Preparation method of organic-inorganic hybrid tin-based illuminant

By co-crystallizing tin-based halides and metal hydroxides, a cladding structure is formed, which solves the problem of instability of tin-based halides in the air, and achieves the stability of tin-based halides and environmentally friendly organic and inorganic hybridization. Preparation of tin-based luminescent bodies, suitable for new display and lighting applications.

CN119039964APending Publication Date: 2024-11-29WENZHOU XINXIN TAIJING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145201.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The tin-based halide luminescent is unstable in the air and is easily oxidized, making it difficult for the light emitting device to work properly in the air.

Method used

By co-crystallizing the tin-based halide and the metal hydroxide, a metal hydroxide-covered structure is formed to isolate the air and prevent the tin-based halide from being oxidized. Ultrasonic dissolution and supersaturation crystallization processes are used to form organic and inorganic hybrid tin-based tin-based ions by using ultrasonic dissolution and supersaturation crystallization processes to form organic and inorganic hybrid tin-based ions Luminous body.

Benefits of technology

It improves the stability of tin-based halides, so that they can work normally in the air, and do not contain harmful heavy metal elements, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039964A_ABST
    Figure CN119039964A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an organic-inorganic hybrid tin-based illuminant, which comprises the following steps: S1, co-dissolving: respectively adding stannous fluoride and tetraethylammonium halide into a metal hydroxide solution for dissolving until the solution is clarified to obtain a mixed solution; s2, supersaturated crystallization: heating the mixed solution obtained in the step S1, and carrying out supersaturated crystallization on the tetraethylammonium tin halide to obtain a metal hydroxide coated product; the tetraethyl ammonium halide comprises at least one of tetraethyl ammonium bromide and tetraethyl ammonium iodide. The tin-based halide and the metal hydroxide are co-crystallized, so that a metal hydroxide coating structure is formed, the effect of isolating air is achieved, the tin-based halide is prevented from being oxidized, and the stability of the tin-based halide is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tin-based luminophore synthesis, and in particular relates to a method for preparing an organic-inorganic hybrid tin-based luminophore. Background Art

[0002] Metal halide crystals are an emerging material that usually have excellent luminescence and optoelectronic properties, especially organic-inorganic hybrid metal halide materials, which have high internal and external quantum yields, large absorption coefficients, and tunable luminescence peak positions, and are of great value in new display and lighting applications. However, the current mainstream metal halide luminescent materials contain heavy metal lead or cadmium, which are not friendly to the environment and human health, and have the problem of unsustainable development. Therefore, it is very important to develop a metal halide luminescent material that does not contain lead or cadmium.

[0003] Tin-based halide is a non-toxic, harmless, and environmentally friendly luminescent material. Tin and lead belong to the same main group element. After tin replaces lead, the halide crystal can still retain excellent luminescence performance. However, since divalent tin ions are easily oxidized to positive tetravalent ions, the crystal structure of its luminescent phase is destroyed, making the tin-based halide luminophore extremely unstable in the air, and light-emitting devices based on tin-based halides are difficult to work normally in the air. Therefore, the development of a tin-based halide luminescent material with air stability is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing an organic-inorganic hybrid tin-based luminophore, which co-crystallizes a tin-based halide and a metal hydroxide to form a metal hydroxide-coated structure, thereby isolating the tin-based halide from air, preventing the tin-based halide from being oxidized, and improving its stability.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing an organic-inorganic hybrid tin-based luminescent body, comprising the following steps:

[0006] S1. Co-dissolving: adding stannous fluoride and tetraethylammonium halide to a metal hydroxide solution and dissolving them respectively until the solution becomes clear to obtain a mixed solution;

[0007] S2, supersaturated crystallization: heating the mixed solution obtained in step S1 to supersaturate the tetraethylammonium tin halide to obtain a product coated with a metal hydroxide;

[0008] The tetraethylammonium halide includes at least one of tetraethylammonium bromide and tetraethylammonium iodide.

[0009] By adopting the above technical solution: in step S1, the metal hydroxide solution helps to dissolve SnF2, thereby obtaining a mixed solution rich in Sn2+ ions and tetraethylammonium ions.

[0010] In step S2, heating is performed to evaporate the water, and the mixed solution is supersaturated to cause crystals to precipitate. The metal hydroxide and the organic-inorganic hybrid tin-based halide are co-crystallized. During the supersaturated crystallization process, a large amount of metal hydroxide easily wraps the crystallized tin-based halide, isolating it from the air and preventing Sn2+ from reacting with oxygen.

[0011] Furthermore, the metal hydroxide solution is a KOH solution.

[0012] Furthermore, the dissolution condition in step S1 is: ultrasonic dissolution stirring. It should be noted that there are many ways to stir the dissolution of a substance, such as mechanical stirring using a stirring paddle, vibration stirring using ultrasound, magnetic stirring using a magnet, etc. These can all achieve the purpose of the present invention, and the ultrasonic dissolution stirring listed in this application is only an example and does not constitute a limitation on the scope of protection of the present invention.

[0013] Furthermore, the concentration of the KOH solution is 0.5 mol / L-5 mol / L.

[0014] Furthermore, the heating temperature of step S2 is 60°C-80°C.

[0015] Furthermore, the product of step S2 is a tin-based halide luminophore coated with KOH to prevent the tin-based halide from being oxidized.

[0016] Furthermore, the molar ratio of stannous fluoride to tetraethylammonium halide in step S1 is 1:3.

[0017] Furthermore, the molar ratio of KOH to stannous fluoride is at least 11:1.

[0018] Furthermore, the molar ratio of KOH to stannous fluoride is (15-20):1.

[0019] The beneficial effects of the present invention are mainly reflected in:

[0020] 1. The tin-based halide luminophore of the present invention does not contain heavy metal elements such as lead and cadmium and is environmentally friendly.

[0021] 2. The present invention provides a method for preparing an organic-inorganic hybrid tin-based luminescent body, by co-crystallizing with KOH to form a KOH-coated structure, which has the effect of isolating the air, preventing the tin-based halide from being oxidized, and improving its stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a photo of the sample in Example 1 of the present invention;

[0023] Figure 2 This is the emission spectrum (PL) of the sample in Example 1 of the present invention under 300nm ultraviolet light excitation;

[0024] Figure 3 is the excitation spectrum (PLE) diagram of the sample in Example 1 of the present invention;

[0025] Figure 4 This is a photo of the sample in Comparative Example 1 of the present invention (with black impurities);

[0026] Figure 5 Emission spectrum (PL) of the sample in Comparative Example 2 of the present invention under 300nm ultraviolet light excitation. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] Embodiment 1:

[0029] Mix 3 mmol of tetraethylammonium iodide and 1 mmol of SnF2 to obtain a mixture. Add 18 ml of 1 mol / L KOH solution to the mixture and stir with ultrasound until the solution is clear and the powder is completely dissolved. Heat at 60°C until the solution is completely dry and take out the sample powder.

[0030] Experimental analysis: Take the final product of the above preparation process, Figure 1 The sample powder photo is given. The product powder is uniformly white, and no black tin oxide particles are found, proving that the preparation process effectively avoids the reaction between tin ions and oxygen. Under 300nm ultraviolet light excitation, the sample powder emits uniform green light, and the luminescence spectrum is as follows: Figure 2 As shown in FIG. 1 , the sample has a luminescence peak in the range of 400-600 nm. Further testing of the excitation spectrum of the sample, as shown in FIG. Figure 3 As shown, the sample can be excited by short-wavelength ultraviolet light with a cutoff edge of approximately 370 nm.

[0031] Embodiment 2:

[0032] The difference from Example 1 is that the amount of KOH solution added to adjust the concentration to 1 mol / L is 15 ml.

[0033] Embodiment 3:

[0034] The difference from Example 1 is that the amount of KOH solution added to adjust the concentration to 1 mol / L is 20 ml.

[0035] Comparative Example 1:

[0036] This comparative example 1 will explore the effect of KOH in preventing the oxidation of tin-based halides. Compared with Example 1, this comparative example reduces the amount of KOH used and observes the changes in the product.

[0037] 3 mmol of tetraethylammonium iodide and 1 mmol of SnF2 were mixed evenly to obtain a mixture. 10 ml of 1 mol / L KOH solution was added to the mixture and ultrasonically stirred until the solution was clear and the powder was completely dissolved. The solution was heated at 60°C until it was completely dry and the sample powder was taken out.

[0038] Experimental analysis: The final product of the above preparation process was taken and it was found that the crystallized sample powder contained black granular impurities. Figure 4 , indicating that when the amount of KOH is reduced to a certain level, it cannot completely prevent the reaction of tin ions with oxygen.

[0039] Comparative Example 2:

[0040] This comparative example 2 will explore the effect of KOH in promoting the formation of tin-based halides. Compared with Example 1, this comparative example does not add KOH and observes the changes in the product.

[0041] 3 mmol of tetraethylammonium iodide and 1 mmol of SnF2 were mixed evenly to obtain a mixture. 18 ml of deionized water was added to the mixture and ultrasonically stirred to dissolve. The solution was heated at 60°C until it was completely dry, and the sample powder was taken out.

[0042] Experimental analysis: The final product of the above preparation process does not emit light under 300nm ultraviolet irradiation. Figure 5 This comparative example shows that the addition of KOH is a necessary condition to promote the formation of tin-based halide luminophores.

[0043] The present invention illustrates the detailed preparation method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed preparation method, that is, it does not mean that the present invention must rely on the above-mentioned products and detailed preparation methods to be implemented. It should be clear to those skilled in the art that any improvement of the present invention, the combination or equivalent replacement of the raw materials of the product of the present invention, all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an organic-inorganic hybrid tin-based luminescent body, characterized in that: The steps include: S1. Co-dissolving: adding stannous fluoride and tetraethylammonium halide to a metal hydroxide solution and dissolving them respectively until the solution becomes clear to obtain a mixed solution; S2, supersaturated crystallization: The mixed solution obtained in step S1 is heated to supersaturate and crystallize tetraethylammonium tin halide to obtain a product coated with a metal hydroxide; The tetraethylammonium halide includes at least one of tetraethylammonium bromide and tetraethylammonium iodide.

2. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 1, characterized in that: The metal hydroxide solution is a KOH solution.

3. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 1, characterized in that: The dissolution conditions in step S1 are: ultrasonic dissolution and stirring.

4. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 2, characterized in that: The concentration of the KOH solution is 0.5 mol / L-5 mol / L.

5. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 1, characterized in that: The heating temperature in step S2 is 60°C-80°C.

6. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 2, characterized in that: The product of step S2 is a tin-based halide luminophore wrapped with KOH to prevent the tin-based halide from being oxidized.

7. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 1, characterized in that: The molar ratio of stannous fluoride to tetraethylammonium halide in step S1 is 1:

3.

8. The method for preparing an organic-inorganic hybrid tin-based luminophore according to claim 4, characterized in that: The molar ratio of KOH to stannous fluoride is at least 11:

1.