Uvioresistant high-flame-retardant carbon black-based pigment for papermaking and preparation process thereof
By mixing carbon black powder, oxide gel and modified hydrotalcite powder, a carbon black-based pigment for papermaking with high UV resistance and flame retardancy was prepared. This solved the problems of carbon black dispersibility and modification cost in water-based pulp, and achieved improved dispersibility, UV resistance and flame retardancy.
Patent Information
- Application Number
- CN202411145735.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-18
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
Existing carbon black is difficult to disperse in water-based pulp, and traditional modification methods lead to a decrease in tensile strength and toughness, making it difficult to achieve high load-bearing capacity and high elongation at break. At the same time, its UV resistance and flame retardant effects are generally poor, and its production cost is high.
A carbon black-based pigment for papermaking with UV resistance and high flame retardancy was formed by using a mixture of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:(1-2):(5-8), adding an adhesive, and through nano-pulverization, mixed solution preparation and vacuum drying processes.
It improves the dispersibility and hydrophilicity of carbon black in water-based pulp, enhances the paper's UV resistance and flame retardancy, and reduces production costs.
Smart Images

Figure BDA0005002135130000081 
Figure BDA0005002135130000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon black-based pigments, and in particular to an ultraviolet-resistant and highly flame-retardant carbon black-based pigment for papermaking and a preparation process thereof. Background Art
[0002] Carbon black is used in the papermaking industry as a black pigment to produce black, gray, or dark paper and cardboard. Compared with other organic pigments, carbon black is relatively cheap, has good light resistance and chemical resistance, and has good coloring and light-shielding properties. It can also make paper conductive. Therefore, paper colored with carbon black is often used for decorative materials, light-proof packaging materials (such as packaging paper for photosensitive films), various atlas papers, high-voltage cable papers, etc.; the particle size of ordinary pigment carbon black is only 8-100 nanometers, the particle surface energy is high, it is easy to self-aggregate, and it is difficult to wet. It is the most difficult variety to disperse among pigments. Carbon black is lipophilic and hydrophobic, and it is difficult to stably disperse carbon black in an aqueous system. If powdered or granular carbon black is used directly for papermaking, it is difficult to mix and disperse in aqueous pulp because the commonly used carbon black is hydrophobic, and it is easy to pollute equipment and the environment. Therefore, it is necessary to post-treat the carbon black powder to meet the use requirements of carbon black in aqueous pulp.
[0003] Carbon black produced under traditional processes are all hydrophobic and oleophilic products and cannot be directly used for color matching of papermaking or other products in aqueous environments. To solve the problem of carbon black application, a common method is to modify traditional carbon black to prepare hydrophilic carbon black products. At present, there are many studies on the hydrophilic modification of carbon black at home and abroad, mainly focusing on two major directions. One is to increase the surface hydrophilic groups of carbon black by strong oxidation and other methods to improve the hydrophilicity of carbon black; the other is to add a large amount of carbon black dispersant, wetting agent, ionic surfactant, defoaming agent and other raw materials in an aqueous environment, prepare it into carbon black slurry through a grinding process, and then obtain hydrophilic carbon black through drying, crushing, grinding and other processes.
[0004] However, both of the above methods have the disadvantages of single carbon black raw material, and the produced carbon black has general anti-ultraviolet effect and poor flame retardant effect, and at the same time greatly increases the raw material and production costs of hydrophilic carbon black. Summary of the invention
[0005] The purpose of the present invention is to provide a carbon black-based pigment for papermaking with high UV resistance and flame retardancy and a preparation process thereof; to solve the following technical problems:
[0006] The existing technology generally achieves this by adding fibers, solid lubricants and other special nano-functional fillers. However, after filling with the above fillers, the tensile strength and toughness are reduced, and it is difficult to achieve high load-bearing capacity and high elongation at break.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A UV-resistant and highly flame-retardant carbon black-based pigment for papermaking, comprising a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:(1-2):(5-8), and an adhesive, wherein the mass ratio of the mixed powder to the adhesive is 100:(2-4);
[0009] The components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:(1-2):(3-5):(10-15); the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of (10-20):(1-3):(2-5).
[0010] In a further embodiment of the present invention, the components of the carbon black-based pigment include a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:(1.2-1.8):(6-7), and also include an adhesive, and the mass ratio of the mixed powder to the adhesive is 100:(2.5-3.5);
[0011] Among them, the components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:(1.2-1.8):(3.5-4.5):(11-14); the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of (12-18):(1.5-2.5):(3-4).
[0012] In a further embodiment of the present invention: the components of the carbon black-based pigment include a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:1.5:6.5, and also include an adhesive, and the mass ratio of the mixed powder to the adhesive is 100:3;
[0013] Among them, the components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:1.5:4:13; the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of 15:2:3.5.
[0014] In a further embodiment of the present invention, the coupling agent is selected from at least one of bis-tetrasulfide, vinyltriethoxysilane and vinyltrimethoxysilane.
[0015] In a further embodiment of the present invention, the modifier includes dimethyl sulfoxide, toluene diisocyanate and dibutyl tin dilaurate.
[0016] In a further embodiment of the present invention, the adhesive is pinene alcohol.
[0017] A process for preparing the above-mentioned ultraviolet resistant and highly flame-retardant carbon black-based pigment for papermaking comprises the following steps:
[0018] (1) Preparing carbon black powder: subjecting carbon black material to nano-crushing treatment to obtain carbon black powder;
[0019] (2) preparing oxide gel; using deionized water as solvent, adding Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol according to the mass ratio to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80° C. for 2-4 hours to obtain a transparent sol;
[0020] (3) preparing modified hydrotalcite powder: grinding the hydrotalcite into powder, adding the coupling agent and the modifier into a reaction kettle according to the mass ratio, sealing, evacuating and filling with nitrogen, and then stirring with a magnetic force for 6-8 hours, and vacuum drying to obtain the modified hydrotalcite powder;
[0021] (4) Preparation of carbon black-based pigment: Add carbon black powder, oxide gel and modified hydrotalcite powder into a reactor according to the mass ratio, mix them evenly, then add adhesive and continue to stir evenly to finally obtain carbon black-based pigment.
[0022] In a further embodiment of the present invention: in step (1), the particle size of the carbon black powder is less than 1500 mesh.
[0023] In a further embodiment of the present invention: in step (4), the temperature of the reactor is 60-120° C., and the stirring time is 3-6 hours.
[0024] Beneficial effects of the present invention:
[0025] (1) The hydrotalcite material used in the present invention is an anionic layered compound. After modification, the azo groups on the surface of the hydrotalcite are introduced to form a reactive hydrotalcite containing azo groups. Then, by adding an adhesive and carrying out a grafting reaction with nano carbon black, the dispersibility between nano carbon black particles can be improved, and the hydrophilicity of the nano carbon black can also be improved.
[0026] (2) The carbon black aggregates in the process of the present invention have an open structure, and the carbon black itself is also a porous substance. Iron and cerium are introduced into the carbon black voids in the form of gel. Since the ultrafine cerium oxide has strong ultraviolet absorption properties and iron oxide is also an excellent black pigment, the system can be combined with nano carbon black to enhance the ultraviolet absorption effect and enhance the coloring strength of the carbon black.
[0027] (3) In the process of the present invention, since both hydrotalcite and composite oxide gel have extremely strong flame retardant properties, during the process of dyeing the pulp, an anti-oxidative flame retardant layer can be formed on the surface of the pulp, thereby enhancing the flame retardant effect of papermaking. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0031] S2: preparing oxide gel; using deionized water as solvent, adding 1g Ce(NO3)3, 1g Fe(NO3)3, 3g citric acid and 10g polyethylene glycol to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80°C for 2h to obtain a stable, uniform, clear and transparent sol;
[0032] S3: Preparation of modified hydrotalcite powder: Grind the hydrotalcite obtained by microwave crystallization into powder less than 10 μm and take 10 g, then take 1 g of 3-triethoxysilylpropyl and 2 g of dimethyl sulfoxide and add them into a reaction kettle, seal and evacuate and fill with nitrogen, then stir with magnetic force for 7 hours, and vacuum dry to obtain modified hydrotalcite powder;
[0033] S4: Preparation of carbon black-based pigment: 100 g of carbon black powder, 5 g of oxide gel and 1 g of modified hydrotalcite powder were added into a reactor, mixed evenly, and then 2 g of pinene alcohol was added. Stirring was continued at 60°C for 3 h to fully wet the carbon black powder, and finally a carbon black-based pigment was obtained.
[0034] Example 2
[0035] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0036] S2: preparing oxide gel; using deionized water as solvent, adding 1g Ce(NO3)3, 1.5g Fe(NO3)3, 4g citric acid and 12g polyethylene glycol to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80°C for 3h to obtain a stable, uniform, clear and transparent sol;
[0037] S3: Preparation of modified hydrotalcite powder: Grind the hydrotalcite obtained by microwave crystallization into powder less than 10 μm and take 12 g, then add 2 g of 3-triethoxysilylpropyl and 3 g of toluene diisocyanate into a reaction kettle, seal and evacuate, fill with nitrogen, and then stir with magnetic force for 7 h, and vacuum dry to obtain modified hydrotalcite powder;
[0038] S4: Preparation of carbon black-based pigment: 100 g of carbon black powder, 6 g of oxide gel and 1.5 g of modified hydrotalcite powder were added into a reactor, mixed evenly, and then 3 g of pine oil was added. Stirring was continued at 80°C for 4 h to fully wet the carbon black powder, and finally a carbon black-based pigment was obtained.
[0039] Example 3
[0040] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0041] S2: preparing oxide gel; using deionized water as solvent, adding 1g Ce(NO3)3, 2g Fe(NO3)3, 5g citric acid and 15g polyethylene glycol to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80°C for 4h to obtain a stable, uniform, clear and transparent sol;
[0042] S3: Preparation of modified hydrotalcite powder: Grind the hydrotalcite obtained by microwave crystallization into a powder less than 10 μm and take 16 g, then add 3 g of 3-triethoxysilylpropyl and 4 g of dibutyltin dilaurate into a reaction kettle, seal and evacuate, fill with nitrogen, and then stir with magnetic force for 7 hours, and vacuum dry to obtain modified hydrotalcite powder;
[0043] S4: Preparation of carbon black-based pigment: 100 g of carbon black powder, 7 g of oxide gel and 1.5 g of modified hydrotalcite powder were added into a reactor, mixed evenly, and then 4 g of pine oil was added. Stirring was continued at 100°C for 5 h to fully wet the carbon black powder, and finally a carbon black-based pigment was obtained.
[0044] Example 4
[0045] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0046] S2: preparing oxide gel; using deionized water as solvent, adding 1g Ce(NO3)3, 2g Fe(NO3)3, 5g citric acid and 15g polyethylene glycol to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80°C for 4h to obtain a stable, uniform, clear and transparent sol;
[0047] S3: Preparation of modified hydrotalcite powder: Grind the hydrotalcite obtained by microwave crystallization into a powder less than 10 μm and take 20 g, then add 1.5 g of 3-triethoxysilylpropyl, 1.5 g of vinyl triethoxyethane and 4 g of dibutyltin laurate into a reaction kettle, seal and evacuate, fill with nitrogen, and then stir with magnetic force for 7 h, and vacuum dry to obtain modified hydrotalcite powder;
[0048] S4: Preparation of carbon black-based pigment: 100 g of carbon black powder, 8 g of oxide gel and 2 g of modified hydrotalcite powder were added into a reactor, mixed evenly, and then 4 g of pine oil was added. Stirring was continued at 120°C for 6 h to fully wet the carbon black powder, and finally a carbon black-based pigment was obtained.
[0049] Comparative Example 1
[0050] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh.
[0051] Comparative Example 2
[0052] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0053] S2: preparing oxide gel; using deionized water as solvent, adding 1g Ce(NO3)3, 1g Fe(NO3)3, 3g citric acid and 10g polyethylene glycol to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80°C for 2h to obtain a stable, uniform, clear and transparent sol;
[0054] S3: Preparation of carbon black-based pigment: 100 g of carbon black powder, 5 g of oxide gel and 1 g of modified hydrotalcite were added into a reactor, mixed evenly, and then 2 g of pinene alcohol was added. Stirring was continued at 60°C for 3 h to fully wet the carbon black powder, and finally a carbon black-based pigment was obtained.
[0055] Comparative Example 3
[0056] S1: preparing carbon black powder: subjecting the carbon black material to nano-crushing treatment to obtain carbon black powder with a particle size less than 1500 mesh;
[0057] S2: Preparation of modified hydrotalcite powder: Grind the hydrotalcite obtained by microwave crystallization into powder less than 10 μm and take 10 g, then take 1 g of 3-triethoxysilylpropyl and 2 g of dimethyl sulfoxide and add them into a reaction kettle, seal and evacuate and fill with nitrogen, then stir with magnetic force for 7 h, and vacuum dry to obtain modified hydrotalcite powder;
[0058] S3: Preparation of carbon black-based pigment: 100 g of carbon black powder, 5 g of oxide gel and 1 g of modified hydrotalcite are added into a reactor, mixed evenly, and then 2 g of pinene alcohol is added. Stirring is continued at 80°C for 4 h to fully wet the carbon black powder, and finally a carbon black-based pigment is obtained.
[0059] Experimental results test
[0060] The properties of the carbon black-based pigments obtained in Examples 1-4 and Comparative Examples 1-3 were tested, and the test items and methods were as follows:
[0061] According to GB / T 7048, the blackness L value of carbon black is tested, and GB / T 10772, the BET specific surface area (m 2 / g), GB / T 3780.2 tests the DBP absorption value of carbon black (cc / 100g), GB / T 3780.7 tests the acidity and pH value of carbon black, GB / T 3780.6 tests the relative tinting strength of carbon black (ITRB=100%), GB / T 3780.8 tests the heating loss of carbon black, GB / T3780.21 tests the sieve residue of carbon black (325 mesh), GB / T 7047 tests the volatile matter of carbon black (950℃), GB / T3780.12 tests the impurities of carbon black, and GB / T 34323 tests the transmittance of carbon black aqueous dispersion.
[0062] According to the Chinese standard GB / T 14656-93 "Test Method for Flame Retardant Paper and Paperboard Combustion", the paper product is vertically hung on the sample rack. Under the specified conditions, the sample is exposed to the flame, and its flame retardant performance is tested based on the burn length, afterburn time, and smoldering time. This method is suitable for paper products with a thickness of less than 1.6mm, a sample size of 21cm*7cm, ignition for 12s, and the afterglow time and carbonization length of the sample are measured.
[0063] The test results are listed in the following Tables 1 and 2, wherein Table 1 is a material performance test table, and Table 2 is a flame retardant effect test table.
[0064] Table 1
[0065]
[0066]
[0067] Table 2
[0068] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Length (cm) 17.6 18.4 17.6 17.3 2.3 8.5 11.5
[0069] By analyzing the data in Table 1 and Table 2, it can be seen that the carbon black-based pigments prepared in Examples 1-4 are darker and have stronger coloring ability, higher specific surface area, and less screen residue after dyeing than those in Comparative Examples 1-3. At the same time, they have a certain flame retardant effect and can increase the anti-burning effect of paper.
[0070] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A UV-resistant and highly flame-retardant carbon black-based pigment for papermaking, characterized in that: The components include a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:(1-2):(5-8), and also include an adhesive, and the mass ratio of the mixed powder to the adhesive is 100:(2-4); The components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:(1-2):(3-5):(10-15); the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of (10-20):(1-3):(2-5).
2. The ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to claim 1, characterized in that: The components include a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:(1.2-1.8):(6-7), and also include an adhesive, and the mass ratio of the mixed powder to the adhesive is 100:(2.5-3.5); Among them, the components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:(1.2-1.8):(3.5-4.5):(11-14); the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of (12-18):(1.5-2.5):(3-4).
3. The ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to claim 2, characterized in that: The components include a mixed powder of carbon black powder, oxide gel and modified hydrotalcite powder in a mass ratio of 100:1.5:6.5, and also include an adhesive, and the mass ratio of the mixed powder to the adhesive is 100:3; Among them, the components of the oxide gel include Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol in a mass ratio of 1:1.5:4:13; the components of the modified hydrotalcite powder include hydrotalcite, coupling agent and modifier in a mass ratio of 15:2:3.
5.
4. The ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to any one of claims 1 to 3, characterized in that: The coupling agent is selected from at least one of bistetrasulfide, vinyltriethoxysilane and vinyltrimethoxysilane.
5. The ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to any one of claims 1 to 3, characterized in that: The modifiers include dimethyl sulfoxide, toluene diisocyanate and dibutyltin dilaurate.
6. The ultraviolet resistant and highly flame retardant carbon black based pigment for papermaking according to any one of claims 1 to 3, characterized in that: The adhesive is pineol.
7. A process for preparing the ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Preparing carbon black powder: subjecting carbon black material to nano-crushing treatment to obtain carbon black powder; (2) preparing oxide gel; using deionized water as solvent, adding Ce(NO3)3, Fe(NO3)3, citric acid and polyethylene glycol according to the mass ratio to obtain a mixed solution, and continuously stirring the mixed solution in a water bath at 80° C. for 2-4 hours to obtain a transparent sol; (3) preparing modified hydrotalcite powder: grinding the hydrotalcite into powder, adding the coupling agent and the modifier into a reaction kettle according to the mass ratio, sealing, evacuating and filling with nitrogen, and then stirring with a magnetic force for 6-8 hours, and vacuum drying to obtain the modified hydrotalcite powder; (4) Preparation of carbon black-based pigment: Add carbon black powder, oxide gel and modified hydrotalcite powder into a reactor according to the mass ratio, mix them evenly, then add adhesive and continue to stir evenly to finally obtain carbon black-based pigment.
8. The process for preparing the ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to claim 7, characterized in that: In step (1), the particle size of the carbon black powder is less than 1500 mesh.
9. The process for preparing the ultraviolet resistant and highly flame retardant carbon black-based pigment for papermaking according to claim 7, characterized in that: In step (4), the temperature of the reactor is 60-120° C. and the stirring time is 3-6 hours.