Heat treatment process for bearing steel containing superfine carbide bainite

Through multi-step austenitization, carbide precipitation and isothermal quenching treatment, a fine and uniformly distributed carbide is formed, solving the problem of bottlenecks in the performance of bearing steel in traditional heat treatment methods, and achieving high performance and wear resistance of bearing steel Improved performance and extend service life.

CN119040584APending Publication Date: 2024-11-29ZHEJIANG UNIV OF TECH SHENGZHOU INNOVATION RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411349442.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional quenched tempered bearing steel heat treatment methods are difficult to significantly improve the performance of bearing steel, especially in terms of wear resistance and toughness, and carbide distribution control is difficult, which affects the performance of the material.

Method used

Using a heat treatment process of ultrafine carbide bainite bearing steel, through multi-step austenitization, carbide precipitation, isothermal quenching and tempering treatment, a fine and uniformly distributed carbide and alloy carbide are formed. Promote the formation of ultrafine nanoscale carbides and solid solution strengthening of matrix structure, combine graded isothermal quenching and low-temperature tempering to optimize the morphology and distribution of bainite and residual austenite.

Benefits of technology

It significantly improves the hardness, tensile strength, impact toughness and wear resistance of bearing steel, extends the service life, and realizes the control of carbide distribution, improving the service performance of high-end bearings and lightweight parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040584A_ABST
    Figure CN119040584A_ABST
Patent Text Reader

Abstract

The invention provides a heat treatment process for bearing steel containing superfine carbide bainite, and belongs to the technical field of heat treatment of alloy for bearings. A bearing steel billet serves as an object, after the billet is subjected to casting, refining, hot forging and natural cooling to the room temperature, the billet is subjected to first austenitizing treatment in a vacuum atmosphere furnace, and oil quenching is conducted to the room temperature; performing carbide precipitation treatment on the steel billet subjected to oil quenching in a vacuum atmosphere furnace; second austenitizing treatment is conducted, then first-step isothermal quenching heat treatment is rapidly conducted, second-step isothermal quenching heat treatment is rapidly conducted, and water cooling is conducted to the room temperature; and after low-temperature tempering heat treatment, air-cooling to room temperature to finish heat treatment. The microstructure of the bearing steel obtained through heat treatment is composed of carbide, tempered martensite, lower bainite and a small amount of retained austenite which are small in size and uniform in distribution, and the bearing steel has excellent tensile property and impact toughness and meanwhile has high abrasion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a heat treatment process for bainite bearing steel containing ultrafine carbides, and belongs to the technical field of heat treatment of bearing alloys. Background Art

[0002] With the rapid development of high-power wind turbines, high-speed railways, shield machines and other fields in my country, people's demand for high-end bearings is increasing, and at the same time, higher requirements are placed on the performance of bearing raw materials. Heat treatment is one of the effective ways to improve the service performance of bearing steel. By changing the process parameters such as heating temperature, holding time, cooling rate, etc., the matrix structure of bearing steel can be adjusted to achieve the strengthening and toughening of bearing steel. However, the traditional quenched and tempered bearing steel can no longer meet the urgent needs of designers and customers for high-performance materials. The related research on quenching and tempering heat treatment of bearing steel has also encountered bottlenecks, and it is difficult to make major breakthroughs in a short period of time. Therefore, we urgently need to propose a heat treatment process that is flexible and practical, easy to operate, does not change the existing equipment, and can significantly improve the performance of bearing steel.

[0003] In 1934, a black needle-like structure that is different from martensite and pearlite was defined as bainite, and it has continued to attract in-depth research by scholars at home and abroad. Bainite soon attracted the attention of bearing companies around the world due to its excellent comprehensive performance. During the isothermal quenching heat treatment, a large amount of lower bainite and residual austenite are formed in the matrix structure of the bearing steel, which makes it have higher elongation and impact toughness, but the wear resistance of ordinary bainitic bearing steel is often not comparable to that of martensitic bearing steel. A large number of experimental results show that the introduction of carbides into the matrix structure can significantly improve the wear resistance of steel materials. The nano-scale carbides in the surface and sub-surface layers have the functions of increasing the hardness of the contact surface, hindering the initiation and expansion of cracks, separating the contact surface of the friction pair, and bearing part of the external load, effectively protecting the wear surface and reducing the wear amount. However, the distribution of carbides cannot be controlled in the current heat treatment method, which leads to a rough distribution of carbides after heat treatment, affecting the strength and toughness of the bearing raw materials. Summary of the invention

[0004] In view of this, the present application provides a heat treatment process for bainitic bearing steel containing ultrafine carbides, which can increase the aggregation amount and reduce the size of carbides, thereby improving the strength and toughness of the material. It not only improves the service performance of high-end bearings and extends their service life, but also realizes the control of carbide distribution and achieves lightweighting of related components.

[0005] Specifically, the present application is implemented through the following scheme:

[0006] A heat treatment process for bearing steel containing ultrafine carbides and bainite, with bearing steel billets as the object, after the billets are cast, refined, hot forged, and naturally cooled to room temperature (generally 20-24°C), the following steps are performed:

[0007] Step 1: austenitizing the steel billet for the first time in a vacuum atmosphere furnace at a temperature of 1000-1100° C. for 20-30 min, followed by oil quenching (denoted as Q) to room temperature;

[0008] Step 2: In a vacuum atmosphere furnace, the oil-quenched steel billet is heated to 650-700°C, kept at this temperature for 20-30 minutes, and then air-cooled to room temperature to complete the carbide precipitation treatment (denoted as P);

[0009] Step 3: performing a second austenitizing treatment on the steel billet in a vacuum atmosphere furnace at a treatment temperature of 900-950° C. for 30-40 minutes;

[0010] Step 4: The steel billet is quickly transferred into a low-temperature salt bath furnace for the first isothermal quenching heat treatment (denoted as A1), the isothermal quenching temperature is 280-320°C, and the treatment time is 5-8 minutes;

[0011] Step 5: The steel billet is quickly transferred into a high-temperature salt bath furnace for a second isothermal quenching heat treatment (denoted as A2), the isothermal quenching temperature is 350-380°C, the treatment time is 25-30 minutes, and the steel billet is water-cooled to room temperature;

[0012] Step six, the steel billet is transferred into a box-type furnace for low-temperature tempering heat treatment (denoted as T), the low-temperature tempering temperature is 120-150°C, the treatment time is 20-30 minutes, and then air-cooled to room temperature to complete the heat treatment.

[0013] The above steps take the steel billet as the treatment object, and complete the first austenitization-oil quenching-carbide precipitation-second austenitization-isothermal quenching heat treatment in a low-temperature salt bath-isothermal quenching heat treatment in a high-temperature salt bath in sequence, forming a new heat treatment process characterized by QP-A1-A2-T. In this process, the formation of carbides and alloy carbides in the organization is promoted through a separate carbide precipitation treatment, and larger carbides and alloy carbides (such as (CrFe)) are formed at the grain boundaries and inside the grains in the bearing steel organization. 23 C6 and Cr 23C6), under the above-mentioned treatment conditions, the size of carbides and alloy carbides is controlled, and the precipitation phase is retained during the air cooling process, increasing the distribution of carbides. In this way, in the subsequent second austenitization treatment, carbides and alloy carbides are partially dissolved at high temperature, and the surface and subsurface carbon of the precipitation phase and alloy elements diffuse. On the one hand, the mechanical properties of the matrix structure can be effectively improved through solid solution strengthening, and on the other hand, the refinement of carbides and alloy carbides can be achieved, so that the size of carbides can be reduced. The combination of two austenitizations and oil quenching and carbide precipitation can form a large number of ultrafine nano-scale carbides in the organization. The final treatment is combined with two steps of graded isothermal quenching heat treatment at different temperatures, which is conducive to the formation of fine lower bainite structure and residual austenite, wherein low-temperature isothermal quenching uses a higher degree of supercooling to improve the nucleation efficiency of lower bainite, providing favorable conditions for the subsequent refinement of lower bainite; and the subsequent high-temperature isothermal quenching promotes the growth of lower bainite and forms island-shaped residual austenite around the lower bainite lath. In the subsequent water-cooling quenching, the unstable austenite is transformed into martensite, which can further improve the hardness, strength and wear resistance of the bearing steel. At the end of the treatment, low-temperature tempering heat treatment is introduced to release residual stress, further improve the impact resistance of the bearing steel, and improve the toughness and plasticity of the bearing steel.

[0014] Further, as a preference:

[0015] In the vacuum atmosphere furnace, the protective gas is nitrogen or argon.

[0016] In step one,

[0017] The quenching medium of the oil quenching is vacuum quenching oil, which includes 95.0wt.% of refined base oil, 0.5wt.% of antioxidant, 3.0wt.% of composite auxiliary agent and 1.5wt.% of catalytic agent.

[0018] The cooling rate of oil quenching is 20-30℃ / s.

[0019] In step four,

[0020] After the second austenitizing treatment, the steel billet is transferred into a low-temperature salt bath furnace within 20 to 30 seconds.

[0021] In the low-temperature salt bath furnace, the salt bath medium is a mixture of KCl:NaCl=1:1 (mass ratio).

[0022] In step five,

[0023] The steel billet after the first step of isothermal quenching heat treatment is transferred to the high-temperature salt bath furnace for the second step of isothermal quenching heat treatment within 10 to 20 seconds.

[0024] In the high-temperature salt bath furnace, the salt bath medium is a mixture of KCl:NaCl:BaCl2=4~5:1.5~2.0:3.0~3.5 (mass ratio).

[0025] The cooling medium of the water cooling is alkaline water (NaOH), and the concentration of NaOH is 5-8wt.%.

[0026] In step six,

[0027] In the second step, the steel billet after isothermal quenching heat treatment is transferred to low temperature tempering heat treatment within 1 to 2 hours.

[0028] The above scheme combines carbide precipitation treatment, graded isothermal quenching heat treatment and low-temperature tempering heat treatment technology. Through precise control of the size, morphology, quantity and distribution characteristics of bearing steel carbides and alloy carbides, tempered martensite, lower bainite and residual austenite, a new type of bearing steel is obtained. Its microstructure is composed of small and evenly distributed carbides, tempered martensite, lower bainite and a small amount of residual austenite, achieving a synergistic improvement in performance indicators such as bearing steel hardness, yield strength, tensile strength, impact toughness and wear resistance, while retaining a high elongation. The research and development of new high-performance bearing steel can greatly improve the service performance and service life of high-end bearings in fields such as wind turbines, high-speed railways, ships and shield machines, and also provide a guarantee for the lightweighting of related components. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0030] Figure 1 This is a metallographic photograph of the product after treatment in Example 1 of this application. DETAILED DESCRIPTION

[0031] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application clearer, the technical solutions in the embodiments of this application will be further described in detail below in conjunction with the drawings in the embodiments of this application. It should be understood that the specific embodiments described herein are only used to explain this application and are not used to limit the technical solutions of this application. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0032] In this embodiment, in the mechanical properties and wear resistance tests: the tensile properties adopt the GB / T228.1-2010 test standard; the impact properties adopt the GB / T229-2007 test standard; the wear resistance test is carried out on a multifunctional friction and wear testing machine, using a ball-disc rotating sliding wear test module, the upper sample is a Si3N4 ceramic ball with a diameter of 6 mm, a hardness of 85 HRC, and a surface roughness of 50±10 nm, the lower sample is bearing steel, with a size of 20 mm (length) ╳ 20 mm (width) ╳ 6 mm (height), a surface roughness of 100±50 nm, an external load of 100 N, a movement speed of 1 m / s, a test time of 20 min, and a test temperature of 22°C.

[0033] Example 1

[0034] (1) After casting, refining and hot forging, the bearing steel billet is naturally cooled to room temperature (22°C);

[0035] (2) The bearing steel billet is subjected to the first austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 1050°C, and the holding time is 20 min;

[0036] (3) Then oil quench (Q) to room temperature (22°C) at a cooling rate of 25°C / s; wherein the quenching medium of the oil quench is U8112 rapid quenching oil.

[0037] (4) Carbide precipitation treatment (P) is then performed, and the oil-quenched bearing steel is heated to 670°C in a vacuum atmosphere furnace and kept at this temperature for 25 minutes; and then air-cooled to room temperature (22°C);

[0038] (5) Then, the bearing steel is subjected to a second austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 925°C, and the holding time is 35 minutes;

[0039] (6) The mixture is then quickly transferred to a low-temperature salt bath furnace for the first isothermal quenching heat treatment (A1), with an isothermal quenching temperature of 295°C and a holding time of 6 min;

[0040] The salt bath medium of the low-temperature salt bath furnace is a mixture of KCl:NaCl=1:1 (mass ratio).

[0041] (7) Then quickly transfer to a high-temperature salt bath furnace for a second step of isothermal quenching heat treatment (A2), the isothermal quenching temperature is 360°C, the heat preservation time is 30 minutes, and then water-cooled to room temperature (22°C);

[0042] The salt bath medium of the high temperature salt bath furnace is a mixture of KCl:NaCl:BaCl2=4:2.0:3.0 (mass ratio). The cooling medium of the water cooling is 6wt.% alkaline water (NaOH).

[0043] (8) Finally, the austempered bearing steel is transferred into a box furnace for low-temperature tempering heat treatment at a tempering temperature of 150 °C for 25 min, and then air-cooled to room temperature (22 °C).

[0044] The steel billet obtained by the above method was tested, and the results are as follows: Figure 1 As shown: the steel billet after heat treatment in the present application shows a fine-sized microstructure, the black needle-shaped structure is bainite, and the carbides, tempered martensite, lower bainite and austenite are evenly distributed.

[0045] Example 2

[0046] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the temperature of the carbide precipitation treatment (P) is 650° C. and the holding time is 20 min.

[0047] Example 3

[0048] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the temperature of the carbide precipitation treatment (P) is 650° C. and the holding time is 30 min.

[0049] Example 4

[0050] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the insulation time of the carbide precipitation treatment (P) is 20 minutes.

[0051] Example 5

[0052] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the insulation time of the carbide precipitation treatment (P) is 30 minutes.

[0053] Example 6

[0054] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the temperature of the carbide precipitation treatment (P) is 690°C.

[0055] Example 7

[0056] The configuration of this embodiment is the same as that of embodiment 1, except that in step (4), the temperature of the carbide precipitation treatment (P) is 700° C. and the holding time is 30 min.

[0057] Table 1: Mechanical properties and wear resistance of bainitic bearing steel under different carbide precipitation treatment conditions

[0058]

[0059] The above Examples 1 to 7 respectively tested the effects of parameters in the carbide precipitation process from the perspectives of temperature, time, and temperature and time.

[0060] It can be seen from Table 1 that under the same conditions, as the temperature of carbide precipitation treatment increases or the time is extended, the yield strength and tensile strength of the bearing steel increase, but its elongation and impact toughness decrease significantly. When the temperature exceeds 670°C, the wear volume of the bearing steel does not change significantly. This shows that increasing the temperature or extending the time in the carbide precipitation treatment can promote the formation of carbides in the matrix, but too high a temperature and too long a time will cause the carbides to coarsen, resulting in a significant decrease in the elongation and impact properties of the bearing steel.

[0061] Example 8

[0062] The configuration of this embodiment is the same as that of embodiment 1, except that in step (2), the temperature of the first austenitizing treatment is 1000°C.

[0063] Example 9

[0064] The configuration of this embodiment is the same as that of embodiment 1, except that in step (2), the temperature of the first austenitizing treatment is 1000° C. and the holding time is 30 min.

[0065] Example 10

[0066] The configuration of this embodiment is the same as that of embodiment 1, except that in step (2), the holding time of the first austenitizing treatment is 30 minutes.

[0067] Embodiment 11

[0068] The configuration of this embodiment is the same as that of embodiment 1, except that in step (2), the temperature of the first austenitizing treatment is 1100°C.

[0069] Example 12

[0070] The configuration of this embodiment is the same as that of embodiment 1, except that in step (2), the temperature of the first austenitizing treatment is 1100° C. and the holding time is 30 min.

[0071] Table 2: Mechanical properties and wear resistance of bainitic bearing steel under different first austenitizing treatment conditions

[0072]

[0073] It can be seen from Table 2 that in the first austenitizing treatment, the influence of austenitizing temperature on the performance of bearing steel is more significant than time. When the temperature is 1000℃ or 1100℃, the yield strength and tensile strength of bearing steel are lower than those at 1050℃, especially when the temperature is 1100℃, the elongation and impact toughness of bearing steel are reduced at the same time. This is because when the temperature is low, the alloy elements in the matrix are not fully diffused, there is segregation, and the mechanical properties of bearing steel are reduced. When the temperature is high, the matrix grains grow too fast and the structure is coarsened, which also has a negative effect on the mechanical properties of bearing steel.

[0074] Example 13

[0075] The configuration of this embodiment is the same as that of embodiment 1, except that in step (5), the second austenitizing treatment temperature is 900° C. and the holding time is 30 min.

[0076] Embodiment 14

[0077] The configuration of this embodiment is the same as that of embodiment 1, except that in step (5), the second austenitizing treatment temperature is 900° C. and the holding time is 40 min.

[0078] Embodiment 15

[0079] The configuration of this embodiment is the same as that of embodiment 1, except that in step (5), the second austenitizing treatment temperature is 950° C. and the holding time is 30 min.

[0080] Example 16

[0081] The configuration of this embodiment is the same as that of embodiment 1, except that in step (5), the second austenitizing treatment temperature is 950° C. and the holding time is 40 min.

[0082] Embodiment 17

[0083] The configuration of this embodiment is the same as that of embodiment 1, except that in step (5), the holding time of the second austenitization is 30 minutes.

[0084] Table 3. Mechanical properties and wear resistance of bainitic bearing steel under different second austenitizing treatment conditions

[0085]

[0086] It can be seen from Table 3 that in the second austenitizing treatment, when the temperature is 900℃, the yield strength and tensile strength of the bearing steel are lower than those at 950℃, especially when the temperature is reduced to 900℃ and the time is extended to 40min, the elongation and impact toughness of the bearing steel also show a significant decrease. When the temperature is 950℃, the yield strength, tensile strength, elongation and impact toughness of the bearing steel are all lower than those at 950℃. When the time is shortened to 30min without changing the temperature, the mechanical properties of the bearing steel are also reduced. This shows that lowering the temperature or shortening the time in the second austenitizing treatment is not conducive to the refinement of carbides in the matrix, resulting in a decrease in the mechanical properties of the bearing steel. However, when the temperature is higher or the time is longer, the carbides in the matrix dissolve, the number decreases, and the strengthening and toughening effect on the matrix is ​​reduced.

[0087] Embodiment 18

[0088] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the first step of isothermal quenching heat treatment temperature is 280° C., and the holding time is 5 min.

[0089] Embodiment 19

[0090] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the first step of isothermal quenching heat treatment temperature is 280° C., and the holding time is 8 minutes.

[0091] Embodiment 20

[0092] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the holding time of the first step of isothermal quenching heat treatment is 7 minutes.

[0093] Embodiment 21

[0094] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the first step of isothermal quenching heat treatment temperature is 300°C.

[0095] Embodiment 22

[0096] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the first step of isothermal quenching heat treatment temperature is 320°C.

[0097] Embodiment 23

[0098] The configuration of this embodiment is the same as that of embodiment 1, except that in step (6), the first step of isothermal quenching heat treatment temperature is 320° C., and the holding time is 8 min.

[0099] Embodiment 24

[0100] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 350° C. and the holding time is 25 min.

[0101] Embodiment 25

[0102] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 350°C.

[0103] Embodiment 26

[0104] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 360° C. and the holding time is 25 min.

[0105] Embodiment 27

[0106] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 370°C.

[0107] Embodiment 28

[0108] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 380° C. and the holding time is 25 min.

[0109] Embodiment 29

[0110] The configuration of this embodiment is the same as that of embodiment 1, except that in step (7), the temperature of the second isothermal quenching heat treatment is 380°C.

[0111] Comparative Example 1

[0112] The configuration of this comparative example is the same as that of Example 1, except that the isothermal quenching heat treatment is completed in one step. That is:

[0113] (1) After casting, refining and hot forging, the bearing steel billet is naturally cooled to room temperature (22°C);

[0114] (2) The bearing steel billet is subjected to the first austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 1050°C, and the holding time is 20 min;

[0115] (3) Then oil quench (Q) to room temperature (22°C) at a cooling rate of 25°C / s;

[0116] (4) Carbide precipitation treatment (P) is then performed, and the oil-quenched bearing steel is heated to 670°C in a vacuum atmosphere furnace and kept at this temperature for 25 minutes; and then air-cooled to room temperature (22°C);

[0117] (5) Then, the bearing steel is subjected to a second austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 925°C, and the holding time is 35 minutes;

[0118] (6) Then quickly transfer to a salt bath furnace for isothermal quenching heat treatment (A), the isothermal quenching temperature is 330°C, the heat preservation time is 25 min, and then water-cooled to room temperature (22°C);

[0119] (7) Finally, the austempered bearing steel is transferred into a box furnace for low-temperature tempering heat treatment at a tempering temperature of 150 °C for 25 min, and then air-cooled to room temperature (22 °C).

[0120] Table 4: Mechanical properties and wear resistance of bainitic bearing steel under different austempering heat treatment conditions

[0121]

[0122]

[0123] The above-mentioned Examples 18 to 23 tested the influence of the parameters (mainly including temperature, duration, temperature + duration) of the first step isothermal quenching heat treatment, and Examples 24 to 29 tested the influence of the parameters (mainly including temperature, temperature + duration) of the second step isothermal quenching heat treatment.

[0124] It can be seen from Table 4 that in the austempering heat treatment, as the first austempering temperature decreases, the yield strength and tensile strength of the bearing steel decrease, but the elongation and impact toughness increase, and the wear resistance decreases. When the first austempering temperature increases, the yield strength and tensile strength of the bearing steel increase, but the elongation and impact toughness decrease, and the wear resistance remains basically unchanged. With the extension of time, the mechanical properties of the bearing steel also decrease. With the increase of the second austempering temperature or the extension of time, the yield strength and tensile strength of the bearing steel decrease, the elongation and impact toughness increase, and the wear resistance decreases. This shows that when the first austempering temperature is too low, a large amount of bainite is formed in the matrix, and the martensite content is insufficient after subsequent quenching, resulting in a decrease in the strength and wear resistance of the bearing steel. When the first austempering temperature is too high, the amount of bainite formed is insufficient, and the amount of martensite increases, resulting in high strength but insufficient toughness and plasticity of the bearing steel. When the second step austempering temperature is high or the time is long, the bainite in the matrix coarsens and the martensite content decreases, resulting in reduced mechanical properties of the bearing steel.

[0125] Comparative Example 1 is a one-step single-stage isothermal quenching heat treatment process. Compared with Comparative Example 1, Example 1 adopts graded isothermal quenching heat treatment, which is conducive to the formation of fine lower bainite structure and residual austenite. The low-temperature isothermal quenching utilizes a higher degree of supercooling to improve the nucleation efficiency of the lower bainite, providing favorable conditions for the subsequent refinement of the lower bainite; and the subsequent high-temperature isothermal quenching promotes the growth of the lower bainite and forms island-shaped residual austenite around the lower bainite lath. These unstable island-shaped residual austenites are transformed into martensite in the subsequent water-cooling quenching, which can further improve the hardness, strength and wear resistance of the bearing steel.

[0126] Embodiment 30

[0127] The configuration of this embodiment is the same as that of embodiment 1, except that in step (8), the holding time of the low-temperature tempering heat treatment is 20 minutes.

[0128] Embodiment 31

[0129] The configuration of this embodiment is the same as that of embodiment 1, except that in step (8), the holding time of the low-temperature tempering heat treatment is 30 minutes.

[0130] Comparative Example 2

[0131] The configuration of this comparative example is the same as that of Example 1, except that no low-temperature tempering heat treatment is performed.

[0132] (1) After casting, refining and hot forging, the bearing steel billet is naturally cooled to room temperature (22°C);

[0133] (2) The bearing steel billet is subjected to the first austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 1050°C, and the holding time is 20 min;

[0134] (3) Then oil quench (Q) to room temperature (22°C) at a cooling rate of 25°C / s;

[0135] (4) Carbide precipitation treatment (P) is then performed, and the oil-quenched bearing steel is heated to 670°C in a vacuum atmosphere furnace and kept at this temperature for 25 minutes; and then air-cooled to room temperature (22°C);

[0136] (5) Then, the bearing steel is subjected to a second austenitizing treatment in a vacuum atmosphere furnace, the austenitizing temperature is 925°C, and the holding time is 35 minutes;

[0137] (6) The mixture is then quickly transferred to a low-temperature salt bath furnace for the first isothermal quenching heat treatment (A1), with an isothermal quenching temperature of 295°C and a holding time of 6 min;

[0138] (7) Then quickly transfer to a high-temperature salt bath furnace for the second step of isothermal quenching heat treatment (A2) at an isothermal quenching temperature of 360°C for 30 min, and then water-cooled to room temperature (22°C).

[0139] Table 5: Effect of different low temperature tempering heat treatment durations on mechanical properties and wear resistance of bainitic bearing steel

[0140]

[0141] The above-mentioned Examples 30 and 31 mainly verify the influence of the low-temperature tempering heat treatment time on the performance of bearing steel.

[0142] It can be seen from Table 5 that under the same conditions, as the low-temperature tempering time increases, the yield strength and tensile strength gradually decrease, while the elongation and impact toughness increase. When the low-temperature tempering time is 30 minutes, the wear volume of the bearing steel increases significantly. This shows that the low-temperature tempering treatment effectively eliminates the internal stress, the yield strength, tensile strength and wear resistance decrease, but the elongation and impact toughness of the bearing steel increase significantly, and the comprehensive performance of the bearing steel is improved.

[0143] At the same time, since bearing steel has high requirements for wear resistance and fatigue resistance, a certain amount of martensite needs to be formed to improve the hardness of the matrix structure. The formation of martensite leads to residual stress in the matrix structure, and the impact toughness and elongation are reduced. Therefore, compared with Comparative Example 2, Example 1 introduces low-temperature tempering heat treatment at the end of the treatment to release residual stress and further improve the toughness and plasticity of the bearing steel.

[0144] The above embodiment achieves precise control of the carbide size in the matrix through separate carbide precipitation treatment and austenitization treatment, and can form nano-scale carbides in the organization. In addition, during the treatment process, the use of graded isothermal quenching heat treatment can effectively refine the bainite organization. First, the control of the size, quantity and morphology of bainite is beneficial to improving the comprehensive performance of bearing steel. Finally, a certain amount of martensite is formed by rapid quenching to improve the strength and wear resistance of bearing steel. Finally, the tempering step is introduced to optimize the organization and performance of bearing steel.

[0145] The above-mentioned embodiments only express several feasible implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention, and the embodiments are not used to limit the scope of protection in the claims of the present invention. For ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and all equivalent implementations or changes that do not depart from the present invention should be included in the technology of the present invention.

Claims

1. A heat treatment process for bainite bearing steel containing ultrafine carbides, characterized in that: The bearing steel billet is used as the object. After casting, refining, hot forging, and natural cooling to room temperature, the billet is processed in the following steps: Step 1: austenitizing the steel billet for the first time in a vacuum atmosphere furnace at a temperature of 1000-1100°C for 20-30 minutes, followed by oil quenching to room temperature; Step 2: Heat the oil-quenched steel billet to 650-700°C in a vacuum atmosphere furnace, keep warm for 20-30 minutes, and then air-cool to room temperature to complete the carbide precipitation treatment; Step 3: performing a second austenitizing treatment on the steel billet in a vacuum atmosphere furnace at a treatment temperature of 900-950°C for 30-40 minutes; Step 4: the steel billet is subjected to the first step of isothermal quenching heat treatment, the isothermal quenching temperature is 280-320°C, and the treatment time is 5-8 minutes; Step 5: The steel billet is subjected to a second isothermal quenching heat treatment at a temperature of 350-380°C for 25-30 minutes, and then water-cooled to room temperature. Step six, the steel billet is subjected to low temperature tempering heat treatment at a temperature of 120-150°C. After the treatment time is 20-30 minutes, it is air-cooled to room temperature to complete the heat treatment.

2. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In the vacuum atmosphere furnace, the protective gas is nitrogen or argon.

3. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In step 1, the quenching medium of the oil quenching is vacuum quenching oil, which includes 95.0wt.% refined base oil, 0.5wt.% antioxidant, 3.0wt.% composite additive and 1.5wt.% catalyzer.

4. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In step 1, the cooling rate of oil quenching is 20~30℃ / s.

5. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In step 4, the steel billet after the second austenitizing treatment is transferred to the first step of isothermal quenching heat treatment in 20 to 30 seconds.

6. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: The salt bath medium of the first step of isothermal quenching heat treatment is a mixture of KCl:NaCl=1:

1.

7. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In step 5, the steel billet after the first step of isothermal quenching heat treatment is transferred to the second step of isothermal quenching heat treatment within 10 to 20 seconds.

8. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: The salt bath medium of the second step isothermal quenching heat treatment is a mixture of KCl:NaCl:BaCl2=4~5:1.5~2.0:3.0~3.

5.

9. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: The cooling medium of the water cooling is alkaline water, and the concentration of the alkaline water is 5-8wt.%.

10. The heat treatment process of a bainite bearing steel containing ultrafine carbides according to claim 1, characterized in that: In step six, the steel billet that has completed the second step of isothermal quenching heat treatment is transferred to low-temperature tempering heat treatment within 1 to 2 hours.

Citation Information

Cited By

  • Treatment process for bainite steel with superfine retained austenite

    CN119614811A

  • High-efficiency precise Marbainite complex-phase heat treatment method for high-carbon steel bearing

    CN119685581A