was purchased from the AX-600 product sold by Japan Synthetic Chemical Industry; sulfonated carbon nanotubes were purchased from the products sold by Xi'an Qiyue Biological, with an average particle size of 10 nm.

[0065] The scattering particles are a combination of aluminum oxide and zirconium oxide, and the mass ratio of the two is 6:4. The average particle size of the aluminum oxide is 120nm, and the average particle size of the zirconium oxide is 1000nm.

[0066] The preparation method of modified particles includes the following steps, calculated by mass: S1: 2.6 parts of zinc oxide, 0.8 parts of sodium dodecyl sulfate, 0.38 parts of γ-aminopropyltriethoxysilane and 1.42 parts of succinic anhydride are mixed evenly in 60 parts of deionized water, heated to 55°C and stirred for 3.2 hours to obtain pretreated zinc oxide; S2: 1 part of pretreated zinc oxide is added to 50 parts of DMF solution and 1.6 parts of trimesic acid are added to mix evenly, and then a DMF solution containing 3.8 parts of copper acetate (30 parts in total) is added dropwise, the dropping temperature is 60°C, the dropping time is 1.2 hours, and after the dropping is completed, the temperature is kept for 3.4 hours, and the particle size is sampled and detected during the period; S3: when the particle size reaches the desired range, triethanolamine is added to adjust the pH to 7, and the pH is naturally reduced to room temperature. The product is centrifuged and filtered, and vacuum dried at 65°C to obtain.

[0067] The average particle size of zinc oxide was 15 nm, and the average particle size of the modified particles was 580 nm.

[0068] The blue light absorber is the JEDEC 1227 model product of Qingdao Jiebaiao.

[0069] The dispersant is BYK-162; the curing agent is isocyanate; and the plasticizer is 3G7.

[0070] The organic solvent is a combination of methanol and isopropanol, and the mass ratio of the two is 4:1.

[0071] The second aspect of the present embodiment provides a method for preparing the above-mentioned high-flexibility display film, and the preparation method includes the following steps: S1: adding PVB resin to an organic solvent and stirring evenly to obtain a resin base liquid for use; S2: mixing the scattering particles and modified particles evenly and mixing them with a plasticizer and adding them to the resin base liquid, heating to 55°C, and then adding a blue light absorber, a dispersant and a curing agent in turn and stirring evenly in a high-speed stirrer to obtain a pre-product; S3: then dehydrating the pre-product and extruding it into a film, heating it at 65°C until it is completely cured into a film, and obtaining the product.

[0072] Comparative Example 1

[0073] The specific implementation of this comparative example is basically the same as that of Example 1, except that the PVB resin is a composition of PVB and modified PVB, and the mass ratio of PVB to modified PVB is 9.5:0.5.

[0074] Comparative Example 2

[0075] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of modified PVB comprises the following steps, measured in parts by mass: S1: dispersing 0.15 parts of sulfonated carbon nanotubes in 50 parts of deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving 20 parts of PVA in 250 parts of deionized water to obtain a PVA solution for standby use; S2: keeping the temperature of the PVA solution at 45°C, adding 10 parts of butyraldehyde and stirring for 0.8h, then adding the sulfonated carbon nanotube dispersion and mixing and stirring evenly, heating to 65°C, keeping warm and stirring for 3h, filtering and washing the product after completion, and drying in vacuo at 50°C to obtain the product.

[0076] Comparative Example 3

[0077] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of modified PVB comprises the following steps, measured in parts by mass: S1: dispersing 1.8 parts of sulfonated carbon nanotubes in 50 parts of deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving 10 parts of PVA in 120 parts of deionized water to obtain a PVA solution for standby use; S2: maintaining the temperature of the PVA solution at 45°C, adding 4 parts of butyraldehyde and stirring for 0.6h, then adding the sulfonated carbon nanotube dispersion and mixing and stirring evenly, heating to 65°C, keeping warm and stirring for 3h, and after completion, filtering and washing the product, and vacuum drying at 50°C to obtain the product.

[0078] Comparative Example 4

[0079] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the raw materials of the high-flexibility display film, in parts by mass, include: 75 parts of PVB resin, 8 parts of scattering particles, 2.5 parts of modified particles, 4.2 parts of blue light absorber, 4 parts of dispersant, 2.5 parts of curing agent, 15 parts of plasticizer, and 100 parts of organic solvent.

[0080] Comparative Example 5

[0081] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles includes the following steps, calculated by mass: S1: 2.6 parts of zinc oxide, 0.8 parts of sodium dodecyl sulfate, 0.38 parts of γ-aminopropyltriethoxysilane and 1.42 parts of succinic anhydride are mixed uniformly in 60 parts of deionized water, heated to 55°C and stirred for 3.2 hours to obtain pretreated zinc oxide; S2: 0.5 parts of pretreated zinc oxide are added to 40 parts of DMF solution and 2.2 parts of trimesic acid are added to mix uniformly, and then a DMF solution containing 4.5 parts of copper acetate (40 parts in total) is added dropwise, the dropping temperature is 60°C, the dropping time is 1.6 hours, and after the dropping is completed, the temperature is kept for 3.2 hours, and the particle size is sampled and detected during the period; S3: when the particle size reaches the desired range, triethanolamine is added to adjust the pH to 7, and the pH is naturally reduced to room temperature. The product is centrifuged and filtered, and vacuum dried at 65°C to obtain.

[0082] Comparative Example 6

[0083] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, in parts by mass: S1: adding 2.6 parts of zinc oxide to 50 parts of DMF solution and adding 1.6 parts of trimesic acid to mix evenly, then adding dropwise a DMF solution containing 3.8 parts of copper acetate (30 parts in total), the dropping temperature is 60°C, the dropping time is 1h, and after the dropping is completed, the mixture is kept warm for 3.2h, during which time the particle size is sampled and detected; S2: when the particle size reaches the desired range, triethanolamine is added to adjust the pH to 6.9, and the mixture is naturally cooled to room temperature, the product is centrifuged and filtered, and vacuum dried at 65°C to obtain the obtained product.

[0084] Comparative Example 7

[0085] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average particle size of zinc oxide is 35 nm, and the average particle size of the modified particles is 740 nm.

[0086] Performance Evaluation

[0087] Waterproofness: The display films prepared in the examples and comparative examples were tested for water resistance. The film thickness was 1.2 mm. The sessile drop method was used for the test. The test water volume was 1.5 μL and the test time was 15 s. The water contact angle of the film surface was obtained. The test value was the average of 10 tests and recorded in Table 1.

[0088] High temperature stability: The display films prepared in the examples and comparative examples were tested for high temperature stability. The film thickness was 1.2 mm. The display films were placed in a constant temperature and humidity chamber at 65°C and 75% humidity for 7 days. After 7 days, the display films were taken out and observed to see if there was obvious yellowing, deterioration, or skin damage. If so, it was recorded as unqualified, otherwise it was qualified. 50 samples were tested in each group, and the qualified rate of each group was calculated and recorded in Table 1.

[0089] Mechanical properties: The display films prepared in the embodiments and comparative examples were subjected to mechanical property tests using a universal tensile tester. The test film dimensions were 1.2 mm thick, 1 cm wide, and 1.5 cm long. The test values ​​were the average values ​​of 10 tests and recorded in Table 1.

[0090] Table 1 Performance test results

[0091]

[0092] It can be seen from the data results of the embodiments and comparative examples of the present application and Table 1 that the embodiments 1 and 2 of the present application have obvious performance advantages over comparative examples 1 to 7 in terms of the mechanics / flexibility, waterproofness and high temperature stability of the display film, and give the display film certain photoelectric properties, which are more suitable for the manufacture of existing projection equipment. This is mainly because the modified particles and modified PVB used in embodiments 1 and 2 can form an excellent connection with the PVB resin system, thereby playing an excellent internal connection and barrier role respectively when external forces act and water molecules invade, and the added modified particles can also effectively improve the waterproof performance and high temperature stability of the display film, the modified particles can absorb and store excess water molecules inside, reduce the attraction of internal water molecules to external moisture, and improve the waterproof performance, and the excellent high temperature stability of the modified particles themselves can maintain the internal molecular stability in a high temperature environment, reduce the collision and contact probability between active molecules in a high temperature environment, and thus reduce the occurrence of active reactions, greatly improving stability.

Claims

1. A highly flexible display film, characterized in that: Highly flexible display film, the raw materials include, by weight: 60-80 parts of PVB resin, 1-10 parts of scattering particles, 5-10 parts of modified particles, 1-5 parts of blue light absorber, 1-5 parts of dispersant, 1-5 parts of curing agent, 10-20 parts of plasticizer, and 60-120 parts of organic solvent; The PVB resin is a composition of PVB and modified PVB; the mass ratio of the PVB to the modified PVB is (6-7): (1-1.5); The preparation method of the modified PVB comprises the following steps: S1: dispersing sulfonated carbon nanotubes in deionized water to obtain a sulfonated carbon nanotube dispersion, and dissolving PVA in deionized water to obtain a PVA solution for standby use; S2: maintaining the temperature of the PVA solution at 40-50° C., adding butyraldehyde and stirring for 0.5-1 h, then adding the sulfonated carbon nanotube dispersion and stirring evenly, heating to 60-80° C., keeping the temperature and stirring for 2-3 h, filtering and washing the product after completion, and vacuum drying at 40-50° C. to obtain the product; The mass ratio of the sulfonated carbon nanotubes, PVA and butyraldehyde is (0.4-0.8): (12-16): (6-8); The average particle size of the sulfonated carbon nanotubes is 5 to 20 nm; The scattering particles are at least one of aluminum oxide, zinc oxide, titanium dioxide, zirconium oxide, antimony oxide, and cesium oxide.

2. The highly flexible display film according to claim 1, characterized in that: The mass ratio of the PVB resin, scattering particles and modified particles is (7-8): (0.3-0.5): (0.6-1).

3. The highly flexible display film according to claim 2, characterized in that: The scattering particles are a composition of aluminum oxide and zirconium oxide.

4. The highly flexible display film according to claim 3, characterized in that: The mass ratio of aluminum oxide to zirconium oxide is (5-7):(3-4).

5. The highly flexible display film according to claim 4, characterized in that: The average particle size of the aluminum oxide is 100-150 nm.

6. The highly flexible display film according to claim 5, characterized in that: The average particle size of the zirconium oxide is 800-1400 nm.

7. The highly flexible display film according to claim 6, characterized in that: Preparation method of the modified particles The following steps are involved: S1: Mix zinc oxide, sodium dodecyl sulfate, silane coupling agent and succinic anhydride in deionized water, heat to 40-60°C and stir for 3-4 hours to obtain pretreated zinc oxide; S2: Add the pretreated zinc oxide to the DMF solution and add trimesic acid to mix evenly, then drop the DMF solution containing copper acetate in a temperature of 60-65°C for 1-1.5 hours. After the dropwise addition is completed, keep warm for 2-4 hours, during which time take samples to detect the particle size; S3: When the particle size reaches the desired range, add triethanolamine to adjust the pH to 6.8-7.2, naturally cool to room temperature, centrifuge and filter the product, and vacuum dry it at 60-70°C to obtain the product.

8. The highly flexible display film according to claim 7, characterized in that: The average particle size of the modified particles is 500-600 nm; the mass ratio of the pretreated zinc oxide, trimesic acid and copper acetate is (0.8-1): (1.5-1.8): (3.5-4).

9. A method for preparing a highly flexible display film according to any one of claims 1 to 8, characterized in that: S1: Add PVB resin to an organic solvent and stir evenly to obtain a resin base liquid for use; S2: Mix the scattering particles and modified particles evenly, mix them with a plasticizer, add them to the resin base liquid, heat it to 50-60°C, add a blue light absorber, a dispersant and a curing agent in sequence, stir evenly in a high-speed stirrer to obtain a pre-product; S3: Dehydrate the pre-product, extrude it into a film, heat it at 60-65°C until it is completely cured into a film, and obtain the product.

10. Use of the highly flexible display film according to any one of claims 1 to 8 in preparing an electronic display film device.