Method for controlling total oxygen content in steel for automobile panel
By controlling multiple parameters in the converter and RH process, the stable control of the inclusion of total oxygen and oxide of the steel in the automotive panel is achieved, and the quality defects caused by excessive total oxygen are solved, and the cleanliness of the steel and the use of automotive panels is improved. The surface quality of steel.
Patent Information
- Application Number
- CN202411202664.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
In automotive panel production, excessive total oxygen content in the steel liquid will lead to mass defects in the casting billet, affecting the fatigue strength, plasticity and impact toughness of the steel, and it is difficult for the prior art to effectively control the level of total oxygen and inclusions in the steel. Affects the cleanliness of the molten steel and the casting ability.
By controlling the free oxygen content after the end point of the converter steel discharge and RH decarbonization, the weight content in the ladle slag, the acid-soluble aluminum content, and the oxygen blowing amount and vacuum degree of the RH process, the alkalinity, calcium-aluminum ratio of the ladle slag and MgO content controls the ladle sedation time and aluminum drop, and achieves stable control of the inclusion of all oxygen and oxides of molten steel throughout the process.
It effectively reduces the level of total oxygen and inclusions in the steel, improves the cleanliness of the steel and casting ability, and improves the surface quality of steel for automobile panels.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steelmaking, and in particular relates to a method for controlling the total oxygen content in steel for automobile panels. Background Art
[0002] With the development of the automobile industry, the quality requirements for automobile steel, especially automobile panel steel, are becoming increasingly stringent, and even zero-defect quality standards have been proposed for automobile outer panel steel. To this end, the quality of cold-rolled coils must be continuously improved. First, the steelmaking process needs to provide high-cleanliness defect-free ingots. Its quality control covers molten iron pretreatment, converter blowing, refining process control, inclusion control, continuous casting and machine cleaning and other steelmaking and continuous casting technologies. It is the top priority in automobile panel production control and a hot research topic for automobile panel manufacturers.
[0003] The total oxygen (TO) in the molten steel of automobile panels is composed of free oxygen in the steel and oxides after deoxidation. The lower the total oxygen value in the molten steel, the cleaner the molten steel. Therefore, total oxygen (TO) is a simple and effective method to evaluate the cleanliness of molten steel and is widely used in actual production. If the free oxygen in the ingot is too high, it is easy to cause bubbles in the ingot, resulting in quality defects. The oxide inclusions in the ingot are not easy to deform. Under the action of cyclic stress, the edges of the oxide inclusions are not easy to deform, and stress concentration is prone to occur, resulting in crack defects. When the content of oxide inclusions in the ingot is too high, it mainly affects the fatigue strength, plasticity, impact toughness and other properties of the steel. Under the same deoxidation method, the free oxygen content in the molten steel is not much different. The difference in total oxygen is mainly reflected in the combined oxygen part in the form of inclusions. Total oxygen can indirectly reflect the content level of non-metallic inclusions in the steel. For the production of automobile panels, the total oxygen content of molten steel is directly related to the inclusion level and surface quality of the product. There are many factors that affect total oxygen, which are affected by factors such as the end conditions of the converter, the process parameters of RH treatment, and secondary oxidation. Correctly analyzing the corresponding relationship between various influencing factors and total oxygen will help to more stably control and reduce the level of total oxygen and inclusions in steel, improve the cleanliness of molten steel, improve continuous casting castability, and thus improve the surface quality of automotive panels. Summary of the invention
[0004] The purpose of the present invention is to provide a method for controlling the total oxygen content in steel for automobile panels, especially for controlling the total oxygen content of molten steel in the process of producing steel for automobile panels in a converter-RH-continuous casting process. The technical solution of the present invention includes the following steps:
[0005] (1) Free oxygen content of molten steel during the whole process [O] D Control: including control of converter tapping endpoint, free oxygen content after RH decarburization and before deoxidation; control of (Fe t O) by weight ≤ 15%, the slag in the ladle after molten steel refining (Fet O) weight content 2% ≤ (Fe t O)≤4%; control the weight content of acid-soluble aluminum [Als] in molten steel ≥0.05%;
[0006] (2) Oxide inclusions in the whole process steel [O] I Control: including controlling the basicity R, calcium-aluminum ratio w(CaO) / w(Al2O3) and MgO content of the ladle slag, controlling the ladle calming time to 8-25min, and controlling the aluminum drop to ≤0.002%;
[0007] (3) RH process: Avoid excessive oxygen blowing, which may cause an increase in free oxygen content after RH decarburization and before deoxidation. The oxygen blowing amount required for RH molten steel decarburization is calculated as follows:
[0008] Q=(K*[C]-[O] in +250) / 2.5
[0009] Where: Q is the oxygen blowing amount required for RH process decarburization of molten steel, m 3 ;
[0010] K is the ratio of oxygen reduction to carbon reduction, which is 0.8 to 1.0;
[0011] [C] is the mass fraction of initial carbon, ppm;
[0012] [O] in is the mass fraction of oxygen in the RH inlet, ppm;
[0013] 250 is the mass fraction of reserved oxygen, ppm.
[0014] Furthermore, in the step (1), the free oxygen content in the molten steel at the end of converter steel tapping is controlled to be 450±100 ppm; and the free oxygen content after RH decarburization and before deoxidation is controlled to be 250-300 ppm.
[0015] Furthermore, in step (1), the [Als] content in the molten steel is controlled to be greater than the [Ti] content, that is, [Als] / [Ti]>1.0.
[0016] Furthermore, in step (2), the ladle slag basicity R=6±2, the calcium-aluminum ratio w(CaO) / w(Al2O3)=1.5±0.3, and the MgO content <10wt%.
[0017] Furthermore, in step (2), the MgO content in the ladle slag is controlled to be 4-6wt%.
[0018] Furthermore, in the step (3), the pre-deoxidation alloy in the RH process is added within 2 to 3 minutes after the vacuum degree reaches 5 kPa.
[0019] Furthermore, in step (3), after the RH process decarburization is completed, the argon blowing flow rate is reduced to 60% to 70% of the maximum flow rate during the decarburization period, and the vacuum degree is reduced to 5 to 8 kPa.
[0020] The beneficial effect of adopting the above technical scheme is that: the present invention more stably controls and reduces the level of total oxygen and inclusions in steel by correctly analyzing the corresponding relationship between various influencing factors in production and total oxygen, and stably controls the total oxygen TO content of molten steel in the continuous casting tundish to ≤18ppm, thereby improving the cleanliness of the molten steel and the continuous casting castability, thereby improving the surface quality of steel for automobile panels. DETAILED DESCRIPTION
[0021] The method for controlling the total oxygen content in steel for automobile panels of the present invention, in particular, is aimed at controlling the total oxygen content in molten steel during the production of steel for automobile panels by a converter-RH-continuous casting process, and specifically comprises the following steps:
[0022] 1. Free oxygen content of molten steel during the whole process [O] D Control:
[0023] Total oxygen (expressed as TO) in the molten steel of automobile panels is composed of free oxygen (expressed as [O] D denoted by [O] I Therefore, to control the total oxygen (TO) content in the molten steel of automobile panels, we must first control the free oxygen content in the molten steel throughout the process [O] D Specific measures include:
[0024] (1) Control the low free oxygen [O] content in molten steel at the end of converter tapping: [O] D =450±100ppm;
[0025] Converter end point [O] D The higher the [O]D is, the higher the [O]D is at the end of RH decarburization. t The higher the O content, the stronger the oxidizing property of the slag, the greater the deoxidizer consumption, and the increasing trend of inclusions and total oxygen in the steel. In order to improve the cleanliness of the steel, the converter end point [O] should be lowered. D This is to reduce the formation of inclusions in steel from the source, reduce the TO content of molten steel, and improve the cleanliness of steel, which is very important for the production of ultra-low carbon steel automotive panels.
[0026] (2) Control the low free oxygen content in ladle slag [O] D : That is, to control the (Fe t O) is ≤15% by mass, and the slag in the ladle after molten steel refining (Fe t O) mass content 2%≤(Fe tO)≤4%;
[0027] The oxygen activity at the slag interface is mainly composed of (Fe t O) is controlled, and it is significantly higher than that in the molten steel, and will be transferred from the slag to the molten steel. To control the transfer of oxygen from the slag to the molten steel during deoxidation, the (Fe t The lower the content of O), the better.
[0028] In order to control the oxygen transfer from slag to molten steel, many literatures require that the slag (Fe t O+MnO)≤1wt%. The applicant found in production practice that (Fe t O) is ≤2%. The slag may reduce the MgO in the ladle refractory to form magnesia-alumina spinel inclusions, which in turn increases the total oxygen (TO) content of the molten steel. Therefore, the content of (Fe t O) mass content 2%≤(Fe t O)≤4%. It breaks through the traditional theoretical requirement that the slag (Fe t The conventional view is that O+MnO)≤1%.
[0029] (3) Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-300 ppm;
[0030] The free oxygen content DEOX after RH decarburization and before deoxidation is one of the main factors affecting TO of molten steel in the tundish. Controlling DEOX is one of the necessary conditions for producing pure steel. Try to control DEOX within the range of 250-300ppm.
[0031] (4) Control the acid-soluble aluminum [Als] in the molten steel to ≥ 0.05%, and the [Als] content in the molten steel is greater than the [Ti] content, that is, [Als] / [Ti]>1.0;
[0032] The dissolved oxygen activity in molten steel is mainly controlled by the aluminum content in the steel. To maintain a low dissolved oxygen activity in molten steel, a certain aluminum content must be guaranteed in the molten steel, ensuring that the acid-soluble aluminum [Als] in the molten steel is ≥ 0.05%. For Ti-containing steels, in order to reduce the negative effects of Ti in the molten steel (reducing the interfacial tension of the slag, generating more inclusions, etc.) and Al-Ti composite inclusions, the [Als] content in the molten steel is guaranteed to be greater than the [Ti] content to avoid secondary oxidation of Ti.
[0033] 2. Oxide inclusions in the whole process steel [O] I Control:
[0034] In the molten steel during steel tapping [O] I →0, TO→[O] D ; But after the molten steel is deoxidized and alloyed, [O] DAlmost all the inclusions are transformed, at this time, [O] D →0, TO→[O] I Therefore, to reduce the TO of molten steel, it is necessary to reduce the oxide inclusions in the steel [O] I content, and oxide inclusions in steel [O] I The removal of oxide inclusions in steel depends on the I The process of floating and slag absorption, therefore, refined slag will also greatly affect the oxygen content in the steel. To obtain low-oxygen clean steel, it is necessary to select suitable refined slag.
[0035] (1) Control ladle slag basicity R = 6 ± 2;
[0036] Ladle slag (a 2 Al2O3 / a 3 SiO2) i.e. the activity of SiO2 and Al2O3 is the factor that affects the absorption of oxide inclusions by ladle slag [O] I The important parameters of 2 Al2O3 / a 3 SiO2) increases with the increase of alkalinity. When the alkalinity is less than 3, (a 2 Al2O3 / a 3 The value of SiO2 increases very rapidly, while when the basicity is greater than 3, its value increases very slowly. This shows that when the basicity is ≥4, it will rarely affect the dissolved oxygen activity in the molten pool, and this basicity is basically close to the maximum deoxidation capacity. Therefore, the basicity of the refined slag should avoid the area less than 4, and when the CaO content in the slag is too high, the precipitation of solid particles in the slag will cause the slag viscosity to rise and the fluidity to deteriorate. Therefore, the basicity of the refined slag should also be avoided to be too large. The appropriate ladle slag basicity is 4 to 8.
[0037] (2) Control the calcium-aluminum ratio of ladle slag w(CaO) / w(Al2O3) = 1.5±0.3;
[0038] The w(CaO) / w(Al2O3) in the ladle slag plays an important role in deoxidation. When the top slag (CaO) / w(Al2O3)=1.2~1.8, the ability of the refined slag to adsorb Al2O3 inclusions reaches the maximum. At the same time, in order to ensure the fluidity of the steel slag, the composition of the refined slag should be controlled so that the composition of the slag is located in the liquid phase region of the low melting point substance in the phase diagram. In particular, the ratio of w(CaO) / w(Al2O3) should be controlled so that it is in the range of 1.2~1.8 to reduce the formation of high melting point phases, reduce viscosity and improve slag fluidity.
[0039] (3) Control the MgO mass content in the ladle slag to 4% to 6%;
[0040] In the CaO-Al2O3-SiO2 slag system used to produce automobile panel steel, adding a small amount of MgO can reduce the activity of SiO2 and Al2O3 and improve the stability of the slag; at the same time, a small amount of MgO can expand the liquid phase of the slag system, which helps to improve the fluidity of the refined slag. Therefore, MgO in the refined slag is indispensable. In actual production, the MgO content in the slag should be controlled within the range of less than 10%, and as far as possible in the range of 4% to 6%.
[0041] (4) Control the ladle calming time to 8 to 25 minutes and control the aluminum drop to ≤ 0.002%;
[0042] The oxygen activity controlled by the Fe-[O] balance at the slag interface is obviously greater than the oxygen activity in the molten steel pool. Therefore, the oxygen at the steel-slag interface will be transferred to the molten steel pool, even if the (Fe t O) content is less than 1%, but the slag (Fe t O) is still an oxygen source for molten steel. Therefore, the residence time of the ladle affects both the change of TO of molten steel in the tundish and the change of aluminum drop. In the actual production process, the ladle calming time is controlled as much as possible within 8 to 25 minutes. The longer the ladle calming time is, the better it is. This corrects the traditional view that the longer the ladle calming time is, the better it is.
[0043] 3. Optimization of RH process:
[0044] RH refining control, based on oxide inclusions in steel [O] I The principle is to produce less, produce earlier and float earlier.
[0045] (1) RH molten steel pre-deoxidation technology
[0046] The oxygen setting in the RH process can accurately control the free oxygen content of the molten steel at the end of decarburization and the oxygen blowing amount required for decarburization. While removing oxygen, the temperature of the molten steel can also be increased. The timing of putting the molten steel pre-deoxidation alloy (metal aluminum, etc.) into use is as early as possible without affecting the vacuum pumping. In production, it is generally best to put the pre-deoxidation alloy into use within 2 to 3 minutes after the vacuum reaches 5kpa.
[0047] (2) Calculation of oxygen blowing amount required for RH molten steel decarburization
[0048] The amount of oxygen blowing required for RH molten steel decarburization is calculated using the following formula to avoid excessive oxygen blowing causing an increase in the free oxygen content DEOX after RH decarburization but before deoxidation.
[0049] Q=(K*[C]-[O] in +250) / 2.5
[0050] Where: Q is the oxygen blowing amount required for RH process decarburization of molten steel, m 3 ;
[0051] K is the ratio of oxygen reduction to carbon reduction, which is 0.8 to 1.0;
[0052] [C] is the mass fraction of initial carbon, ppm;
[0053] [O] in is the mass fraction of oxygen in the RH inlet, ppm;
[0054] 250 is the mass fraction of reserved oxygen, ppm.
[0055] (3) After the RH decarburization is completed, the argon blowing flow rate is reduced to 60%-70% of the maximum flow rate during the decarburization period, and the vacuum degree is reduced to 5-8kPa;
[0056] After RH decarburization is completed, the argon blowing flow rate and vacuum degree are reduced, the circulation flow rate and flow rate of molten steel in RH are reduced, the follow-up of inclusions is reduced, which is conducive to the floating of small inclusions, and finally reduces oxide inclusions [O] I The content of and TO content of molten steel.
[0057] The present invention will be further described below by way of examples.
[0058] Example 1
[0059] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0060] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0061] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =350ppm;
[0062] Control the content of Fe(Fe t O) has a mass content of 13.0%, and the slag in the ladle after molten steel refining has a mass content of (Fe t O) has a mass content of 2.0%;
[0063] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-260ppm;
[0064] The acid-soluble aluminum [Als] in the molten steel is controlled to 0.05%, the [Ti] in the molten steel is controlled to 0.04%, and [Als] / [Ti]=1.25.
[0065] (2) Oxide inclusions in the whole process steel [O] I Control:
[0066] The ladle slag basicity R is controlled to be 4, the calcium-aluminum ratio w(CaO) / w(Al2O3)=1.2, and the MgO content is 4.0%;
[0067] The ladle calming time is controlled to 25 minutes and the aluminum content is controlled to drop to 0.002%.
[0068] (3) Optimization of RH process:
[0069] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 2.5 minutes after the vacuum starts;
[0070] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 400ppm; RH inlet oxygen mass fraction [O] in =350ppm, reserved oxygen mass fraction = 250ppm; K value is 0.9, then the oxygen blowing amount required for RH process decarburization Q = 104m 3 ;
[0071] After RH decarburization, the argon blowing flow rate was reduced to 70% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 5kpa, and the inclusions smaller than 50μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and the TO of the molten steel in the tundish was measured to be 15.8ppm.
[0072] Example 2
[0073] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0074] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0075] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =550ppm;
[0076] Control the content of Fe(Fe t O) has a mass content of 15.0%, and the slag in the ladle after molten steel refining has a mass content of 15.0%. t O) has a mass content of 4.0%;
[0077] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-300ppm;
[0078] The acid-soluble aluminum [Als] in the molten steel is controlled to 0.06%, the [Ti] in the molten steel is controlled to 0.04%, and [Als] / [Ti]=1.5.
[0079] (2) Oxide inclusions in the whole process steel [O] IControl:
[0080] The ladle slag basicity R is controlled to be 8, the calcium-aluminum ratio w(CaO) / w(Al2O3)=1.8, and the MgO content is 6%;
[0081] The ladle calming time is controlled to 8 minutes and the aluminum content is controlled to drop to 0.0018%.
[0082] (3) Optimization of RH process:
[0083] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 3 minutes after the vacuum starts;
[0084] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 550ppm; RH inlet oxygen mass fraction [O] in =550ppm, reserved oxygen mass fraction = 250ppm; K value is 1.0, then the oxygen blowing amount required for RH process decarburization Q = 100m 3 ;
[0085] After RH decarburization, the argon blowing flow rate was reduced to 60% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 5kpa, and the inclusions smaller than 20μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and TO of the molten steel in the tundish was measured to be 18ppm.
[0086] Example 3
[0087] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0088] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0089] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =500ppm;
[0090] Control the content of Fe(Fe t O) is 14.5% by mass, and the slag in the ladle after molten steel refining is (Fe t O) has a mass content of 3.0%;
[0091] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-290ppm;
[0092] The acid-soluble aluminum [Als] in the molten steel is controlled to 0.06%, the [Ti] in the molten steel is controlled to 0.05%, and [Als] / [Ti]=1.2.
[0093] (2) Oxide inclusions in the whole process steel [O] I Control:
[0094] Control ladle slag basicity R to 5, calcium aluminum ratio w(CaO) / w(Al2O3)=1.7, MgO content to 5%;
[0095] The ladle calming time is controlled to 20 minutes and the aluminum content is controlled to drop to 0.0015%.
[0096] (3) Optimization of RH process:
[0097] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 2.0min after the vacuum starts;
[0098] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 500ppm; RH inlet oxygen mass fraction [O] in =500ppm, reserved oxygen mass fraction = 250ppm; K value is 0.8, then the oxygen blowing amount required for RH process decarburization Q = 60m 3 ;
[0099] After RH decarburization, the argon blowing flow rate was reduced to 65% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 8kpa, and the inclusions smaller than 40μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and the TO of the molten steel in the tundish was measured to be 17.5ppm.
[0100] Example 4
[0101] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0102] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0103] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =450ppm;
[0104] Control the content of Fe(Fe t O) is 14.0% by mass, and the slag in the ladle after molten steel refining is (Fe t O) has a mass content of 2.5%;
[0105] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-270ppm;
[0106] The acid-soluble aluminum [Als] in the molten steel is controlled to be 0.055%, the [Ti] in the molten steel is controlled to be 0.05%, and [Als] / [Ti]=1.1.
[0107] (2) Oxide inclusions in the whole process steel [O] I Control:
[0108] The ladle slag basicity R is controlled to be 6, the calcium-aluminum ratio w(CaO) / w(Al2O3)=1.6, and the MgO content is 5%;
[0109] The ladle calming time is controlled to 11 minutes and the aluminum content is controlled to drop to 0.0016%.
[0110] (3) Optimization of RH process:
[0111] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 2.5 minutes after the vacuum starts;
[0112] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 400ppm; RH inlet oxygen mass fraction [O] in =450ppm, reserved oxygen mass fraction = 250ppm; K value is 1.0, then the oxygen blowing amount required for RH process decarburization Q = 80m 3 ;
[0113] After RH decarburization, the argon blowing flow rate was reduced to 70% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 6kpa, and the inclusions smaller than 30μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and the TO of the molten steel in the tundish was measured to be 17.5ppm.
[0114] Example 5
[0115] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0116] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0117] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =400ppm;
[0118] Control the content of Fe(Fe t O) has a mass content of 13.5%, and the slag in the ladle after molten steel refining has a mass content of (Fe t O) has a mass content of 3.0%;
[0119] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-280ppm;
[0120] The acid-soluble aluminum [Als] in the molten steel is controlled to be 0.07%, the [Ti] in the molten steel is controlled to be 0.06%, and [Als] / [Ti]=1.16.
[0121] (2) Oxide inclusions in the whole process steel [O] I Control:
[0122] The ladle slag basicity R is controlled to be 7, the calcium-aluminum ratio w(CaO) / w(Al2O3)=1.5, and the MgO content is 5%;
[0123] The ladle calming time is controlled to 17 minutes and the aluminum content is controlled to drop to 0.0018%.
[0124] (3) Optimization of RH process:
[0125] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 2.0min after the vacuum starts;
[0126] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 400ppm; RH inlet oxygen mass fraction [O] in =400ppm, reserved oxygen mass fraction = 250ppm; K value is 0.8, then the oxygen blowing amount required for RH process decarburization Q = 68m 3 ;
[0127] After RH decarburization, the argon blowing flow rate was reduced to 60% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 5kpa, and the inclusions smaller than 20μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and TO of the molten steel in the tundish was measured to be 18ppm.
[0128] Example 6
[0129] A factory produces steel for automobile panels through the blast furnace-converter-RH-continuous casting process. The control of the total oxygen content of the molten steel includes the following steps:
[0130] (1) Free oxygen content of molten steel during the whole process [O] D Control:
[0131] Controlling low free oxygen content in molten steel at the end of converter tapping[O] D =400ppm;
[0132] Control the content of Fe(Fe t O) is 14.0% by mass, and the slag in the ladle after molten steel refining is (Fe tO) has a mass content of 3.0%;
[0133] Control the free oxygen content DEOX after RH decarburization and before deoxidation within the range of 250-290ppm;
[0134] The acid-soluble aluminum [Als] in the molten steel is controlled to 0.06%, the [Ti] in the molten steel is controlled to 0.05%, and [Als] / [Ti]=1.2.
[0135] (2) Oxide inclusions in the whole process steel [O] I Control:
[0136] Control ladle slag basicity R to 5, calcium aluminum ratio w(CaO) / w(Al2O3)=1.4, MgO content to 5%;
[0137] The ladle calming time is controlled to 20 minutes and the aluminum content is controlled to drop to 0.0018%.
[0138] (3) Optimization of RH process:
[0139] After the vacuum degree reaches 5kpa, add the pre-deoxidized alloy within 2.5 minutes after the vacuum starts;
[0140] The oxygen blowing amount required for RH molten steel decarburization is calculated by the formula Q = (K*[C] - [O] in +250) / 2.5, initial carbon mass fraction [C] = 350ppm; RH inlet oxygen mass fraction [O] in =400ppm, reserved oxygen mass fraction = 250ppm; K value is 1.0, then the oxygen blowing amount required for RH process decarburization Q = 80m 3 ;
[0141] After RH decarburization, the argon blowing flow rate was reduced to 65% of the maximum flow rate during the decarburization period, the vacuum degree was reduced to 6kpa, and the inclusions smaller than 20μm floated fully. A full oxygen sample was taken from the continuous casting tundish, and TO of the molten steel in the tundish was measured to be 17.0ppm.
Claims
1. A method for controlling the total oxygen content in steel for automobile panels, characterized in that: The converter-RH-continuous casting production process is adopted, which specifically includes the following steps: (1) Free oxygen content of molten steel during the whole process [O] D Control: including control of converter tapping endpoint, free oxygen content after RH decarburization and before deoxidation; control of (Fe t O) by weight ≤ 15%, the slag in the ladle after molten steel refining (Fe t O) weight content 2% ≤ (Fe t O)≤4%; control the weight content of acid-soluble aluminum [Als] in molten steel ≥0.05%; (2) Oxide inclusions in the whole process steel [O] I Control: including controlling the basicity R, calcium-aluminum ratio w(CaO) / w(Al2O3) and MgO content of the ladle slag, controlling the ladle calming time to 8-25min, and controlling the aluminum drop to ≤0.002%; (3) RH process: Avoid excessive oxygen blowing, which may cause an increase in free oxygen content after RH decarburization and before deoxidation. The oxygen blowing amount required for RH molten steel decarburization is calculated as follows: Q=(K*[C]-[O] in +250) / 2.5 Where: Q is the oxygen blowing amount required for RH process decarburization of molten steel, m 3 ; K is the ratio of oxygen reduction to carbon reduction, which is 0.8 to 1.0; [C] is the mass fraction of initial carbon, ppm; [O] in is the mass fraction of oxygen in the RH inlet, ppm; 250 is the mass fraction of reserved oxygen, ppm.
2. The method for controlling the total oxygen content in steel for automobile panels according to claim 1, characterized in that: In the step (1), the free oxygen content in the molten steel at the end point of converter tapping is controlled to be 450±100 ppm.
3. The method for controlling the total oxygen content in steel for automobile panels according to claim 2, characterized in that: In the step (1), the free oxygen content after RH decarburization and before deoxidation is controlled to be 250 to 300 ppm.
4. The method for controlling the total oxygen content in steel for automobile panels according to claim 3, characterized in that: In the step (1), the [Als] content in the molten steel is controlled to be greater than the [Ti] content, that is, [Als] / [Ti]>1.
0.
5. The method for controlling the total oxygen content in steel for automobile panels according to claim 4, characterized in that: In the step (2), the basicity of the ladle slag is controlled to be R=6±2, the calcium-aluminum ratio w(CaO) / w(Al2O3) is controlled to be 1.5±0.3, and the MgO content is controlled to be less than 10wt%.
6. The method for controlling the total oxygen content in steel for automobile panels according to claim 5, characterized in that: In the step (2), the MgO content in the ladle slag is controlled to be 4-6wt%.
7. The method for controlling the total oxygen content in steel for automobile panels according to claim 6, characterized in that: In the step (3), the pre-deoxidation alloy in the RH process is added within 2 to 3 minutes after the vacuum degree reaches 5 kPa.
8. The method for controlling the total oxygen content in steel for automobile panels according to any one of claims 1 to 7, characterized in that: In the step (3), after the RH process decarburization is completed, the argon blowing flow rate is reduced to 60% to 70% of the maximum flow rate during the decarburization period, and the vacuum degree is reduced to 5 to 8 kPa.