High-performance self-lubricating sliding block material and preparation method thereof

By using high-performance self-lubricating slider materials composed of nylon 6, alkali-free glass fiber micro powder, silica micro powder, polytetrafluoroethylene micro powder and silane coupling agent, the nylon slider needs to be regularly applied to grease in the prior art. Problem, oil-free lubrication and low friction coefficient are achieved, and are suitable for engineering machinery and other fields.

CN119039776APending Publication Date: 2024-11-29SHANGHAI JIAOTONG (XUZHOU) NEW MATERIAL RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180281.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Nylon sliders in existing construction machinery need to be regularly applied to reduce friction, but this leads to high maintenance costs, easy dirt and affects the stability of the equipment's operation.

Method used

Using high-performance self-lubricating slider material composed of nylon 6, alkali-free glass fiber micro powder, silica micro powder, polytetrafluoroethylene micro powder and silane coupling agent, it is used to dry, mix, twin screw extrusion and injection molding processes. Form a composite material with high strength and low friction coefficient to achieve oil-free lubrication.

Benefits of technology

It realizes oil-free lubrication without regular grease application, reduces maintenance costs, and improves the mechanical properties and wear resistance of the slider. The dynamic friction coefficient is less than 0.14, and is suitable for engineering machinery and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039776A_ABST
    Figure CN119039776A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of materials, and particularly relates to a high-performance self-lubricating sliding block material and a preparation method thereof, and the sliding block material is mainly prepared from the following raw materials in parts by weight: 1000 parts of nylon 6, 100-200 parts of alkali-free glass fiber micro powder, 2-10 parts of silicon dioxide micro powder, 10-50 parts of polytetrafluoroethylene micro powder and 0.5-2 parts of a silane coupling agent. The sliding block material is high in strength, low in friction coefficient and large in working temperature range, oil-free lubrication can be achieved, regular grease smearing is not needed, the equipment use requirement is met, and the maintenance cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of materials, and in particular relates to a high-performance self-lubricating sliding block material and a preparation method thereof. Background Art

[0002] With the pursuit of lightweight and high-performance materials, polymer-based composite materials have been widely used in many fields. However, improving the comprehensive performance of the polymer matrix remains a major challenge. Among them, the slider made of polymer-based composite materials is a key component that plays a role in bearing weight and ensuring smoothness during the telescopic movement of the cantilever arm of construction machinery such as cranes.

[0003] At present, most of the domestic engineering machinery industry uses nylon sliders. In order to reduce the friction between the nylon slider and the crane boom or other rigid structural parts to avoid scratching the boom, it is usually necessary to open an oil groove on the ordinary slider and apply grease regularly, which is time-consuming and labor-intensive, and the maintenance cost is extremely high. At the same time, the grease makes the boom easy to be contaminated with dirt, causing jitter and poor operation during the telescopic movement of the boom. Therefore, it is urgent to develop a high-performance self-lubricating slider with high toughness and wear resistance to achieve oil-free lubrication, without the need for regular grease application, meet the equipment use requirements, and reduce maintenance costs. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a high-performance self-lubricating slider material and a preparation method thereof. The slider material has high strength, low friction coefficient, and a wide operating temperature range. It can achieve oil-free lubrication and does not require regular application of grease, thus meeting equipment use requirements and reducing maintenance costs.

[0005] The technical solution provided by the present invention is as follows: The present invention provides a high-performance self-lubricating slider material, characterized in that the slider material is mainly composed of the following raw materials in parts by weight: Nylon 6: 1000 parts, alkali-free glass fiber powder: 100-200 parts, silicon dioxide powder: 2-10 parts, polytetrafluoroethylene powder: 10-50 parts, silane coupling agent: 0.5-2 parts.

[0006] Furthermore, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0007] Furthermore, the alkali-free glass fiber powder is a filling and reinforcing material obtained by chopping, grinding and screening alkali-free glass fiber raw fibers produced by a pool kiln drawing method.

[0008] The present invention also provides a method for preparing the high-performance self-lubricating slider material according to the above, comprising the following steps: Putting nylon 6 powder, alkali-free glass fiber powder, silicon dioxide powder and polytetrafluoroethylene powder into a drying oven and drying them at 80-90° C. to obtain dried nylon 6 powder, dried alkali-free glass fiber powder, dried silicon dioxide powder and dried polytetrafluoroethylene powder; Put the dried nylon 6 powder, the dried alkali-free glass fiber powder, the dried silica powder, the dried polytetrafluoroethylene powder and the silane coupling agent into a V-type mixer, mix them evenly and then take them out to obtain a composite; The composite material is added into a twin-screw extruder, extruded after melt blending, water-cooled, and pelletized by a pelletizer to obtain composite material pellets; The prepared particles are dried, injection molded by an injection molding machine, and cooled at room temperature to obtain a high-performance self-lubricating slider material.

[0009] Furthermore, the main engine speed of the twin-screw extruder is 100-120 rpm / min, and the feeding speed is 8-10 rpm / min.

[0010] Furthermore, the twin screw extruder is provided with 10 temperature zones, the temperature of the first zone is 190-205°C, the temperature of the second zone is 205-220°C, the temperature of the third zone is 225-235°C, the temperature of the fourth zone is 235-245°C, the temperature of the fifth to ninth zones is 235-245°C, and the temperature of the die head and melt zone is 240-245°C.

[0011] Furthermore, the screw speed of the injection molding machine is 55-70 rpm / min.

[0012] Furthermore, the injection molding machine is provided with 5 injection molding sections, the temperature of the first section is 245-255°C, the temperature of the second to fifth sections is 245-255°C, and the temperature of the nozzle section is 255-270°C.

[0013] Furthermore, the injection pressure is 75~90 MPa, the holding pressure is 15~25 MPa, and the holding time is 3~6 s.

[0014] Furthermore, post-processing steps are also included: The injection molded high-performance self-lubricating slider material is subjected to constant temperature post-treatment in a water bath at 75-85°C or an oil bath at 115-125°C for 12-24 hours.

[0015] Beneficial Effects

[0016] (1) The present invention uses alkali-free glass fiber powder and silica powder to reinforce the PA6 substrate and improve its mechanical properties and wear resistance, and uses a single solid lubricant (polytetrafluoroethylene) to further improve the tribological properties of the composite material. At the same time, an organic-inorganic hybrid network is constructed by introducing a cross-linking agent (silane coupling agent), thereby achieving a significant improvement in the performance of high-performance self-lubricating slider materials, such as a tensile strength of 71 MPa, a bending strength of more than 88 MPa, and a dynamic friction coefficient of less than 0.14. It has the advantages of high strength, low friction coefficient, and a wide operating temperature range, and its comprehensive performance has reached the international leading level.

[0017] (2) The present invention can be widely used in engineering machinery, automobiles, conveyor production lines and other fields, and plays a role in bearing weight and ensuring smoothness in key sliding parts. The slider of the present invention has been verified and used on the telescopic boom of a crane, and can achieve oil-free lubrication without the need for regular grease application, meeting the equipment use requirements and reducing maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a processing flow chart of the high-performance self-lubricating slider material of the present invention.

[0019] Figure 2 is a photograph of the modified granules after drying of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The embodiment of the present invention provides a high-performance self-lubricating slider material, characterized in that the slider material is mainly composed of the following raw materials in parts by weight: Nylon 6: 1000 parts, alkali-free glass fiber powder: 100-200 parts, silicon dioxide powder: 2-10 parts, polytetrafluoroethylene powder: 10-50 parts, silane coupling agent: 0.5-2 parts.

[0022] In this embodiment, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0023] In this embodiment, the alkali-free glass fiber powder is a filling and reinforcing material obtained by chopping, grinding and screening the alkali-free glass fiber raw filaments produced by a pool kiln wire drawing method.

[0024] The embodiment of the present invention further provides a method for preparing the high-performance self-lubricating slider material according to the above, comprising the following steps: Putting nylon 6 powder, alkali-free glass fiber powder, silicon dioxide powder and polytetrafluoroethylene powder into a drying oven and drying them at 80-90° C. to obtain dried nylon 6 powder, dried alkali-free glass fiber powder, dried silicon dioxide powder and dried polytetrafluoroethylene powder; Put the dried nylon 6 powder, the dried alkali-free glass fiber powder, the dried silica powder, the dried polytetrafluoroethylene powder and the silane coupling agent into a V-type mixer, mix them evenly and then take them out to obtain a composite; The composite material is added into a twin-screw extruder, extruded after melt blending, water-cooled, and pelletized by a pelletizer to obtain composite material pellets; The prepared particles are dried, injection molded by an injection molding machine, and cooled at room temperature to obtain a high-performance self-lubricating slider material.

[0025] In this embodiment, the main engine speed of the twin-screw extruder is 100-120 rpm / min, and the feeding speed is 8-10 rpm / min.

[0026] In this embodiment, the twin screw extruder is provided with 10 temperature zones, the temperature of the first zone is 190-205°C, the temperature of the second zone is 205-220°C, the temperature of the third zone is 225-235°C, the temperature of the fourth zone is 235-245°C, the temperature of the fifth to ninth zones is 235-245°C, and the temperature of the die head and melt zone is 240-245°C.

[0027] In this embodiment, the screw speed of the injection molding machine is 55-70 rpm / min.

[0028] In this embodiment, the injection molding machine is provided with 5 injection molding sections, the temperature of the first section is 245-255°C, the temperature of the second to fifth sections is 245-255°C, and the temperature of the nozzle section is 255-270°C.

[0029] In this embodiment, the injection pressure is 75-90 MPa, the holding pressure is 15-25 MPa, and the holding time is 3-6 s.

[0030] In this embodiment, a post-processing step is also included: The injection molded high-performance self-lubricating slider material is subjected to constant temperature post-treatment in a water bath at 75-85°C or an oil bath at 115-125°C for 12-24 hours.

[0031] The following is a detailed description of a high-performance self-lubricating slider material and a preparation method thereof provided by the present invention in conjunction with the embodiments (eg Figure 1 and Figure 2 ), but they should not be understood as limiting the scope of protection of the present invention.

[0032] Example 1

[0033] 1000 parts of PA6 after drying, 100 parts of alkali-free glass fiber powder, 10 parts of polytetrafluoroethylene powder, 2 parts of silica powder and 0.5 parts of silane coupling agent were added into a mixer and mixed thoroughly. Then the mixed materials were added into a twin-screw extruder. The main engine speed of the twin-screw extruder was 100 rpm / min and the feeding speed was 8 rpm / min; each heating section is set according to the following conditions: 190℃ for the first zone, 205℃ for the second zone, 225℃ for the third zone, 235℃ for the fourth zone, 240℃ for the fifth to ninth zones, and 240℃ for the die and melt zone; after melt extrusion, water cooling and granulation are carried out, and modified pellets are obtained after drying; about the temperature of the extrusion section, it should be noted that: since the heating section is continuous, there is no middle temperature higher than the two sides, and its temperature must be guaranteed to increase gradually; when the temperature is low, the melting of the multi-component modified material is not good and agglomeration is easy to occur; when the temperature is too high, bubbling will occur, the wire is easy to break, and it is difficult to effectively cool and granulate; the temperature of the die and melt must ensure that the mixed material can be extruded and granulated; the feeding speed should match the pelletizing speed.

[0034] A certain amount of dried modified pellets was added to the feed port of the injection molding machine and set according to the following conditions: the screw speed of the injection molding machine was 60 rpm / min; the first section of the heating part of the injection molding machine was 245℃, the second to fifth sections were 250℃, and the temperature of the nozzle section was 255℃; the injection pressure was 80 MPa, the holding pressure was 20 MPa, and the holding time was 4 s. Regarding the temperature of the injection section, it should be noted that the pressure during injection molding was adjusted according to the feed speed and mold conditions. Subsequently, the high-performance self-lubricating slider material after injection molding was subjected to temperature post-treatment in an 80℃ water bath for 18 hours.

[0035] Example 2

[0036] 1000 parts of PA6, 130 parts of alkali-free glass fiber powder, 30 parts of polytetrafluoroethylene powder, 4 parts of silica powder and 1 part of silane coupling agent after drying were added into a mixer and mixed thoroughly. Then the mixed materials were added into a twin-screw extruder. The main engine speed of the twin-screw extruder was 100 rpm / min, and the feeding speed was 8 rpm / min. Each heating section was set according to the following conditions: 200°C for the first zone, 215°C for the second zone, 235°C for the third zone, 240°C for the fourth zone, 240°C for the fifth to ninth zones, and 240°C for the die and melt zone. After melt extrusion, water cooling and granulation were performed, and modified granules were obtained after drying. Attention should be paid to the temperature of the extrusion section: since the heating section is continuous, there is no middle temperature higher than the two sides. When the temperature is low, the melting of the multi-modified material is poor and agglomeration is easy to occur. When the temperature is too high, bubbling will occur, the wire will break easily, and it is difficult to effectively cool and granulate.

[0037] Add a certain amount of dried modified pellets into the injection molding machine feed port (drying conditions are as follows Figure 2 As shown in the figure, the following conditions are set: the screw speed of the injection molding machine is 60 rpm / min; the first section of the heating part of the injection molding machine is 255℃, the second to fifth sections are 250℃, and the temperature of the nozzle section is 260℃; the injection pressure is 85MPa, the holding pressure is 20MPa, and the holding time is 4s. Regarding the temperature of the injection section, it should be noted that the pressure during injection molding is adjusted according to the feed speed and mold conditions. Subsequently, the high-performance self-lubricating slider material after injection molding is subjected to temperature post-treatment in an 80℃ water bath for 18 hours.

[0038] Example 3

[0039] 1000 parts of PA6, 200 parts of alkali-free glass fiber powder, 50 parts of polytetrafluoroethylene powder, 10 parts of silica powder and 2 parts of silane coupling agent after drying were added into a mixer and mixed thoroughly. Then the mixed materials were added into a twin-screw extruder. The main engine speed of the twin-screw extruder was 100 rpm / min and the feeding speed was 8 rpm / min. Each heating section was set according to the following conditions: 190°C for the first zone, 205°C for the second zone, 225°C for the third zone, 235°C for the fourth zone, 240°C for the fifth to ninth zones, and 240°C for the die and melt zone. After melt extrusion, water cooling and granulation were performed, and modified granules were obtained after drying. Attention should be paid to the temperature of the extrusion section: since the heating section is continuous, there is no middle temperature higher than the two sides. When the temperature is low, the melting of the multi-modified material is poor and agglomeration is easy to occur. When the temperature is too high, bubbling will occur, the wire will break easily, and it is difficult to effectively cool and granulate.

[0040] A certain amount of dried modified pellets was added to the feed port of the injection molding machine and set according to the following conditions: the screw speed of the injection molding machine was 60 rpm / min; the first section of the heating part of the injection molding machine was 245℃, the second to fifth sections were 250℃, and the temperature of the nozzle section was 255℃; the injection pressure was 80 MPa, the holding pressure was 20 MPa, and the holding time was 4 s. Regarding the temperature of the injection section, it should be noted that the pressure during injection molding was adjusted according to the feed speed and mold conditions. Subsequently, the high-performance self-lubricating slider material after injection molding was subjected to temperature post-treatment in an 80℃ water bath for 18 h.

[0041] The performance of the slider materials prepared in Examples 1-3 was tested according to national standards, and the test results are shown in Table 1.

[0042] Table 1 Performance of high-performance self-lubricating slider

[0043]

[0044] It can be seen from the above table:

[0045] 1) Based on the characteristics of a single modified material, alkali-free glass fiber transfers the load to the adjacent matrix by transmitting and dispersing the load, greatly increasing the amount of material bearing the load; this reduces the plowing effect of the dual-surface micro-convexities on the PA6 matrix, thereby improving the friction and wear properties of the material. In terms of the content of alkali-free glass fiber: when its content is 100-200 parts, the interface between the fiber and the matrix is ​​better, and the fiber effectively bears the load in the matrix. However, when its content is greater than 200 parts, the dispersion of the fiber in the matrix becomes worse, it is easy to be exposed, and it is easy to break and shatter without the protection of the matrix. These exposed fibers act as abrasive particles on the friction surface, resulting in an increase in the friction coefficient. Therefore, the amount of alkali-free glass fiber powder added should be appropriate.

[0046] Silica nanoparticles fall off from the surface of the composite material during the alternating stress process. These extremely small nanoparticles produce a rolling effect, thereby reducing the friction coefficient. In addition, the nanoparticles can be embedded in the grooves of the dual surface and the friction surface, promoting the formation of the transfer film and exerting a mechanical riveting effect on the transfer film, causing friction to occur between the polymer composite body and the composite transfer film, thereby reducing the friction coefficient. However, when the nanoparticle content exceeds a certain threshold (10 parts), the nanoparticles tend to agglomerate in the matrix, destroying the continuity of the matrix PA6, thereby increasing the friction coefficient.

[0047] Polytetrafluoroethylene (PTFE) is a solid lubricant with an extremely low friction coefficient (0.02). It can form a lubricating film on the wear surface and quickly form a transfer film on the mating surface, which causes friction to occur between the polymer transfer film and the polymer, thereby reducing the friction coefficient. Under the premise of ensuring good dispersion of PTFE, as its content increases, the more complete the transfer film formed, the more beneficial it is to reducing the friction coefficient.

[0048] 2) Comprehensively consider the possible synergistic effects among multiple modified materials:

[0049] aPTFE and glass fiber have a synergistic effect in reducing the friction and wear of PA6. Because glass fiber is coarse and the particle size of PTFE is small, a structure with complementary size and function is formed, which helps to improve the tribological properties of the composite material. In addition, PTFE helps to quickly form a transfer film, while glass fiber improves the composite material's ability to resist deformation and strengthens the adhesion strength between the transfer film and the mating surface. Therefore, PTFE further reduces the friction coefficient of the PA6 / glass fiber composite material.

[0050] b. PTFE and silica have a synergistic effect in improving the tribological properties of PA6, and the presence of silane coupling agent further enhances this effect. ① First, due to its high surface activity, silica particles are preferentially filled in the grooves of the dual surface, which is conducive to the rapid formation of a continuous and uniform transfer film by PTFE. ② Secondly, the friction coefficient of PTFE itself is extremely low, and the molecular layers can easily slide to form a transfer film and a surface lubricating film, which plays a role of solid lubrication, which makes the friction occur between polymers, thereby reducing the friction coefficient and wear; ③ In addition, the silane coupling agent and PTFE jointly improve the compatibility of inorganic phase silica and organic phase PA6, and enhance the dispersion of silica in the matrix; ④ Finally, PTFE is easier to migrate to the surface than PA6, and the lubricating film formed on the wear surface is "pinned" to the PA6 surface by silica. At this time, PTFE plays a lubricating role, and silica acts as a stress support point to prevent the metal peaks from penetrating into the surface layer and reduce the deformation of the matrix.

Claims

1. A high-performance self-lubricating slider material, characterized in that: The slider material is mainly composed of the following raw materials in parts by weight: Nylon 6: 1000 parts, alkali-free glass fiber powder: 100-200 parts, silica powder: 2-10 parts, polytetrafluoroethylene powder: 10-50 parts, silane coupling agent: 0.5-2 parts.

2. The high-performance self-lubricating slider material according to claim 1, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane.

3. The high-performance self-lubricating slider material according to claim 1, characterized in that: The alkali-free glass fiber powder is a filling and reinforcing material obtained by chopping, grinding and screening the alkali-free glass fiber raw filaments produced by a pool kiln wire drawing method.

4. A method for preparing a high-performance self-lubricating slider material according to claim 1, characterized in that: The following steps are involved: Putting nylon 6 powder, alkali-free glass fiber powder, silicon dioxide powder and polytetrafluoroethylene powder into a drying oven and drying them at 80-90° C. to obtain dried nylon 6 powder, dried alkali-free glass fiber powder, dried silicon dioxide powder and dried polytetrafluoroethylene powder; Put the dried nylon 6 powder, the dried alkali-free glass fiber powder, the dried silica powder, the dried polytetrafluoroethylene powder and the silane coupling agent into a V-type mixer, mix them evenly and then take them out to obtain a composite; The composite material is added into a twin-screw extruder, extruded after melt blending, water-cooled, and pelletized by a pelletizer to obtain composite material pellets; The prepared particles are dried, injection molded by an injection molding machine, and cooled at room temperature to obtain a high-performance self-lubricating slider material.

5. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: The main engine speed of the twin-screw extruder is 100-120 rpm / min, and the feeding speed is 8-10 rpm / min.

6. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: The twin-screw extruder is provided with 10 temperature zones in total, the temperature of the first zone is 190-205°C, the temperature of the second zone is 205-220°C, the temperature of the third zone is 225-235°C, the temperature of the fourth zone is 235-245°C, the temperature of the fifth to ninth zones is 235-245°C, and the temperature of the die and melt zone is 240-245°C.

7. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: The screw speed of the injection molding machine is 55-70 rpm / min.

8. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: The injection molding machine is provided with 5 injection molding sections in total, the temperature of the first section is 245-255°C, the temperature of the second to fifth sections is 245-255°C, and the temperature of the nozzle section is 255-270°C.

9. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: The injection pressure is 75~90 MPa, the holding pressure is 15~25 MPa, and the holding time is 3~6 s.

10. The method for preparing a high-performance self-lubricating slider material according to claim 4, characterized in that: Post-processing steps are also included: The injection molded high-performance self-lubricating slider material is subjected to constant temperature post-treatment in a water bath at 75-85°C or an oil bath at 115-125°C for 12-24 hours.